A negative electrode sheet and a battery comprising the negative electrode sheet
By designing a double-layer negative electrode material structure in a lithium-ion battery, using graphite and natural graphite with a particle size distribution of less than or equal to 0.8, the ratio of conductive agent and binder is optimized, and the problem of long charging time of thick electrodes is solved and the charging efficiency of the battery is improved and power performance.
Patent Information
- Application Number
- CN202211632862.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-19
AI Technical Summary
Thick electrodes in existing lithium-ion batteries lead to long charging time and poor dynamic performance, which requires overcoming this defect.
Design a negative electrode sheet, including upper and lower negative electrode material layers, the upper material contains graphite with a particle size distribution discrete degree of less than or equal to 0.8, the lower material contains natural graphite, the proportion of conductive agent and binder is optimized, and the additives are combined to improve charging capacity and ions Mechanical properties of migration.
Through the design and proportional control of the upper and lower layers of material, the charging capacity of the battery is significantly improved, the interface and charge transfer impedance are reduced, and the charging time is shortened.
Smart Images

Figure CN115954436B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a negative electrode sheet and a battery comprising the negative electrode sheet. Background Art
[0002] Lithium-ion batteries have become one of the most ideal energy sources due to their high energy density, long cycle life, low environmental pollution and no memory effect, and have been widely used in mobile energy, laptops, electric vehicles, drones and other products. Electric vehicles are increasingly popular in the market, and lithium-ion batteries, as the ideal power source for electric vehicles, are facing unprecedented challenges - they need to balance energy density and power performance.
[0003] In terms of battery process technology, the development of thick electrodes is one of the important strategies to improve the energy density of lithium-ion batteries. However, there are some problems that need to be solved in thick electrodes. The increase in electrode thickness leads to a long ion migration path and poor kinetic performance, which results in prolonged charging time. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of the thick electrode in the prior art that the charging time is long, thereby providing a negative electrode sheet and a battery comprising the negative electrode sheet.
[0005] The present invention provides a negative electrode sheet, comprising a negative electrode current collector, a lower negative electrode material layer coated on the negative electrode current collector and in contact with the negative electrode current collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode current collector;
[0006] The upper negative electrode material layer includes a first negative electrode active material, a first binder, a first conductive agent, and a first dispersant; the lower negative electrode material layer includes a second negative electrode active material, a second binder, a second conductive agent, and a second dispersant, the first negative electrode active material is selected from graphite with a discreteness of particle size distribution less than or equal to 0.8, and the second negative electrode active material includes natural graphite and graphite with a discreteness of particle size distribution less than or equal to 0.8;
[0007] The mass of the second conductive agent is 1.2-3.5 times the mass of the first conductive agent; and / or the mass of the second adhesive is 1.5-4 times the mass of the first adhesive.
[0008] Furthermore, the mass of the second conductive agent is 1.8-3.5 times the mass of the first conductive agent.
[0009] Furthermore, the mass ratio of the upper negative electrode material layer to the lower negative electrode material layer is 1:0.8-1.2, preferably 1:1.
[0010] Furthermore, the first binder or the second binder is one or more of styrene-butadiene rubber, styrene-acrylic emulsion, and acrylate; and / or the ratio of the sum of the mass of the first binder and the second binder to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.5-3:100.
[0011] Furthermore, the first conductive agent or the second conductive agent is one or more of carbon black, carbon nanotubes, acetylene black, and Ketjen black; and / or the ratio of the sum of the mass of the first conductive agent and the second conductive agent to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.4-2.5:100.
[0012] Furthermore, the raw material of the upper negative electrode material layer also includes additives, and the additives are selected from one or more of NaCl, PMMA, and sulfonylhydrazine; preferably, the ratio of the mass of the additive to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.5-5:100.
[0013] Furthermore, the first dispersant or the second dispersant is one or more of acrylic acid, sodium carboxymethyl cellulose, and nanocellulose; the mass ratio of the first dispersant to the upper negative electrode material layer is 0.2-1.3:100; the mass ratio of the second dispersant to the lower negative electrode material layer is 0.3-1.5:100.
[0014] The present invention also provides a method for preparing the above-mentioned negative electrode sheet, wherein the components of the upper negative electrode material layer and the lower negative electrode material layer are mixed separately to prepare an upper slurry and a lower slurry, and after coating and drying, a negative electrode sheet containing a lower negative electrode material layer and an upper negative electrode material layer is obtained.
[0015] Furthermore, the coating surface density of the upper negative electrode material layer and the lower negative electrode material layer is 3-8 mg / cm 2 Preferably, the surface density of the upper negative electrode material layer and the lower negative electrode material layer is the same.
[0016] The present invention also provides a battery, comprising any of the above-mentioned negative electrode sheets or the negative electrode sheets prepared by the above-mentioned preparation methods.
[0017] The technical solution of the present invention has the following advantages:
[0018] 1. The negative electrode sheet provided by the present invention comprises a negative electrode current collector, a lower negative electrode material layer coated on the negative electrode current collector and in contact with the negative electrode current collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode current collector; the upper negative electrode material layer comprises a first negative electrode active material, a first binder, a first conductive agent and a first dispersant; the lower negative electrode material layer comprises a second negative electrode active material, a second binder, a second conductive agent and a second dispersant, the first negative electrode active material is selected from graphite with a discreteness of particle size distribution less than or equal to 0.8, and the second negative electrode active material comprises natural graphite and graphite with a discreteness of particle size distribution less than or equal to 0.8; the mass of the second conductive agent is 1.2-3.5 times the mass of the first conductive agent; and / or the mass of the second binder is 1.5-4 times the mass of the first binder.
[0019] Through the design of the upper and lower layers, the upper layer uses graphite with a particle size distribution discreteness of less than or equal to 0.8, and the lower layer uses natural graphite and graphite with a particle size distribution discreteness of less than or equal to 0.8. In addition, by controlling the content ratio of the two layers of conductive agent and binder, the battery's charging capacity is significantly improved while improving the ion migration kinetics and the utilization rate of active materials, thereby reducing the interface impedance and charge transfer impedance and shortening the charging time.
[0020] 2. In the negative electrode sheet provided by the present invention, additives such as NaCl, PMMA, and sulfonylhydrazide are also added to the upper negative electrode material layer; in particular, the ratio of the mass of the additives to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is controlled to be 0.5-5:100, so that the porosity of the upper negative electrode material layer is greater than that of the lower negative electrode material layer, and the microstructure of the gradient porosity in the thickness direction is beneficial to the electrolyte infiltration of the thick electrode, which can further reduce the internal resistance of the electrode and shorten the charging time. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 is the particle size distribution diagram of artificial graphite A and artificial graphite B;
[0023] Figure 2 This is a characterization diagram of the porosity of the upper and lower layers of the cross-section of Example 1. DETAILED DESCRIPTION
[0024] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0025] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0026] Among them, the dispersion of the particle size distribution of artificial graphite A is 0.8, and the dispersion of artificial graphite B is 1.0. Dispersion = (D90-D10) / D50, where D90, D50 and D10 are the particle sizes when the cumulative distribution of the number reaches 90%, 50% and 10%, respectively. Figure 1 As shown, the particle size range of artificial graphite A is 4.30-33.15 microns, and the particle size range of artificial graphite B is 1.55-55.24 microns.
[0027] Example 1
[0028] This embodiment provides a negative electrode sheet, including a negative electrode collector (copper foil with a thickness of 6 um), a lower negative electrode material layer coated on the negative electrode collector and in contact with the negative electrode collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode collector.
[0029] Preparation method: Weigh 96.9g of artificial graphite A, 0.7g of carbon black, 1.2g of styrene-butadiene rubber, and 1.2g of sodium carboxymethyl cellulose to make the upper negative electrode slurry, and weigh 75.7g of artificial graphite A, 20g of natural graphite, 1.8g of styrene-butadiene rubber, 1.3g of carbon black, and 1.2g of sodium carboxymethyl cellulose to make the lower negative electrode slurry. After coating, drying, and winding with a double-layer coating machine, a negative electrode sheet containing a lower negative electrode material layer and an upper negative electrode material layer was obtained, and the coating surface density of each layer was 4.5mg / cm 2 .
[0030] Example 2
[0031] This embodiment provides a negative electrode sheet, including a negative electrode collector (copper foil with a thickness of 6 um), a lower negative electrode material layer coated on the negative electrode collector and in contact with the negative electrode collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode collector.
[0032] Preparation method: Weigh 96.9g of artificial graphite A, 0.7g of carbon black, 1.2g of styrene-butadiene rubber, 1.2g of sodium carboxymethyl cellulose, and 2.0g of p-toluenesulfonyl hydrazide to prepare the upper negative electrode slurry, and weigh 75.7g of artificial graphite A, 20g of natural graphite, 1.8g of styrene-butadiene rubber, 1.3g of carbon black, and 1.2g of sodium carboxymethyl cellulose to prepare the lower negative electrode slurry. After coating, drying, and winding with a double-layer coating machine, a negative electrode sheet containing a lower negative electrode material layer and an upper negative electrode material layer was obtained, and the coating surface density of each layer was 4.5mg / cm 2 .
[0033] Example 3
[0034] This embodiment provides a negative electrode sheet, including a negative electrode collector (copper foil with a thickness of 6 um), a lower negative electrode material layer coated on the negative electrode collector and in contact with the negative electrode collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode collector.
[0035] Preparation method: 97.4g of artificial graphite A, 0.6g of carbon black, 0.8g of styrene-butadiene rubber, 1.2g of sodium carboxymethyl cellulose, and 2.0g of acrylic resin PMMA were weighed and mixed to prepare the upper negative electrode slurry; 55.8g of artificial graphite A, 40g of natural graphite, 1.6g of styrene-butadiene rubber, 1.4g of carbon black, and 1.2g of sodium carboxymethyl cellulose were weighed and mixed to prepare the lower negative electrode slurry. The components of the upper negative electrode material layer and the lower negative electrode material layer were mixed separately to prepare the upper slurry and the lower slurry, and a double-layer coating machine was used to coat, dry, and roll up to obtain a negative electrode sheet containing the lower negative electrode material layer and the upper negative electrode material layer, and the coating surface density of each layer was 4.5mg / cm 2 .
[0036] Example 4
[0037] The present embodiment provides a negative electrode sheet and a preparation method thereof, which are basically the same as those of Embodiment 1, except that the contents of the substances in the upper negative electrode material layer are different. In this comparative example, based on the total mass of the upper negative electrode material layer being 100wt%, the upper negative electrode material layer includes 96.6wt% artificial graphite A, 1.0wt% carbon black, 1.2wt% styrene-butadiene rubber and 1.2wt% sodium carboxymethyl cellulose.
[0038] Comparative Example 1
[0039] This comparative example provides a negative electrode sheet and a preparation method thereof, comprising a negative electrode current collector (copper foil with a thickness of 6 um), and a negative electrode material layer coated on the negative electrode current collector and in contact with the negative electrode current collector.
[0040] Based on the total mass of the negative electrode material layer being 100 wt %, the negative electrode material layer includes 96 wt % of artificial graphite B, 1.0 wt % of carbon black, 1.8 wt % of styrene-butadiene rubber, and 1.2 wt % of sodium carboxymethyl cellulose.
[0041] Preparation method: The components of the negative electrode material layer are mixed to obtain a slurry, which is then coated, dried and rolled using a single-layer coating machine to obtain a negative electrode sheet containing a negative electrode material layer. The coating surface density is 9 mg / cm 2 .
[0042] Comparative Example 2
[0043] This comparative example provides a negative electrode sheet and a preparation method thereof, which are basically the same as comparative example 1, except that artificial graphite A is used instead of artificial graphite B.
[0044] Comparative Example 3
[0045] This comparative example provides a negative electrode sheet and a preparation method thereof, which are basically the same as Example 1, except that the contents of various substances in the upper negative electrode material layer are different. In this comparative example, based on the total mass of the upper negative electrode material layer being 100wt%, the upper negative electrode material layer includes 96wt% artificial graphite A, 1.0wt% carbon black, 1.8wt% styrene-butadiene rubber, and 1.2wt% sodium carboxymethyl cellulose.
[0046] Comparative Example 4
[0047] This comparative example provides a negative electrode sheet and a preparation method thereof, which are basically the same as those in Example 1, except that silicon oxide (manufacturer: Shin-Etsu, brand: KSC1265) of the same mass is used instead of natural graphite.
[0048] Experimental Example 1
[0049] 1. The resistivity of the negative electrode sheets prepared in each embodiment and comparative example was tested, and the results are shown in Table 1.
[0050] 2. The electrochemical performance of button cells assembled with negative electrode sheets prepared in each embodiment and comparative example was tested and analyzed, as follows:
[0051] S1: Prepare the positive electrode. Mix the nickel-cobalt-manganese positive electrode material NCM111, conductive carbon black SP, carbon nanotubes CNT and polyvinylidene fluoride PVDF in a weight ratio of 96.3:1.8:0.7:1.2, and disperse them in N-methylpyrrolidone NMP to form a uniform slurry. Then coat the slurry on a 12um aluminum foil with a coating surface density of 15mg / cm 2 , and dried in vacuum at 70 °C for 0.3 h.
[0052] S2: Button half-cells were assembled in a glove box filled with inert gas, using PP as the separator and 1 mol / L lithium hexafluorophosphate, EC:EMC:DMC solution with a volume ratio of 1:1:1 as the electrolyte. Constant current charge / discharge tests were performed at room temperature using a LAND CT2001A battery test system.
[0053] The test procedure of 25℃ / 50%SOC / DCR(mΩ) is as follows: fully charge at 0.33C constant current and constant voltage to 4.2V / 0.05C at 25℃, stand for 30min, discharge at 0.33C constant current to 3.7V, then 50%SOC; stand for 30min, discharge at 4C constant current for 10S, stand for 10min, charge at 3C constant current for 10S, stand for 10min, end.
[0054] The test procedure for charging time is as follows: three-electrode preparation, constant current charging to 4.2V at different rates of 0.5 / 0.75 / 1 / 1.5 / 2C, detection of the third electrode voltage, calculation and fitting of the charging rate corresponding to different SOCs, obtaining the rate-SOC curve, and calculating the charging time.
[0055] Table 1 Test results
[0056]
[0057] The results show that compared with comparative examples 1-4, examples 1-4 of the present invention can simultaneously reduce DC impedance and shorten charging time by using two-layer coating, combining the upper layer with artificial graphite A with a narrow particle size distribution as the negative electrode material, the lower layer with artificial graphite A with a narrow particle size distribution and natural graphite as the negative electrode material, and controlling the mass ratio of the two layers of conductive agent and / or binder. In particular, by controlling the ratio of the two layers of conductive agent in examples 1-3 within the preferred range, the introduction of additives in examples 2 and 3 can further shorten the charging time.
[0058] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A negative electrode sheet, characterized in that: It includes a negative electrode current collector, a lower negative electrode material layer coated on the negative electrode current collector and in contact with the negative electrode current collector, and an upper negative electrode material layer in contact with the lower negative electrode material layer and away from the negative electrode current collector; The upper negative electrode material layer includes a first negative electrode active material, a first binder, a first conductive agent and a first dispersant; the lower negative electrode material layer includes a second negative electrode active material, a second binder, a second conductive agent and a second dispersant; the first negative electrode active material is selected from graphite with a discreteness of particle size distribution less than or equal to 0.8, and the second negative electrode active material includes natural graphite and graphite with a discreteness of particle size distribution less than or equal to 0.8; The mass of the second conductive agent is 1.2-3.5 times the mass of the first conductive agent; the mass of the second adhesive is 1.5-4 times the mass of the first adhesive.
2. The negative electrode sheet according to claim 1, characterized in that: The mass of the second conductive agent is 1.8-3.5 times the mass of the first conductive agent.
3. The negative electrode sheet according to claim 1 or 2, characterized in that: The mass ratio of the upper negative electrode material layer to the lower negative electrode material layer is 1:0.8-1.
2.
4. The negative electrode sheet according to claim 1 or 2, characterized in that: The mass ratio of the upper negative electrode material layer to the lower negative electrode material layer is 1:
1.
5. The negative electrode sheet according to claim 1 or 2, characterized in that: The first binder or the second binder is one or more of styrene-butadiene rubber, styrene-acrylic emulsion, and acrylate; and / or the ratio of the sum of the mass of the first binder and the second binder to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.5-3:
100.
6. The negative electrode sheet according to claim 1 or 2, characterized in that: The first conductive agent or the second conductive agent is one or more of carbon black and carbon nanotubes; and / or the ratio of the sum of the mass of the first conductive agent and the second conductive agent to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.4-2.5:
100.
7. The negative electrode sheet according to claim 1 or 2, characterized in that: The first conductive agent or the second conductive agent is one or more of acetylene black and Ketjen black.
8. The negative electrode sheet according to claim 1 or 2, characterized in that: The raw material of the upper negative electrode material layer further includes an additive, and the additive is selected from one or more of NaCl, PMMA, and sulfonyl hydrazide.
9. The negative electrode sheet according to claim 8, characterized in that: The ratio of the mass of the additive to the total mass of the upper negative electrode material layer and the lower negative electrode material layer is 0.5-5:
100.
10. The negative electrode sheet according to claim 1 or 2, characterized in that: The first dispersant or the second dispersant is one or more of acrylic acid, sodium carboxymethyl cellulose, and nanocellulose; the mass ratio of the first dispersant to the upper negative electrode material layer is 0.2-1.3:100; the mass ratio of the second dispersant to the lower negative electrode material layer is 0.3-1.5:
100.
11. A method for preparing a negative electrode sheet according to any one of claims 1 to 10, characterized in that: The components of the upper negative electrode material layer and the lower negative electrode material layer are mixed respectively to prepare an upper slurry and a lower slurry, and after coating and drying, a negative electrode sheet containing the lower negative electrode material layer and the upper negative electrode material layer is obtained.
12. The method for preparing a negative electrode sheet according to claim 11, characterized in that: The coating surface density of the upper negative electrode material layer and the lower negative electrode material layer is 3-8 mg / cm 2 .
13. The method for preparing a negative electrode sheet according to claim 12, characterized in that: The upper negative electrode material layer and the lower negative electrode material layer have the same surface density.
14. A battery, characterized in that: The invention comprises the negative electrode sheet described in any one of claims 1 to 10 or the negative electrode sheet prepared by the preparation method described in any one of claims 11 to 13.
Citation Information
Patent Citations
Lithium ion battery negative plate, preparation method thereof and lithium ion battery
CN114899357A
Secondary battery, battery module including same, battery pack, and device
CN114902450A
Nonaqueous electrolyte secondary battery
JP2009026514A
Negative electrode and method for manufacturing same
WO2022080979A1