Calcium-doped barium titanate powder, preparation method and use thereof

By doping barium titanate powder with Ca element and combining normal pressure hydrothermal and solid-state preparation processes, the problem of insufficient operability of BaTiO3 ceramic powder in the high temperature range is solved, and high tetragonality and high dielectric properties are achieved. Preparation of barium titanate powder with electrical constant, suitable for high performance multilayer ceramic capacitors.

CN115959703BActive Publication Date: 2024-10-11SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111192498.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-13
Publication Date
2024-10-11
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

The existing BaTiO3 ceramic powder has low operability in the high temperature range and is difficult to meet the high capacity, high temperature, high voltage, high frequency, high reliability and miniaturization needs of multilayer ceramic capacitors in the 5G era.

Method used

Through a preparation process that combines atmospheric pressure hydrothermal method and solid phase method, Ca element is doped into barium titanate powder, and the reaction temperature and raw material ratio are adjusted to obtain calcium-doped titanium with high tetragonality and high dielectric constant. Barium acid powder.

Benefits of technology

The tetragonality and dielectric constant of barium titanate powder are improved, and its temperature operating range is broadened. It is suitable for the dielectric layer of high-performance multilayer ceramic capacitors. The process is simple, the raw materials are easily available, and the product stability is high.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115959703B_ABST
    Figure CN115959703B_ABST
Patent Text Reader

Abstract

The invention relates to calcium-doped barium titanate powder, a preparation method and its use, and specifically discloses a preparation method of calcium-doped barium titanate powder, which is mainly based on a solid phase method and supplemented by a hydrothermal method. At a low hydrothermal temperature under normal pressure, a soluble Ba source and a Ti source with TiO2 as a seed are dispersed in an aqueous solution and stirred for reaction; then a second Ba source and a Ca source are added and mixed by ball milling, and the calcium-doped barium titanate powder is obtained by drying and calcining. The invention adopts a preparation method of a normal pressure hydrothermal assisted solid phase method, and appropriately dopes the Ca element into the barium titanate-based material, thereby greatly improving the tetragonality of the barium titanate-based material and greatly enhancing the dielectric properties of the material. The invention has a simple process, easy-to-obtain raw materials, and high product stability. The method provides a new technical support for preparing ceramic powders in multilayer ceramic capacitors with high capacitance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dielectric ceramic powder preparation, and in particular to calcium-doped barium titanate powder, a preparation method and application thereof. Background Art

[0002] Multilayer ceramic capacitors (MLCCs) are one of the most widely used and most important electronic components in electronic devices. They are known as the "rice of industry". They have high capacitance, high reliability and excellent high-frequency characteristics. In order to meet the development needs of multilayer ceramic capacitors in the 5G era, namely, high capacitance, high temperature, high voltage, high frequency, high reliability and miniaturization, it is imperative to develop high-performance dielectric ceramic powders suitable for industrial production and application. MLCCs are chip-type multilayer capacitors composed of ceramic dielectrics and metal inner electrodes stacked and end electrodes packaged. By selecting dielectric materials with higher dielectric constants, smaller ceramic dielectric filling powders, and increasing the number of dielectric layers, the performance requirements of rapidly developing electronic devices can be met. Therefore, the synthesis of ceramic powders for dielectric layers and metal internal electrodes is crucial.

[0003] In MLCC, the commonly used dielectric ceramic filling powder is BaTiO3-based material. The dielectric constant of high dielectric materials is related to the microstructure of the material, that is, tetragonality. When BaTiO3 ceramic powder is not modified, the tetragonality and the operable range of the temperature range of MLCC are small. In order to adapt to the rapid development of the electronics industry, it is necessary to develop dielectric materials with better performance. Among them, improving the preparation process and doping and modifying the barium titanate-based material to improve the performance of the barium titanate-based material are the two most commonly used methods. Among them, Ca-doped BaTiO3-based (BaTiO3-based 1-X Ca x TiO3, BCT) is considered to be the most important candidate material for lead-free optoelectronic modulators and memory devices. BCT material has a more stable tetragonal ferroelectric phase, better capacitance-temperature characteristics and a higher dielectric constant, which can broaden the temperature operating range of barium titanate for MLCC. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a calcium-doped barium titanate powder, a preparation method and uses thereof. By improving the preparation process of barium titanate powder and doping Ca element into the barium titanate powder, the obtained barium titanate-based powder has good tetragonality and can be applied to the dielectric layer of multilayer ceramic capacitors.

[0005] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0006] The first aspect of the present invention provides a method for preparing calcium-doped barium titanate powder, comprising the following steps:

[0007] Step (1), preparing powder I by a normal pressure hydrothermal method: adding a first Ba source into water, stirring to dissolve, then adding an aqueous dispersion containing a Ti source, stirring to react at a certain temperature, and then drying to obtain powder I;

[0008] Step (2), preparing calcium-doped barium titanate powder by a solid phase method: adding a second Ba source and a Ca source to powder I, mixing and ball milling, drying, sieving, grinding, and finally calcining to obtain calcium-doped barium titanate powder;

[0009] In step (1), the molar ratio of Ba contained in the first Ba source and the second Ba source is 0.05-0.5, the molar ratio of the total Ba contained in the first Ba source and the second Ba source to the Ti contained in the Ti source is 0.99-1.01, and in step (2), the molar ratio of Ca contained in the Ca source to the total Ba contained in the first Ba source and the second Ba source is 0.01-0.5.

[0010] In certain specific embodiments, in step (1), the molar ratio of Ba contained in the first Ba source to that contained in the second Ba source is 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or any value therebetween.

[0011] In certain specific embodiments, in step (1), the molar ratio of the total Ba contained in the first Ba source and the second Ba source to the Ti contained in the Ti source is 0.99, 1.00, 1.01 or any value therebetween.

[0012] In certain specific embodiments, in step (2), the molar ratio of Ca contained in the Ca source to the total Ba contained in the first Ba source and the second Ba source is 0.01, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or any value therebetween.

[0013] Furthermore, in step (1), the first Ba source is a water-soluble Ba source, and the Ti source is TiO2 having an anatase phase; the stirring reaction environment is alkaline, and PH>10.

[0014] In some specific embodiments, the first Ba source is barium hydroxide, barium nitrate, barium chloride or any other water-soluble Ba source, which can be used alone or in any combination.

[0015] Furthermore, in step (2), the second Ba source is BaCO3, and the Ca source is CaCO3.

[0016] Furthermore, in step (1), after adding the aqueous dispersion containing the Ti source, the stirring reaction temperature is 80°C-120°C, and the stirring reaction time is 30min-12h.

[0017] In certain specific embodiments, in step (1), after adding the aqueous dispersion containing the Ti source, the stirring reaction temperature is 80°C, 90°C, 100°C, 110°C, 120°C or any temperature therebetween.

[0018] In certain specific embodiments, in step (1), the stirring reaction time is 30 min, 1 h, 3 h, 5 h, 7 h, 10 h, 12 h or any reaction time therebetween.

[0019] Furthermore, in step (2), the calcination temperature is 300°C-1300°C, the calcination time is 30min-4h, and the heating rate is 2-15°C / min.

[0020] In some specific embodiments, in step (2), the calcination temperature is 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C or any temperature therebetween.

[0021] In certain specific embodiments, in step (2), the calcination time is 30 min, 1 h, 2 h, 3 h, 4 h or any reaction time therebetween.

[0022] In certain specific embodiments, in step (2), the heating rate is 2°C / min, 3°C / min, 4°C / min, 5°C / min, 7°C / min, 10°C / min, 12°C / min, 15°C / min or any heating rate therebetween.

[0023] Furthermore, in step (2), the ball milling medium is zirconium beads and deionized water, and the ball milling time is 24 hours. In the technical solution of the present invention, the ball milling operation allows the hydrothermal product of step (1) to be evenly mixed with the second Ba source and the Ca source.

[0024] Furthermore, in step (2), the sieving operation is performed using a 200-mesh sieve.

[0025] The second aspect of the present invention provides calcium-doped barium titanate powder obtained by the above preparation method. In the technical solution of the present invention, the calcium-doped barium titanate powder obtained by the above preparation method, the Ca element in the Ca source can partially replace the A position of the barium titanate group.

[0026] Furthermore, the chemical formula of the calcium-doped barium titanate powder is Ba x Ca 1-x TiO3, where x is 0.8-0.9, has a tetragonality of c / a=1.009-1.011.

[0027] In some specific embodiments, the chemical structure of the calcium-doped barium titanate powder is Bax Ca 1-x The x in TiO3 is 0.8, 0.81, 0.9 or any value therebetween, and the tetragonality c / a thereof is 1.009, 1.010, 1.011 or any value therebetween.

[0028] The third aspect of the present invention provides the use of the calcium-doped barium titanate powder as a dielectric material. Further, the barium titanate powder is used to prepare electronic components, and the electronic components are multilayer ceramic capacitors.

[0029] The above technical solution has the following advantages or beneficial effects:

[0030] The invention adopts a preparation method of hydrothermal assisted solid phase synthesis at normal pressure. First, a soluble Ba source and a Ti source with TiO2 as a seed are dispersed in an aqueous solution at a low hydrothermal temperature at normal pressure, and stirred for reaction; then a second Ba source and a Ca source are mixed with the hydrothermal product by a solid phase synthesis method, ball milled, and dried and calcined to obtain a calcium-doped barium titanate powder with high tetragonality. The invention performs Ca doping on the barium titanate material, and by adjusting the reaction temperature and the raw material ratio, the Ca element partially replaces the A position of the barium titanate base, thereby improving the tetragonality and dielectric constant of the barium titanate powder, and by adjusting the raw material ratio, a suitable final stoichiometric product is obtained, and the particle properties of the product can be controlled by changing the process. The invention has the advantages of simple process, easy-to-obtain raw materials, high product stability, and provides a new technical support for the preparation of ceramic powders in high-capacitance multilayer ceramic capacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the XRD pattern of the calcium-doped barium titanate powder synthesized in Example 1 of the present invention;

[0032] Figure 2 is a SEM image of the calcium-doped barium titanate powder synthesized in Example 1 of the present invention;

[0033] Figure 3 is the XRD pattern of the calcium-doped barium titanate powder synthesized in Example 2 of the present invention;

[0034] Figure 4 This is a SEM image of the calcium-doped barium titanate powder synthesized in Example 2 of the present invention. DETAILED DESCRIPTION

[0035] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0036] The technical solution of the present invention is to design a preparation method of calcium-doped barium titanate powder, which is mainly based on a solid phase method and supplemented by a normal pressure hydrothermal method. The barium titanate powder is doped with Ca element, which can greatly improve the dielectric constant of the barium titanate-based material.

[0037] In the following embodiments:

[0038] (1) The selected raw materials are Ba(OH)2·8H2O, anatase phase TiO2, BaCO3 and CaCO3;

[0039] (2) Control the addition ratio of raw materials Ba(OH)2·8H2O and BaCO3, and change the addition ratio of CaCO3;

[0040] (3) In the normal pressure hydrothermal method, Ba(OH)2·8H2O is first dissolved in water, heated and stirred, and then anatase phase TiO2 is added. Water is continued to be added to the dispersion, the heating temperature is set, and the stirring reaction is continued for several hours. The pH of the stirring reaction is greater than 10;

[0041] (4) After the normal pressure hydrothermal reaction is completed, the hydrothermal product is transferred to a ball mill, dried, and a certain proportion of BaCO3 and CaCO3 are added, and deionized water and zirconium beads are used as ball milling media for solid phase synthesis, and mixed ball milling is performed for several hours;

[0042] (5) After the ball milling is completed, the product is dried, sieved and ground, and an appropriate amount of powder is taken for calcination.

[0043] Embodiment 1:

[0044] In this embodiment, the molar ratio of Ba / Ca in the total Ba source and the Ca source in the whole reaction process is 0.9 / 0.1, the molar ratio of Ba(OH)2·8H2O to BaCO3 is 0.25 / 0.75, the molar ratio of Ba / Ti in the whole reaction is 1, and the ingredients are prepared according to the molar ratio of Ba(OH)2·8H2O:BaCO3:CaCO3=0.225:0.675:0.1. The obtained barium titanate powder is Ba 0.9 Ca 0.1TiO3. First weigh 7.2427g of Ba(OH)2·8H2O into a three-necked flask, add 25ml of water, and continue stirring for 30min. Then weigh 0.1mol of 8.003g of TiO2 and 15ml of water into the aqueous dispersion of Ba, set the heating temperature to 100℃, and perform hydrothermal reaction at normal pressure for 6h. After the hydrothermal reaction, transfer the hydrothermal product to a ball mill for drying. Weigh BaCO3 and CaCO3 in proportion into a ball mill. The ball milling medium is zirconium beads and deionized water. Mix the hydrothermal product with BaCO3 and CaCO3 and ball mill for 24h. After the ball milling is completed, dry the mixture, grind it and pass it through a 200-mesh sieve. Take about 1g of the powder and place it in a muffle furnace for calcination at 950℃-1100℃. The heating rate is 5℃ / min and the insulation time is 2h. Figure 1 The BaTiO2 powder prepared by calcining the calcium-doped barium titanate powder synthesized in this example at 950°C, 1000°C, and 1100°C for 2h is 0.9 Ca 0.1 XRD pattern of TiO3 powder, Figure 2 The BaTiO2 powder synthesized in this example was calcined at 1000°C and 1100°C for 2h to prepare the BaTiO2 powder. 0.9 Ca 0.1 SEM image of TiO3 powder.

[0045] Embodiment 2:

[0046] In this embodiment, the molar ratio of Ba / Ca in the Ba source and the Ca source in the whole reaction process is 0.8 / 0.2, the molar ratio of Ba(OH)2·8H2O to BaCO3 is 0.25 / 0.75, the molar ratio of Ba / Ti in the whole reaction is 1, and the ingredients are prepared according to the molar ratio of Ba(OH)2·8H2O:BaCO3:CaCO3=0.2:0.6:0.2. The prepared calcium-doped barium titanate powder is Ba 0.8 Ca 0.2 TiO3. First weigh 6.4381g of Ba(OH)2·8H2O into a three-necked flask, add 25ml of water, and continue stirring for 30min. Then weigh 8.003g of TiO2 and 15ml of water in proportion to the aqueous dispersion of Ba, set the heating temperature to 100℃, and perform hydrothermal reaction at normal pressure for 6h. After the hydrothermal reaction, transfer the hydrothermal product to a ball mill for drying, weigh BaCO3 and CaCO3 in proportion and put them into the ball mill. The ball milling media are zirconium beads and deionized water. The hydrothermal product is mixed with BaCO3 and CaCO3 and ball milled for 24h. After the ball milling is completed, dry the mixture, grind it and pass it through a 200-mesh sieve. Take about 1g of powder and place it in a muffle furnace for calcination at 950℃-1100℃. The heating rate is 5℃ / min and the insulation time is 2h. Figure 3The powder of this example was prepared by calcining at 950°C, 1000°C, and 1100°C for 2h. 0.8 Ca 0.2 XRD pattern of TiO3 powder, Figure 4 The powder of this example was calcined at 1000℃ and 1100℃ for 2h to prepare Ba 0.8 Ca 0.2 SEM image of TiO3 powder.

[0047] Comparative Example:

[0048] In this comparative example, the molar ratio of Ba / Ca in the Ba source and the Ca source in the entire reaction process is 1, the molar ratio of Ba(OH)2·8H2O and BaCO3 is 0.25 / 0.75, the molar ratio of Ba / Ti in the entire reaction is 1, and the ingredients are prepared according to the molar ratio of Ba(OH)2·8H2O:BaCO3:CaCO3=0.25:0.75:0, and the prepared barium titanate powder is BaTiO3. First, weigh 8.0474g of Ba(OH)2·8H2O in a three-necked flask, add 25ml of water, and continue stirring for 30min. Then, weigh a certain amount of TiO2 and 15ml of water in proportion to the aqueous dispersion of Ba, set the heating temperature to 100℃, and perform hydrothermal reaction at normal pressure for 6h. After the hydrothermal reaction, transfer the hydrothermal product to a ball mill for drying, weigh BaCO3 in proportion to the ball mill, and use zirconium beads and deionized water as the ball milling medium. Mix the hydrothermal product and BaCO3 and ball mill for 24h. After the ball milling is completed, dry the mixture, grind it and pass it through a 200-mesh sieve. Take about 1g of the powder and place it in a muffle furnace for calcination at 950℃, 1000℃, and 1050℃. The heating rate is 5℃ / min, and the insulation time is 2h. Table 1 shows the c / a values ​​of this comparative example and Example 1 at different calcination temperatures.

[0049] In the above experimental results, for Example 1, Figure 1 It can be seen from the XRD diagram that with the increase of calcination temperature, the peak splitting degree in the range of 44°-46° is enhanced, indicating that Ba 0.9 Ca 0.1 The tetragonality of TiO3 increases with the calcination temperature; Figure 2 It can be seen from the SEM image that the particles are square, the particle surface is relatively smooth and round, and as the calcination temperature increases, the particle size increases accordingly.

[0050] For Example 2, from Figure 3 It can be seen from the XRD diagram that with the increase of calcination temperature, the peak splitting degree in the range of 44°-46° is enhanced, indicating that Ba 0.8 Ca 0.2The tetragonality of TiO3 increases with increasing calcination temperature, while the degree of splitting at 1000℃ is the same as that at 1100℃; Figure 4 It can be seen from the SEM image that at 1000°C, the particles are square and the surface of the particles is relatively smooth and round, but at 1100°C, there are no obvious grain boundaries between the particles, and they are about to be overburned.

[0051] Table 1 c / a values ​​and dielectric constants of barium titanate powders of Examples and Comparative Examples at different calcination temperatures.

[0052]

[0053] As can be seen from Table 1, the high tetragonality barium titanate-based material can be prepared by the process of atmospheric pressure hydrothermal assisted solid phase method. When a small amount of Ca element is doped, the tetragonality of the barium titanate-based material is greatly improved. 0.8 Ca 0.2 When TiO3 is calcined at 1000℃, c / a=1.01, Ba 0.9 Ca 0.1 When TiO3 is calcined at 1100℃, c / a=1.011. At the same calcination temperature, Ba 0.8 Ca 0.2 TiO3 has a higher tetragonality, so the calcination temperature has a great relationship with the doping amount of Ca. When Ca is doped at the A position of BaTiO3, the required calcination temperature decreases as the doping amount increases. The dielectric constant is usually positively correlated with the size of the tetragonality c / a value. BaTiO3 and calcium-doped barium carbonate (BCT) materials prepared under the above conditions, the BCT with a Ca doping amount of 0.2 has a much larger dielectric constant than BaTiO3, and the former is more than twice that of the latter.

[0054] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent transformation made using the contents of the present invention description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing calcium-doped barium titanate powder, characterized in that: The steps include: Step (1), preparing powder I by normal pressure hydrothermal method: adding a first Ba source into water, stirring to dissolve, then adding an aqueous dispersion containing a Ti source, stirring and reacting at 80°C-120°C for 30 min-12 h, and then drying to obtain powder I; Step (2), preparing calcium-doped barium titanate powder by solid phase method: adding a second Ba source and a Ca source to powder I, mixing and ball milling, drying, sieving, grinding, and finally calcining to obtain calcium-doped barium titanate calcium powder; In step (1), the first Ba source is a water-soluble Ba source, the molar ratio of Ba contained in the first Ba source to that contained in the second Ba source is 0.25:0.75, and the molar ratio of the total Ba contained in the first Ba source and the second Ba source to the Ti contained in the Ti source is 0.99-1.

01. In step (2), the second Ba source is BaCO3, the Ca source is CaCO3, the molar ratio of Ca contained in the Ca source to the total Ba contained in the first Ba source and the second Ba source is 0.2:0.8, the calcination temperature is 1000°C-1100°C, and the calcination time is 30 min-4 h.

2. The preparation method according to claim 1, characterized in that: In step (1), the Ti source is TiO2 having anatase phase; and the pH of the stirring reaction environment is > 10.

3. The preparation method according to claim 1, characterized in that: In step (2), the heating rate of calcination is 2-15°C / min.

4. The preparation method according to claim 1, characterized in that: In step (2), the ball milling medium is zirconium beads and deionized water, and the ball milling time is 24 h.

5. The preparation method according to claim 1, characterized in that: In step (2), the sieving operation is performed using a 200-mesh sieve.

6. Calcium-doped barium titanate powder obtained according to the preparation method according to any one of claims 1 to 5.

7. The calcium-doped barium titanate powder according to claim 6, characterized in that: The chemical structural formula of the calcium-doped barium titanate powder is Ba x Ca 1-x TiO3, where x is 0.8, has a tetragonality of c / a=1.01-1.

011.

8. The use of calcium-doped barium titanate powder as a dielectric material according to claim 6, characterized in that: The invention discloses a use of calcium-doped barium titanate powder for preparing electronic components, wherein the electronic components are multilayer ceramic capacitors.