Phase change microcapsules, diaphragms, pole pieces, batteries and electrical devices

By applying a specific proportion of phase change microcapsules on the battery separator and the edge of the tab, and using its gradient melting characteristics to absorb welding heat, the short circuit problem caused by excessive temperature of the separator after laser welding is solved, and the stability and life of the battery are improved.

CN115966839BActive Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202111189223.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-12
Publication Date
2024-10-18
Estimated Expiration
2041-10-12

Smart Images

  • Figure CN115966839B_ABST
    Figure CN115966839B_ABST
Patent Text Reader

Abstract

A phase change microcapsule, a diaphragm, a pole piece, a battery and an electrical device, belonging to the field of batteries. The phase change microcapsule includes: a core material and an insulating heat-conducting wall material that wraps the core material. The core material includes a first phase change component and a second phase change component, the first phase change component is paraffin with a melting point of 37-42°C, the second phase change component is paraffin with a melting point of 65-75°C, and the melting point of the insulating heat-conducting wall material is greater than 75°C. The mass ratio of the first phase change component to the second phase change component is 35:45-77. The phase change microcapsule is applied to the battery in the form of a coating, so that the bent pole ear and the diaphragm are connected by the coating, and the specific first phase change component and the second phase change component with a specific melting point and a specific ratio in the core material cooperate with each other, so that when the pole ear is laser welded to the current collecting assembly, the diaphragm can be avoided from being burned, and the internal short circuit of the battery can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular, to a phase change microcapsule, a diaphragm, a pole piece, a battery and an electrical device. Background Art

[0002] During the battery production process, the current collecting assembly is used to electrically connect the tabs and electrode terminals of the battery cell to transmit electrical energy from the electrode assembly to the electrode terminals, and then to the outside of the battery cell through the electrode terminals; multiple battery cells are electrically connected through the current collecting components to achieve series, parallel or mixed connection of multiple battery cells.

[0003] However, it is found that laser welding of current collector components can easily cause short circuits inside the battery. Summary of the invention

[0004] The present application provides a phase change microcapsule, a diaphragm, a pole piece, a battery and an electrical device, which can avoid the technical problem of short circuit easily caused inside the battery.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, the present application example provides a phase change microcapsule, which includes: a core material and an insulating and heat-conductive wall material wrapping the core material.

[0007] The core material includes a first phase change component and a second phase change component, the first phase change component is paraffin with a melting point of 37-42°C, the second phase change component is paraffin with a melting point of 65-75°C, and the melting point of the insulating heat-conducting wall material is greater than 75°C.

[0008] The mass ratio of the first phase change component to the second phase change component is 35:45-77.

[0009] The beneficial effects of the technical solution of this application include:

[0010] In the present application, a phase change microcapsule with a core-shell structure is provided, which is applied to a battery, such as a lithium battery, in the form of a coating, so that the negative electrode tab of the lithium battery is connected to the diaphragm through the coating, and the first phase change component with a specific melting point and the second phase change component in the core material are matched with each other in a specific ratio, so that when the tab and the current collecting assembly are welded, the first phase change component undergoes a phase change and quickly absorbs heat, buffering the temperature rise rate of the diaphragm, avoiding the instantaneous temperature of the diaphragm being higher than the minimum temperature at which it is scalded before the second phase change component undergoes a phase change, and while keeping the instantaneous temperature of the diaphragm lower than the minimum temperature at which it is scalded, the second phase change component undergoes a phase change to continuously absorb a large amount of heat, avoiding the diaphragm being scalded due to excessive temperature in the later stage of laser welding. At the same time, the melting point of the insulating heat-conductive wall material is greater than 75°C, which can also avoid the insulating heat-conductive wall material being destroyed during the phase change of the core material and flowing out of the insulating heat-conductive wall material.

[0011] That is, the first phase change component and the second phase change component cooperate with each other, can absorb welding heat and can melt in a gradient manner, thereby controlling the temperature rise rate and temperature of the diaphragm, ensuring that the real-time temperature of the diaphragm during welding is always lower than the minimum temperature at which it can be scalded, so as to avoid internal short circuit of the battery caused by scalding the diaphragm.

[0012] In some exemplary embodiments, the first phase change component uses paraffin wax with a structural formula of: n H 2n+2 , where 18≤n≤21; the structural formula of the paraffin used in the second phase change component is: C n’ H 2n’+2 , where 25≤n'≤28.

[0013] The beneficial effects of the above technical solution include: the paraffin wax with the above specific structural formula can better meet the melting point requirements and has the advantages of abundant sources.

[0014] In some exemplary embodiments, the insulating thermally conductive wall material includes a substrate and ceramic particles dispersed in the substrate, and the substrate is a polymer.

[0015] The beneficial effects of the above technical solution include: the introduction of ceramic particles in the wall material, on the one hand, can make the wall material have better high temperature resistance, and at the same time, it is also beneficial for the core material to absorb the heat generated during the welding of the current collecting assembly in time, and on the other hand, it can avoid excessive shrinkage of the part of the diaphragm in contact with the negative electrode sheet during welding.

[0016] Optionally, the polymer comprises a phenolic resin.

[0017] In some exemplary embodiments, in the phase change microcapsules, the mass ratio of the wall material to the core material is 1:3-4.

[0018] The beneficial effects of the above technical solution include: reasonably controlling the ratio range of wall material and core material, controlling the thickness of the wall material under the condition that the particle size of the phase change microcapsule meets the use requirements, ensuring a reasonable thickness of the wall material, ensuring the stability of the phase change microcapsule during use, so that it can protect the diaphragm against instantaneous high temperature during welding.

[0019] In some exemplary embodiments, in the phase change microcapsules, the mass ratio of the substrate to the ceramic particles is 3:4-5, and the mass ratio of the substrate to the core material is 1:2-3.

[0020] The beneficial effects of the above technical solution include: controlling the amount of substrate, ceramic particles and core material within the above range can ensure the stability of the phase change microcapsules, so that they can protect the diaphragm against instantaneous high temperatures during welding.

[0021] In some exemplary embodiments, the ceramic particles include silica particles.

[0022] The beneficial effects of the above technical solution include: silica particles have excellent high temperature resistance, insulation and thermal conductivity, which can improve the high temperature resistance, insulation and thermal conductivity of wall materials, improve the stability and heat absorption capacity of phase change microcapsules when welding current collecting components, and also have the advantages of abundant sources and easy acquisition.

[0023] In some exemplary embodiments, the particle size of the silica particles is 60-90 nm.

[0024] The beneficial effects of the above technical solution include: the silicon dioxide particles with the above specific particle size are conducive to doping and uniform dispersion in the substrate.

[0025] In some exemplary embodiments, the particle size of the phase change microcapsules is 0.5-4 μm.

[0026] The beneficial effects of the above technical solution include: the phase change microcapsules have a suitable particle size, which is convenient for forming a coating and effectively prevents the edge of the diaphragm located on the negative electrode side from being burned when welding the current collecting assembly.

[0027] In a second aspect, the present application provides an example of a diaphragm, the edge of which is provided with a coating, and the coating contains the phase change microcapsules provided in the first aspect of the present application.

[0028] The beneficial effects of the above technical solution include: when the above diaphragm is applied to a battery, the coating on the edge of the diaphragm corresponds to the pole ear with a thermal conductivity of ≥380W / mk. At this time, when welding the current collecting assembly, the coating can absorb the heat transferred from the pole ear to ensure that the real-time temperature of the diaphragm during welding is always lower than the minimum temperature at which it can be scalded, so as to avoid internal short circuit of the battery caused by scalding the diaphragm, and because the coating is mainly located at the edge of the diaphragm, it basically does not affect the performance of the diaphragm itself.

[0029] In some exemplary embodiments, the thickness of the coating is 10-35 μm, optionally 10-20 μm, optionally 25-35 μm.

[0030] The beneficial effects of the above technical solution include: the coating thickness is reasonable, and when the above diaphragm is applied to a battery, when laser welding the pole ear and the current collecting assembly is adopted, not only can the diaphragm be avoided from being burned, but also the size of the edge position of the diaphragm is basically not affected.

[0031] In the third aspect, the example of the present application provides a pole piece, which includes a current collector and a pole ear connected to each other, the thermal conductivity of the pole ear is ≥380W / mk, and at least one side of the pole ear is provided with a coating, and the coating contains the phase change microcapsules provided in the first aspect of the present application.

[0032] The beneficial effects of the above technical solution include:

[0033] Since the thermal conductivity of the tab is ≥380W / mk, it is applied to the battery so that the coating containing phase change microcapsules is set between the tab and the diaphragm, and the diaphragm and the tab are prevented from direct contact. When welding the current collector assembly, the coating can be used to absorb the heat transferred by the tab, so that the real-time temperature of the diaphragm is always lower than the minimum temperature at which it can be burned, so as to avoid internal short circuit caused by burning the diaphragm.

[0034] In some exemplary embodiments, the thickness of the coating is 10-35 μm, optionally 10-20 μm, optionally 25-35 μm.

[0035] The beneficial effects of the above technical solution include: the coating thickness is reasonable, which can not only avoid scalding of the diaphragm matched with the above-mentioned pole lug when welding the current collecting assembly, but also basically does not affect the size of the edge position of the diaphragm matched with the pole lug.

[0036] In a fourth aspect, the present application example provides a battery, which includes a separator and a pole piece, and the pole piece includes a current collector and a pole ear connected to each other.

[0037] There is a coating between the electrode tab and the separator, and the coating is formed on the electrode tab and / or on the separator.

[0038] The coating contains the phase change microcapsules provided in the first aspect of the present application.

[0039] The beneficial effects of the above technical solution include: a coating containing phase change microcapsules can be provided between the tab and the diaphragm, and the coating can absorb the heat transferred from the tab when welding the current collecting assembly, ensuring that the real-time temperature of the diaphragm during welding is always lower than the minimum temperature at which it can be burned, so as to avoid internal short circuit of the battery caused by burning the diaphragm.

[0040] In some exemplary embodiments, the thickness of the coating between the separator and the tab is 20-35 μm.

[0041] The beneficial effects of the above technical solution include: the coating thickness is reasonable, which can not only avoid the edge of the diaphragm that matches the tab from being burned when welding the current collecting assembly, but also basically does not affect the size of the edge position of the diaphragm.

[0042] In a fifth aspect, the present application example provides an electrical device equipped with the battery provided in the fourth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0044] Figure 1 A schematic diagram of the structure of a vehicle according to some embodiments of the present application;

[0045] Figure 2 A schematic diagram of the exploded structure of a battery according to some embodiments of the present application;

[0046] Figure 3 A schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application;

[0047] Figure 4 A schematic diagram of the structure of a wound electrode assembly after unfolding provided in some embodiments;

[0048] Figure 5 A schematic diagram of the structure of the flattened negative electrode region provided in some embodiments;

[0049] Figure 6 This is a scanning electron microscope image of the phase change microcapsule provided in Example 1;

[0050] Figure 7 A photograph of the membrane edge region provided for Examples 2-7 unfolded after welding;

[0051] Figure 8 A photograph of the diaphragm edge region provided for Example 1 and Comparative Examples 1-5 unfolded after welding;

[0052] In the drawings, the drawings are not drawn to scale.

[0053] The reference numerals in the specific implementation manner are as follows:

[0054] 1000-Vehicles;

[0055] 100-battery; 200-controller; 300-motor;

[0056] 10-box; 11-first part; 12-second part;

[0057] 20-battery cell; 21-end cover; 21a-electrode terminal; 22-insulating member; 23-current collecting assembly; 24-housing; 25-electrode assembly;

[0058] 251 - positive electrode current collector; 252 - positive electrode tab; 253 - negative electrode current collector; 255 - negative electrode tab; 256 - separator; 257 - separator edge region; 258 - tab region; 259 - coating. DETAILED DESCRIPTION

[0059] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0061] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.

[0062] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0063] In the description of the embodiments of the present application, the term "plurality" refers to more than two (including two).

[0064] At present, from the perspective of market development, the application of power batteries is becoming more and more extensive. Power batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric cars, as well as military equipment and aerospace and other fields. With the continuous expansion of the application field of power batteries, the market demand is also constantly expanding.

[0065] The inventors have noticed that after laser welding of the current collecting assembly, a short circuit is likely to occur inside the battery. Taking lithium-ion batteries as an example, the inventors have conducted research and found that since the negative electrode tabs of lithium-ion batteries are generally thin copper foils with good thermal conductivity, and the instantaneous temperature is very high during laser welding of the current collecting assembly, holes, excessive shrinkage and other burns may appear on the edges of the diaphragm where the diaphragm contacts the negative electrode tab, thereby causing a short circuit inside the battery.

[0066] Based on the above findings, the inventors tried to set a coating on the edge where the negative electrode tab of the lithium battery and the diaphragm are attached to isolate the two and avoid direct contact between the two, and applied phase change material in the coating to absorb the heat transferred to the tab during laser welding to reduce the temperature of the diaphragm. Theoretically, the above technical problems can be solved by using the phase change heat absorption of the phase change material to reduce the temperature of the diaphragm. However, it was found in actual operation that different phase change materials have different phase change response speeds. The laser welding light emission time is generally 0.1s, and the instantaneous temperature of the light emission can reach 1000°C. As a result, although the final temperature of the diaphragm is lower than the minimum temperature required for it to be burned, during the phase change process, the phase change material cannot respond to the phase change quickly, resulting in the instantaneous temperature of the diaphragm being greater than the minimum temperature required for it to be burned, and the diaphragm still has the problem of being burned.

[0067] Based on this, the applicant provides a phase change microcapsule, which is arranged on the edge of the diaphragm and / or at least one side of the pole ear, assembled into a battery cell and applied to the battery. In the process of connecting the pole ear and the current collecting assembly with a thermal conductivity coefficient ≥380W / mk by laser welding, the first phase change component and the second phase change component with a specific ratio and different melting points in the phase change microcapsule are combined to achieve gradient melting of the first phase change component and the second phase change component, thereby controlling the temperature rise rate of the diaphragm and the real-time temperature of the diaphragm, which can effectively avoid the problem of the diaphragm being burned during laser welding of the current collecting assembly, resulting in internal short circuit of the battery cell.

[0068] The battery disclosed in the embodiment of the present application can be used in, but not limited to, electrical devices such as vehicles, ships or aircraft. A power supply system comprising the battery disclosed in the present application can be used to form the electrical device, which is beneficial to avoid internal short circuits in the battery and improve the stability of battery performance and battery life.

[0069] The embodiment of the present application provides an electric device using a battery as a power source, and the electric device may be, but is not limited to, a mobile phone, a tablet, a laptop, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0070] For the convenience of description, the following embodiments are described by taking a vehicle 1000 as an example of an electrical device according to an embodiment of the present application.

[0071] Please refer to Figure 1 , Figure 1A schematic diagram of the structure of a vehicle 1000 provided for some embodiments of the present application. The vehicle 1000 may be a fuel vehicle, a gas vehicle or a new energy vehicle, and the new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 may be provided at the bottom, head or tail of the vehicle 1000. The battery 100 may be used to power the vehicle 1000, for example, the battery 100 may be used as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300, and the controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.

[0072] In some embodiments of the present application, the battery 100 can not only serve as an operating power source for the vehicle 1000, but also serve as a driving power source for the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.

[0073] Please refer to Figure 2 , Figure 2 An exploded view of a battery 100 provided in some embodiments of the present application. The battery 100 includes a box 10 and a battery cell 20, and the battery cell 20 is contained in the box 10. Among them, the box 10 is used to provide a storage space for the battery cell 20, and the box 10 can adopt a variety of structures. In some embodiments, the box 10 may include a first part 11 and a second part 12, the first part 11 and the second part 12 cover each other, and the first part 11 and the second part 12 jointly define a storage space for accommodating the battery cell 20. The second part 12 may be a hollow structure with one end open, the first part 11 may be a plate-like structure, and the first part 11 covers the open side of the second part 12, so that the first part 11 and the second part 12 jointly define a storage space; the first part 11 and the second part 12 may also be hollow structures with one side open, and the open side of the first part 11 covers the open side of the second part 12. Of course, the box 10 formed by the first part 11 and the second part 12 may be in a variety of shapes, such as a cylinder, a cuboid, etc.

[0074] In the battery 100, there may be multiple battery cells 20, and the multiple battery cells 20 may be connected in series, in parallel, or in a mixed connection. A mixed connection means that the multiple battery cells 20 are both connected in series and in parallel. The multiple battery cells 20 may be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 20 is accommodated in the box 10; of course, the battery 100 may also be a battery module formed by connecting multiple battery cells 20 in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 10. The battery 100 may also include other structures, for example, the battery 100 may also include a busbar component for realizing electrical connection between the multiple battery cells 20.

[0075] Each battery cell 20 may be a secondary battery or a primary battery, or a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto. The battery cell 20 may be cylindrical, flat, rectangular, or in other shapes.

[0076] Please refer to Figure 3 , Figure 3 The schematic diagram of the exploded structure of the battery cell 20 provided in some embodiments of the present application. The battery cell 20 refers to the smallest unit that constitutes the battery. Figure 3 The battery cell 20 includes an end cap 21, an insulating member 22, a current collecting assembly 23, a shell 24, an electrode assembly 25, an electrolyte (not shown) and other functional components.

[0077] The end cap 21 refers to a component that covers the opening of the shell 24 to isolate the internal environment of the battery cell 20 from the external environment. Without limitation, the shape of the end cap 21 can be adapted to the shape of the shell 24 to match the shell 24. Optionally, the end cap 21 can be made of a material with a certain hardness and strength (such as aluminum alloy), so that the end cap 21 is not easily deformed when squeezed and collided, so that the battery cell 20 can have a higher structural strength and the safety performance can also be improved. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for releasing the internal pressure when the internal pressure or temperature of the battery cell 20 reaches a threshold. The material of the end cap 21 can also be a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose any special restrictions on this.

[0078] Functional components such as electrode terminals 21a are provided on the end cap 21. The electrode terminal 21a can be used to electrically connect to the electrode assembly 25 to output or input the electrical energy of the battery cell 20. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for releasing the internal pressure when the internal pressure or temperature of the battery cell 20 reaches a threshold. The material of the end cap 21 can also be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose any special restrictions on this.

[0079] The insulating member 22 is located inside the end cap 21, and can be used to isolate the electrical connection components in the housing 24 from the end cap 21 to reduce the risk of short circuit. For example, the insulating member 22 can be made of plastic, rubber, etc.

[0080] The current collecting assembly 23 is located on a side of the insulating member 22 away from the end cover 21 , and is used to electrically connect the electrode terminal 21 a with the electrode assembly 25 to transmit electrical energy from the electrode assembly 25 to the electrode terminal 21 a , and then to the outside of the electrode assembly 25 via the electrode terminal 21 a .

[0081] The shell 24 is a component used to cooperate with the end cap 21 to form the internal environment of the battery cell 20, wherein the formed internal environment can be used to accommodate the electrode assembly 25, the electrolyte and other components. The shell 24 and the end cap 21 can be independent components, and an opening can be set on the shell 24, and the internal environment of the battery cell 20 is formed by covering the opening with the end cap 21 at the opening. Without limitation, the end cap 21 and the shell 24 can also be integrated. Specifically, the end cap 21 and the shell 24 can form a common connection surface before other components are put into the shell, and when the interior of the shell 24 needs to be encapsulated, the end cap 21 covers the shell 24. The shell 24 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 24 can be determined according to the specific shape and size of the electrode assembly 25. The material of the shell 24 can be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiment of the present application does not impose any special restrictions on this.

[0082] The electrode assembly 25 is a component where an electrochemical reaction occurs in the battery cell 20. One or more electrode assemblies 25 may be contained in the housing 24.

[0083] See also Figure 4 as well as Figure 5 The electrode assembly 25 is mainly formed by winding or stacking a positive electrode sheet and a negative electrode sheet, and a separator 256 is usually provided between the positive electrode sheet and the negative electrode sheet. The positive electrode sheet has a positive electrode collector 251 with a positive electrode active material on the surface, and the negative electrode sheet has a negative electrode collector 253 with a negative electrode active material on the surface. The positive electrode collector 251 coated with the positive electrode active material and the negative electrode collector 253 coated with the negative electrode active material together constitute the main body of the electrode assembly 25. The positive electrode tab 252 and the negative electrode tab 255 are electrically connected to the corresponding positive electrode collector 251 and the negative electrode collector 253 respectively, and there is no active material on the surface.

[0084] The positive electrode tab 252 and the negative electrode tab 255 can be located at one end of the main body or at both ends of the main body. During the charge and discharge process of the battery 100, the positive electrode active material and the negative electrode active material react with the electrolyte, and the tab 23a connects the electrode terminal 21a to form a current loop.

[0085] Taking the battery cell 20 as a lithium-ion battery as an example, optionally, the thermal conductivity of the negative electrode tab 255 is ≥380 W / mk.

[0086] The wound electrode assembly 25 is unwound to obtain Figure 4 , Figure 4 2 is a schematic diagram of the structure of the electrode assembly 25 after it is unfolded. The separator 256 has a separator edge area 257. In actual use, when the separator 256 is applied to a wound battery, the edge of the separator 256 is the long edge of the separator 256 close to the negative electrode tab 255 with a thermal conductivity of ≥380W / mk. When the separator 256 is applied to a laminated battery, the edge is the edge of the separator 256 close to the negative electrode tab 255 with a thermal conductivity of ≥380W / mk.

[0087] according to Figure 4 The negative electrode sheet has a tab area 258. Before the tab area 258 is bent, the diaphragm 256 faces and extends out of the negative electrode current collector 253 and an edge thereof that is used to fit with the negative electrode tab 255 serves as a diaphragm edge area 257. A coating 259 containing phase change microcapsules is applied to the diaphragm edge area 257.

[0088] Since the length of the diaphragm 256 extending out of the electrode tab does not exceed 4 mm, therefore, 4 mm ≤ the width of the diaphragm edge area 257 ≤ 8 mm, with the end of the diaphragm 256 extending out of the negative electrode tab 255 as the first end, and the other end opposite to the first end as the second end, and the diaphragm 256 extending from the first end to the second end. The width here refers to the distance extending from the first end of the diaphragm 256 in the above-mentioned extension direction.

[0089] The diaphragm edge area 257 and the negative electrode tab 255 are bent at the same time to obtain Figure 5 The schematic diagram of the structure of the flattened negative electrode region is shown in FIG. Figure 5 The tab region 258 includes a diaphragm edge region 257 , a coating 259 and a negative electrode tab 255 . The coating 259 of the tab region 258 is located directly below the negative electrode tab 255 , and the negative electrode tab 255 is bonded to the diaphragm edge region 257 via the coating 259 .

[0090] The thickness of the coating 259 may be 25-35 μm, for example, 30 μm.

[0091] At this time, the negative electrode tab 255 in the flattened negative electrode area is laser welded to the current collecting assembly 23. Since the laser is shot downward from directly above the current collecting assembly 23, the current collecting assembly 23 and the negative electrode tab 255 are welded together. At this time, the heat will be transferred from the current collecting assembly 23 to the negative electrode tab 255, and then the negative electrode tab 255 transfers the heat to the coating 259 and is absorbed by the coating 259, thereby protecting the diaphragm edge area 257 located in the tab area 258.

[0092] According to some embodiments of the present application, the present application provides a phase-change microcapsule, which includes: a core material and an insulating heat-conducting wall material wrapping the core material. The core material includes a first phase-change component and a second phase-change component, the first phase-change component is paraffin with a melting point of 37-42°C, the second phase-change component is paraffin with a melting point of 65-75°C, and the melting point of the insulating heat-conducting wall material is greater than 75°C. The mass ratio of the first phase-change component to the second phase-change component is 35:45-77.

[0093] The core material refers to the contents encapsulated in the insulating and heat-conducting wall material.

[0094] The phase change microcapsules provided in this application are of core-shell structure. When applied to batteries, the wall material is insulating under the working conditions of the battery, that is, it has good resistivity, for example, the resistivity is 1013Ω·cm-1014Ω·cm, so that the phase change microcapsule coating has excellent insulation effect as a whole. The wall material has good thermal conductivity, for example, the thermal conductivity is 0.22W / mK or higher than 0.22W / mK, etc., so that the phase change microcapsules have good heat absorption effect, and can timely absorb the heat generated during the welding of the current collecting assembly to achieve the purpose of preventing the diaphragm from being burned. At the same time, the wall material is inert under the working state of the battery and does not react with the electrolyte, etc. At the same time, the melting point of the wall material is greater than 75°C, so that in the process of laser welding to connect the pole ear and the current collecting assembly with a thermal conductivity of ≥380W / mk, the core material that has undergone phase change and is molten will not destroy the insulating heat-conducting wall material and flow out of it.

[0095] The core material includes a first phase change component and a second phase change component. Since both the first phase change component and the second phase change component are paraffin wax, they are easy to mix evenly. The first phase change component is paraffin wax with a melting point of 37-42°C, and the second phase change component is paraffin wax with a melting point of 65-75°C. Both of them not only have good thermal phase transition performance, but also have a high endothermic value during the transition process, and the highest melting point of the first phase change component is significantly lower than the lowest melting point of the second phase change component, so that when the laser welding collector assembly is performed, the first phase change component with a lower temperature first undergoes a rapid phase change response, absorbs enough heat to phase change into a liquid state, so as to buffer the temperature rise rate of the diaphragm and control the real-time temperature of the diaphragm, and then the second phase change component absorbs a large amount of heat to phase change into a liquid state, further slowing down the temperature rise rate of the diaphragm and controlling the real-time temperature of the diaphragm, that is, when the temperature is higher than the melting point of the first phase change component and the second phase change component, the first phase change component and the second phase change component change from solid to liquid. Since the first phase change component and the second phase change component are evenly distributed, they can be in a gradient melting state as a whole during the temperature increase process, so as to control the real-time temperature of the diaphragm to always be lower than the minimum temperature at which the diaphragm is burned. At the same time, the core material as a whole will be sealed in the chemically inert wall material.

[0096] The ratio of the first phase change component and the second phase change component affects the temperature rise rate and temperature of the diaphragm during the welding of the current collecting assembly. The ratio of the first phase change component and the second phase change component is reasonable. Under the premise of avoiding the diaphragm heating rate being too fast, the core material's overall heat absorption capacity is guaranteed to be good, thereby effectively reducing the diaphragm temperature. If the proportion of the first paraffin component is too high, the core material's overall heat absorption capacity will be insufficient, causing the diaphragm's real-time temperature to be higher than its lowest scalding temperature. If the proportion of the first paraffin component is too low, the second phase change component has a short phase change response time, so that before the second phase change component responds to the phase change, the diaphragm will heat up quickly and its real-time temperature will shock to a temperature higher than its lowest scalding temperature, which may cause diaphragm scalding.

[0097] Optionally, the mass ratio of the first phase change component to the second phase change component is any ratio of 35:45, 35:47, 35:50, 35:55, 35:60, 35:65, 35:70, 35:75, 35:77 or between any two ratios.

[0098] Among them, it should be noted that there are many types of paraffins with a melting point of 37-42°C. The first phase change component can be a specific paraffin with a melting point within 37-42°C, or it can be a mixture of at least two specific paraffins with melting points between 37-42°C in any ratio. Similarly, the composition of the second phase change component can be obtained, which is not limited here.

[0099] According to some embodiments of the present application, optionally, the first phase change component uses paraffin wax with the structural formula: C n H 2n+2, where 18≤n≤21; the structural formula of the paraffin used in the second phase change component is: C n’ H 2n’+2 , where 25≤n'≤28.

[0100] According to some embodiments of the present application, optionally, in the phase change microcapsule, the mass ratio of the wall material to the core material is 1:3-4. For example, in the phase change microcapsule, the mass ratio of the wall material to the core material is any ratio of 1:3, 1:3.3, 1:3.5, 1:3.7, 1:3.9, 1:4 or between any two ratios.

[0101] Under the condition that the particle size of the phase-change microcapsules is constant, the thickness of the wall material can be limited by using the above ratio, thereby improving the stability of the phase-change microcapsules.

[0102] According to some embodiments of the present application, optionally, the thermally conductive wall material includes a substrate and ceramic particles dispersed in the substrate, and the substrate is a polymer.

[0103] The ceramic particles are particles made of ceramic materials with high temperature resistance and thermal conductivity. The material of the ceramic particles includes but is not limited to at least one of boron nitride, silicon nitride, silicon carbide, silicon dioxide, etc.

[0104] The polymer is compatible with paraffin and is insulating.

[0105] According to some embodiments of the present application, optionally, the polymer includes a phenolic resin, that is, the polymer includes but is not limited to a phenolic resin, and may also be any one of a polyacrylonitrile resin, a melamine formaldehyde resin, and a phenolic resin polymer.

[0106] Under the above settings, the wall material not only has better insulation, but also the introduction of ceramic particles can make the wall material have better high temperature resistance, and also help the core material to absorb the heat generated by the welding of the current collector in time, and on the other hand, avoid excessive shrinkage of the part of the diaphragm in contact with the negative electrode during welding. In addition, the setting of the polymer as the base material ensures that the wall material has good compatibility with paraffin, can form a stable interface with it, and improve the thermal stability of the phase change microcapsules.

[0107] Optionally, the polymer is a phenolic resin.

[0108] The substrate of the above material has better compatibility with paraffin wax, and also facilitates the uniform dispersion of ceramic particles, thereby ensuring the stability of the phase change microcapsules.

[0109] According to some embodiments of the present application, optionally, in the phase change microcapsule, the mass ratio of the substrate to the ceramic particles is 3:4-5, and the mass ratio of the substrate to the core material is 1:2-3. For example, in the phase change microcapsule, the mass ratio of the substrate to the ceramic particles is any ratio of 3:4, 3:4.3, 3:4.5, 3:4.6, 3:4.9, 3:5 or between any two ratios, and the mass ratio of the substrate to the core material is any ratio of 1:2, 1:2.3, 1:2.5, 1:2.7, 1:2.9, 1:3 or between any two ratios.

[0110] By controlling the amount of substrate, ceramic particles and core material within the above range, the stability of the phase change microcapsule can be ensured, so that it can play the role of protecting the diaphragm against the instantaneous high temperature during welding.

[0111] According to some embodiments of the present application, the ceramic particles are optionally silicon dioxide particles. Silicon dioxide particles have excellent high temperature resistance, insulation and thermal conductivity, which can improve the high temperature resistance, insulation and thermal conductivity of the wall material, improve the stability and heat absorption capacity of the phase change microcapsules when welding the current collecting components, and also have the advantages of abundant sources and easy acquisition.

[0112] Optionally, the particle size of the silica particles is 60-90 nm. The particle size here refers to the average particle size of the silica particles. For example, the particle size of the silica particles is any value of 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 83 nm, 85 nm, 90 nm or between any two values. The silica particles of the above specific particle size are conducive to doping and uniform dispersion in the substrate.

[0113] According to some embodiments of the present application, the particle size of the phase change microcapsules is optionally 0.5-4 μm, where the particle size is the average particle size of the phase change microcapsules. Phase change microcapsules of this specification are convenient for forming a coating located at the edge of the tab and the diaphragm, effectively avoiding burns to the edge of the diaphragm that matches the tab when the tab and the current collecting assembly are laser welded.

[0114] The phase change microcapsules can be obtained by in-situ polymerization, where the wall material covers the core material.

[0115] The in-situ polymerization method is as follows: one or more mixtures of phase change materials can be dispersed in water under the action of an emulsifier to form an oil-in-water emulsion, one or more water-soluble monomers or resin low molecular weight prepolymer aqueous solutions are added dropwise in one step or in steps to the emulsion, the stirring speed, reaction temperature, pH, etc. of the system are adjusted to cause a condensation reaction, and small molecules (such as water molecules) are further removed from the prepolymer molecules to form a non-water-soluble condensation polymer with a cross-linked three-dimensional network structure at the emulsion interface, that is, a phase change microcapsule encapsulated with a phase change material is formed.

[0116] In some exemplary embodiments, the method for preparing phase change microcapsules comprises the following steps:

[0117] The ceramic particles are dispersed in water to form an aqueous phase.

[0118] The first phase change component and the second phase change component are mixed and heated to a molten state to form an oil phase.

[0119] The aqueous phase and the oil phase are mixed and stirred to form a Pickering emulsion, and a low molecular weight prepolymer aqueous solution of the resin is added to the Pickering emulsion, and the polymerization is carried out by stirring at room temperature for at least 4 hours.

[0120] In some other exemplary embodiments, the method for preparing phase change microcapsules comprises the following steps:

[0121] The ceramic particles are dispersed in water to form an aqueous phase.

[0122] The first phase change component, the second phase change component, the synthetic monomer of the polymer, the crosslinking agent and the initiator are mixed and heated to a molten state to form an oil phase.

[0123] The aqueous phase and the oil phase are mixed and stirred to form a Pickering emulsion, and then polymerized at 60-80°C with stirring.

[0124] The in-situ polymerization method is used to form a polymer on the surface of the core material, which can ensure that the wall material is wrapped around the core material to form a core-shell structure. It is easy to obtain the first phase change component and the second phase change component that are evenly mixed and wrapped in the wall material. At the same time, the preparation method is controllable and can be mass-produced.

[0125] It should be noted that after the polymer is formed on the surface of the core material by the in-situ polymerization method, if the phase change microcapsules are not used temporarily, the phase change microcapsule powder can be dried to facilitate storage and transportation. When used, it can be mixed with a binder to form a slurry according to actual needs. If phase change microcapsules are needed, after the polymer is formed on the surface of the core material by the in-situ polymerization method, there is no need to dry it. The binder can be directly added to the phase change microcapsule emulsion formed after the polymerization, and the mixture can be used to form a slurry.

[0126] The binder is used to fix the phase change microcapsules on the diaphragm or the tab. The binder includes but is not limited to water-based styrene-butadiene rubber (SBR) binder and sodium carboxymethyl cellulose (CMC). For example, the binder is a single SBR binder, or a mixture of CMC and SBR in a mass ratio of 3:6-8.

[0127] According to some embodiments of the present application, the present application provides a diaphragm, wherein an edge of the diaphragm is provided with a coating, and the coating contains phase change microcapsules.

[0128] In actual use, for example, when the diaphragm is applied to a wound battery, the edge of the diaphragm is the long side edge of the diaphragm close to the tab with a thermal conductivity of ≥380W / mk. When the diaphragm is applied to a laminated battery, the edge is the edge of the diaphragm close to the tab with a thermal conductivity of ≥380W / mk.

[0129] The coating includes a substrate and phase change microcapsules dispersed in the substrate. The substrate refers to a material that can disperse the aforementioned phase change microcapsules and can form a film and adhere to the surface of the diaphragm, such as a binder, and the binder is, for example, SBR binder and / or CMC, etc. SBR binder has excellent thermal stability, and SBR binder and CMC are highly compatible with phase change capsules. The diaphragm material includes but is not limited to polypropylene (PP) or polyethylene (PE), etc., which can be selected according to actual needs and are not limited here.

[0130] In actual use, when the tab with a thermal conductivity of ≥380W / mk is a full tab, the coating completely covers the edge of the diaphragm, wherein the full tab means that the edge of the current collector is used as the tab. When the tab with a thermal conductivity of ≥380W / mk is a single-pole tab or a multi-pole tab, the coating can completely cover the edge of the diaphragm, so that after the tab is bent, the diaphragm and the tab can be completely isolated by the coating, or the coating is only provided on the portion corresponding to the edge and the tab, or the diaphragm and the tab can be completely isolated by the coating, wherein a single tab means that only one tab is extended from each pole sheet for current conduction. Multi-pole tabs mean that at least two tabs are extended from each pole sheet for current conduction.

[0131] According to some embodiments of the present application, optionally, the thickness of the coating is 10-35 μm, optionally 10-20 μm, or optionally 25-35 μm.

[0132] When assembling the battery, when both the diaphragm and the tab are coated, the thickness of the coating formed on the diaphragm is 10-20 μm, and when only the diaphragm is coated but the tab is not coated, the thickness of the coating formed on the diaphragm is 25-35 μm, for example, the thickness of the coating is any value of 25 μm, 27 μm, 28 μm, 30 μm, 35 μm or between any two values. The above coating thickness is reasonable, ensuring effective regulation of the temperature and temperature rise rate of the diaphragm, while substantially not affecting the size of the diaphragm edge position.

[0133] Optionally, the coating can be prepared in the following manner: the phase change microcapsules and the binder provided in the first aspect are mixed in a mass ratio of, for example, 1:7-9 to form a coating slurry, and the coating slurry is then applied to the edge of the diaphragm and dried; or, the binder is directly added to the phase change microcapsule emulsion formed after polymerization, for example, CMC dry powder is first added, and after the CMC is completely dissolved, SBR emulsion is added, wherein the CMC / SBR mass ratio is 3:7, to form a coating slurry, and the coating slurry is then applied to the edge of the diaphragm and dried at 70-80°C.

[0134] According to some embodiments of the present application, optionally, the present application provides a pole piece, which includes a current collector and a pole ear connected to each other, the thermal conductivity of the pole ear is ≥380W / mk, and at least one side of the pole ear is provided with a coating, and the coating contains the phase change microcapsules provided in the first aspect of the present application.

[0135] The coating includes a substrate and phase change microcapsules dispersed in the substrate. The substrate refers to a material that can disperse the aforementioned phase change microcapsules and form a film and adhere to the surface of the diaphragm, such as a binder, and the binder is, for example, an SBR binder, which has excellent thermal stability and strong compatibility with the phase change capsules.

[0136] After the electrode is assembled to the battery, in order to further avoid contact between the electrode and the separator, the coating can extend from the electrode ear to the current collector.

[0137] After the electrode piece is assembled to the battery, the length of the diaphragm extending out of the electrode ear generally does not exceed 4mm. Therefore, the width of the coating on the electrode ear can be 1mm≤4mm, and the width of the coating on the current collector can be 0≤4mm, that is, the total width of the coating can be 4mm≤8mm, where the coating width is the distance from the end of the coating close to the current collector to the end away from the current collector.

[0138] Among them, the thermal conductivity of the tab is ≥380W / mk, that is, the tab is a high thermal conductivity metal, and the material of the tab can be copper, silver, silver-plated copper, etc.

[0139] Optionally, the material of the tab is copper.

[0140] The tab and the current collector can be connected by welding or formed in one piece.

[0141] Among them, the pole piece can be a single-pole ear pole piece, a multi-pole ear pole piece or a full-pole ear pole piece, which is not limited here.

[0142] According to some embodiments of the present application, optionally, the thickness of the coating is 10-35 μm, optionally 10-20 μm, or optionally 25-35 μm.

[0143] When assembling the battery, when both the diaphragm and the tab are coated, the thickness of the coating formed on the tab is 10-20 μm, and when only the tab is coated but the diaphragm is not coated, the thickness of the coating formed on the tab is 25-35 μm, for example, the thickness of the coating is any value of 25 μm, 27 μm, 28 μm, 30 μm, 35 μm or between any two values. The above coating thickness is reasonable, effectively adjusts the temperature and temperature rise rate of the diaphragm, and basically does not affect the size of the edge position of the diaphragm matching the tab.

[0144] Optionally, the coating can be prepared in the following manner: the phase change microcapsules and the binder provided in the first aspect are mixed in a mass ratio of, for example, 1:7-9 to form a coating slurry, and the coating slurry is then applied to the tab and dried; or, the binder is directly added to the phase change microcapsule emulsion formed after polymerization, for example, CMC dry powder is added first, and after the CMC is completely dissolved, SBR emulsion is added, wherein the CMC / SBR mass ratio is 3:7, to form a coating slurry, and the coating slurry is then applied to the tab and dried at 70-80°C.

[0145] According to some embodiments of the present application, optionally, the present application provides a battery, which includes a diaphragm and a pole piece, the pole piece includes a current collector and a pole ear connected to each other, the thermal conductivity of the pole ear is ≥380W / mk; there is a coating between the pole ear and the diaphragm, the coating is formed on the pole ear and / or on the diaphragm; the coating contains the phase change microcapsules provided in the first aspect of the present application.

[0146] The coating is used to separate the edge of the diaphragm and the pole ear to avoid direct contact between the two. When welding the current collecting assembly, the coating absorbs the heat transferred from the pole ear, reduces the heat transferred to the diaphragm, and controls the temperature rise rate of the diaphragm, ensuring that the real-time temperature of the diaphragm during welding is always lower than the minimum temperature at which it can be burned, thereby avoiding internal short circuits caused by burning the diaphragm.

[0147] Optionally, the thickness of the coating between the diaphragm and the pole piece is 20-35 μm, for example, the thickness of the coating is any value of 20 μm, 25 μm, 28 μm, 30 μm, 32 μm, 35 μm or between any two values. The above coating thickness is reasonable to ensure effective regulation of the temperature and temperature rise rate of the diaphragm, while substantially not affecting the size of the diaphragm edge position.

[0148] In some embodiments, the coating is formed only on one side of the electrode tab and is located between the electrode tab and the separator. In this case, the thickness of the coating is 20-35 μm.

[0149] In some embodiments, the coating is formed only on the edge of the separator and between the tab and the separator. In this case, the thickness of the coating is 20-35 μm.

[0150] In some embodiments, the tab forms a first coating, the edge of the diaphragm forms a second coating, the first coating and the second coating are bonded together, wherein the first coating has a thickness of 10-20 μm, the second coating has a thickness of 10-20 μm, and the total thickness of the first coating and the second coating is 20-35 μm.

[0151] According to some embodiments of the present application, optionally, the present application example provides an electrical device equipped with a battery according to any of the above solutions.

[0152] The power-consuming device may be any of the aforementioned devices or systems using batteries.

[0153] The phase change microcapsule, diaphragm, electrode, battery and electrical device of the present application are further described in detail below in conjunction with the embodiments.

[0154] Examples 1-6

[0155] A phase-change microcapsule is prepared by the following method:

[0156] The silica particles shown in Table 1 were dispersed in 100 g of water to form an aqueous phase.

[0157] The first phase change component and the second phase change component shown in Table 1 were mixed and then heated to 75° C. to form a molten oil phase.

[0158] After the oil phase and the water phase are mixed, they are stirred at high speed for 10 minutes with the stirring speed not less than 5000 rar / min to obtain a Pickering emulsion.

[0159] Emulsifier and phenolic resin were added to the Pickering emulsion, and then polymerized at 25°C for 5 hours to obtain a phase change microcapsule emulsion. The amount of emulsifier added in Table 1 is the mass percentage of the corresponding Pickering emulsion.

[0160] Table 1 Ingredients and their ratio parameters

[0161]

[0162] Among them, the melting point of the first phase change material in Example 7 is 37°C / 39°C, which means that paraffin with a melting point of 37°C and paraffin with a melting point of 39°C are mixed in a mass ratio of 1:1, and the melting point of the first phase change material is 65°C / 70°C, which means that paraffin with a melting point of 65°C and paraffin with a melting point of 70°C are mixed in a mass ratio of 1:1.

[0163] The phase-change microcapsule emulsion of Example 1 was dried to obtain Figure 6 . Figure 6 The scanning electron microscope image of the phase change microcapsule obtained in Example 1 is shown in FIG. Figure 6 , it can be seen that the particle size of the phase change microcapsules is 0.5-4μm.

[0164] Comparative Examples 1-5

[0165] The only difference between Comparative Example 1 and Example 1 is that paraffin with a melting point of 40° C. is used to replace the core material in Example 1.

[0166] The difference between Comparative Example 2 and Example 1 is that the core material is paraffin with a melting point of 70° C. instead of the core material in Example 1.

[0167] The only difference between Comparative Example 3 and Example 1 is that the core material is paraffin with a melting point of 52° C. instead of the core material in Example 1.

[0168] The only difference between Comparative Example 4 and Example 1 is that the mass ratio of the first phase change component to the second phase change component is 35:80.

[0169] The only difference between Comparative Example 5 and Example 1 is that the mass ratio of the first phase change component to the second phase change component is 50:45.

[0170] Test Example 1

[0171] The phase change microcapsule emulsions prepared in Examples 1-7 and Comparative Examples 1-5 were first added with CMC dry powder shown in Table 2, and after the CMC dry powder was dissolved, the SBR emulsion shown in Table 2 was added to obtain a slurry. The slurry was applied to the edge of a diaphragm of the same specifications (diaphragm dimensions: length 9310 mm, width 128.5 mm, material PP, and width of the diaphragm edge 8 mm), and dried so that a 20 μm thick coating containing the above-mentioned phase change microcapsules was present between the edge of the diaphragm and the copper foil (as a tab, the thermal conductivity of the copper foil was 400 W / (m*K)). After flattening, the side of the copper foil facing away from the diaphragm was fastened to the collector plate, and then a laser with the same parameters was used to shoot downward from directly above the collector plate of the same specifications and material, and the collector plate and the copper foil were connected by laser welding (light emission time 0.1 s, light emission instantaneous temperature 1000°C). After welding, the diaphragm was unfolded to observe the changes on the side of the diaphragm facing away from the coating.

[0172] Among them, the addition amounts of SBR emulsion and CMC dry powder in Comparative Examples 1-5 and Example 1 are the same.

[0173] Table 2 Addition amount of CMC dry powder and SBR emulsion

[0174]

[0175]

[0176] The test results are as follows Figure 7 as well as Figure 8 As shown, since the tabs need to be flattened and then unfolded during the test, it is inevitable that there are creases on the surface of the diaphragm.

[0177] according to Figure 7 as well as Figure 8 It can be clearly seen that the edges of the diaphragms of Examples 1-7 are smooth and free of burns. Figure 8 , wherein the frame line indicates the burned portion of the diaphragm edge, wherein the diaphragm edge areas of Comparative Examples 1-5 all have different degrees of shrinkage and gaps caused by the burns compared to Example 1.

[0178] It is explained that the phase change microcapsules provided in the present application can be applied to batteries in the form of a coating, so that the bent pole ear and the diaphragm are connected by bonding the coating, and the specific first phase change component and the second phase change component with a specific melting point and a specific ratio in the core material cooperate with each other, so that the diaphragm can be avoided from being burned when the pole ear is laser welded to the current collecting assembly, thereby avoiding internal short circuit of the battery.

[0179] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A phase change microcapsule, characterized in that: include: A core material and an insulating heat-conducting wall material wrapping the core material; The core material includes a first phase change component and a second phase change component, the first phase change component is paraffin with a melting point of 37-42°C, the second phase change component is paraffin with a melting point of 65-75°C, and the melting point of the insulating heat-conducting wall material is greater than 75°C; The mass ratio of the first phase change component to the second phase change component is 35:45-77.

2. The phase change microcapsule according to claim 1, characterized in that: The structural formula of the paraffin used in the first phase change component is: n H 2n+2 , where 18≤n≤21; The structural formula of the paraffin used in the second phase change component is: n’ H 2n’+2 , where 25≤n'≤28.

3. The phase change microcapsule according to claim 1, characterized in that: In the phase-change microcapsule, the mass ratio of the wall material to the core material is 1:3-4.

4. The phase-change microcapsule according to any one of claims 1 to 3, characterized in that: The insulating heat-conducting wall material comprises a substrate and ceramic particles dispersed in the substrate, and the substrate is a polymer.

5. The phase change microcapsule according to claim 4, characterized in that: The polymer includes a phenolic resin.

6. The phase change microcapsule according to claim 4, characterized in that: In the phase-change microcapsules, the mass ratio of the substrate to the ceramic particles is 3:4-5, and the mass ratio of the substrate to the core material is 1:2-3.

7. The phase-change microcapsule according to claim 4, characterized in that: The ceramic particles include silicon dioxide particles.

8. The phase change microcapsule according to claim 7, characterized in that: The particle size of the silicon dioxide particles is 60-90 nm.

9. The phase-change microcapsule according to any one of claims 1 to 3, characterized in that: The particle size of the phase change microcapsule is 0.5-4 μm.

10. A diaphragm, characterized in that: The edge of the diaphragm is provided with a coating, and the coating contains the phase change microcapsule according to any one of claims 1-9.

11. The diaphragm according to claim 10, characterized in that The coating has a thickness of 10-35 μm.

12. The diaphragm according to claim 10, characterized in that The coating has a thickness of 10-20 μm.

13. The diaphragm according to claim 10, characterized in that The coating has a thickness of 25-35 μm.

14. A pole piece, characterized in that: The pole piece includes a current collector and a pole ear that are connected to each other. The thermal conductivity of the pole ear is ≥380W / mk. At least one side of the pole ear is provided with a coating, and the coating contains the phase change microcapsule according to any one of claims 1-9.

15. The pole piece according to claim 14, characterized in that: The coating has a thickness of 10-35 μm.

16. The pole piece according to claim 14, characterized in that: The coating has a thickness of 10-20 μm.

17. The pole piece according to claim 14, characterized in that: The coating has a thickness of 25-35 μm.

18. A battery, characterized in that: It includes a diaphragm and a pole piece, wherein the pole piece includes a current collector and a pole ear connected to each other; There is a coating between the electrode tab and the diaphragm, and the coating is formed on the electrode tab and / or on the diaphragm; The coating contains the phase change microcapsules according to any one of claims 1 to 9.

19. The battery according to claim 18, characterized in that The thickness of the coating between the separator and the tab is 20-35 μm.

20. An electrical device, characterized in that: Equipped with a battery as claimed in any one of claims 18 to 19.

Citation Information

Patent Citations

  • Power battery diaphragm and preparation method thereof as well as power battery comprising power battery diaphragm

    CN105355824A

  • Preparation method of phase change microcapsule for improving safety of lithium battery

    CN111378418A

  • Phase change temperature control type electrode, preparation method thereof and lithium ion battery

    CN111430709A

  • Low-melting-point metal phase change microcapsule as well as preparation method and application thereof

    CN112226208A

  • Preparation method of heat-conducting wave-absorbing phase-change composite material, and composite material

    CN112300501A