Magnetic drug-loaded nanoparticles for drug-coated balloons and preparation method thereof
By spraying magnetic drug-loaded nanoparticles on drug-coated balloons and using external magnetic fields to guide them, the problem of low drug utilization is solved, drug targeting and sustained release are achieved, and the therapeutic effect on atherosclerosis is improved. .
Patent Information
- Application Number
- CN202211537034.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-02
AI Technical Summary
During the intravascular delivery of drugs by drug-coated balloons, the drug utilization rate is low, and the addition of polymers or adhesives leads to difficulty in drug release and poor biocompatibility, making it difficult to achieve targeted release.
Magnetic drug-loaded nanoparticles are prepared and fixed on the lesion site under the action of an external magnetic field to slowly and efficiently release the drug and improve the bioavailability of the drug. The method includes dissolving, mixing, precipitating, filtering and drying magnetic nanoparticles and antioxidant agents in a specific ratio, spraying them on the surface of the drug-coated balloon, and using magnetic field guidance to achieve targeting and sustained release.
Improves the bioavailability of drugs and enhances the therapeutic effect on atherosclerotic plaques. By loading antioxidant agents on the surface of magnetic nanoparticles, it blocks the properties of peroxidase, reduces adverse effects on the body, and improves Effectiveness of magnetic nanoparticles.
Smart Images

Figure GDA0004072079890000071 
Figure HDA0004072079900000011 
Figure HDA0004072079900000012
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of medical devices, and in particular relates to magnetic drug-loaded nanoparticles used in drug-coated balloons and a preparation method thereof. Background Art
[0002] With the change of people's living and working methods, cardiovascular diseases have gradually become a huge threat to human health. Among them, atherosclerotic cardiovascular diseases account for more than 90%. From a pathological point of view, atherosclerosis is a chronic arterial inflammation secondary to oxidative stressors, which occurs limitedly in the bends or branches of large and medium-sized arteries, causing blockage and rupture of blood vessels. At present, the clinical treatment methods for atherosclerosis are drug therapy and surgical treatment. Among them, percutaneous coronary transluminal angioplasty (PCTA) is widely used due to its advantages of low risk factor, rapid effect, low trauma, and fast recovery. However, the use of metal or non-metallic structural stents in PCTA surgery inevitably damages the inner wall of the blood vessel, leading to restenosis. Even drug-eluting stents loaded with anti-proliferative drugs have the risk of restenosis and late thrombosis.
[0003] Drug-coated balloon (DCB) is a new type of drug-carrying device developed in recent years for the field of coronary intervention. During the treatment process, DCB expands the diseased blood vessels and releases the anti-endothelial cell proliferation drug coated on its surface, thereby inhibiting endothelial cell proliferation. Compared with other coronary intervention devices, DCB has the advantages of no foreign body residue in the body, no stent thrombosis, short dual antiplatelet time, low bleeding risk, wider application range, and reduced restenosis incidence. However, due to the blood flow in the blood vessels, a large amount of drugs will be washed away during the balloon drug delivery process, and the drug utilization rate is low. In order to improve the drug utilization problem, some studies have added polymers, adhesives, etc. between the drug and the coating to enhance the adsorption of the drug, but this has led to new problems such as difficulty in drug release and poor biocompatibility. Therefore, how DCB can achieve targeted drug release has become the key to improving drug utilization. Summary of the invention
[0004] In view of the above problems existing in the prior art, the present invention provides a magnetic drug-loaded nanoparticle for use in drug-coated balloons and a preparation method thereof. The drug-loaded nanoparticle can be fixed at the lesion site under the action of an external magnetic field, slowly and efficiently release the carried drug, improve the bioavailability of the drug, and effectively solve the problem of poor drug utilization in existing drug administration methods.
[0005] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:
[0006] A method for preparing magnetic drug-loaded nanoparticles for drug-coated balloons comprises the following steps:
[0007] (1) dissolving the magnetic nanoparticles and the antioxidant agent in a solvent respectively to prepare a solution 1 and a solution 2, and mixing the solution 1 and the solution 2 to prepare a mixture solution 1;
[0008] (2) dissolving the agent, and then adding the mixture solution 1 in step (1) thereto, mixing well to obtain a mixture solution 2, allowing the mixture solution 2 to stand to form a precipitate, filtering and washing the precipitate, and drying to obtain.
[0009] Furthermore, in step (1), the mass ratio of the magnetic nanoparticles to the antioxidant agent in the mixture solution 1 is 1:1-5.
[0010] Furthermore, the magnetic nanoparticles in step (1) are ferroferric oxide, ferrous sulfide or nano-NdFeB nanoparticles, and the particle size of the magnetic nanoparticles is 10-200 nm.
[0011] Furthermore, the antioxidant agent in step (1) is an agent containing a catechol group.
[0012] Furthermore, the antioxidant agent in step (1) is one of epigallocatechin gallate, dopamine, tannic acid, gallic acid, apple polyphenols, pomegranate polyphenols, tea polyphenols, chlorogenic acid or cocoa polyphenols.
[0013] Furthermore, in step (1), the solvent is a Tris buffer solution.
[0014] Furthermore, the mixing method in step (1) or step (2) is an intermittent ultrasonic method, specifically: each ultrasonic treatment is 50-70 minutes, and then allowed to stand for 10-20 minutes, and repeated 3-5 times.
[0015] Furthermore, the drug in step (2) is paclitaxel, rapamycin, doxorubicin, aspirin or a statin.
[0016] Furthermore, in step (2), the mass ratio of the drug to the magnetic nanoparticles in the second mixed solution is 1:4-6.
[0017] A magnetic drug-loaded nanoparticle used in a drug-coated balloon is prepared by the above-mentioned preparation method.
[0018] The beneficial effects produced by the present invention are:
[0019] In the present invention, an antioxidant agent is loaded on the surface of the magnetic nanoparticles. The catechol structure on the antioxidant agent can coordinate with iron ions to prevent the inherent peroxidase characteristics of the magnetic nanoparticles from promoting the Fenton reaction in the body to generate ROS, which has an adverse effect on atherosclerotic plaques and also improves the effectiveness of the magnetic nanoparticles. The agent is loaded on the surface of the magnetic nanoparticles through adsorption to exert a therapeutic effect on intravascular stenosis.
[0020] In the present invention, antioxidant agents, disease treatment agents and magnetic nanoparticles are loaded together to construct a nano drug delivery system, which is sprayed onto the surface of the drug-coated balloon. Under the guidance of the magnetic field, the drug's targeting and sustained release effects are achieved, which can maximize the bioavailability of the drug and improve the therapeutic effect on atherosclerosis. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the UV absorption spectrum of Fe3O4-EGCG-PTX and Fe3O4-EGCG;
[0022] Figure 2 The infrared spectra of Fe3O4-EGCG-PTX, Fe3O4-EGCG and Fe3O4;
[0023] Figure 3 The microscopic morphology of Fe3O4 nanoparticles and Fe3O4-EGCG-PTX nanoparticles;
[0024] Figure 4 is the linear regression equation of EGCG concentration and absorbance (A);
[0025] Figure 5 This is the zeta potential diagram of Fe3O4 nanoparticles and iron oxide nanoparticles treated with epigallocatechin gallate, gallic acid and tannic acid. DETAILED DESCRIPTION
[0026] Example 1
[0027] A magnetic drug-loaded nanoparticle used in a drug-coated balloon, wherein the preparation method comprises the following steps:
[0028] (1) Dissolving ferrous oxide and epigallocatechin gallate with a particle size of 20 nm in a Tris buffer solution respectively and dispersing them uniformly by ultrasonication to obtain solution 1 and solution 2, mixing solution 1 and solution 2, and then subjecting them to intermittent ultrasonic treatment to obtain a mixture solution 1, specifically: ultrasonic treatment for 60 min each, standing for 20 min, and repeating 4 times; the mass ratio of ferrous oxide to epigallocatechin gallate in the mixture solution 1 is 1:4;
[0029] (2) Paclitaxel was dissolved in an ethanol solution at a concentration of 1 mg / mL, and then the mixture solution 1 in step (1) was added thereto, and intermittent ultrasonic treatment was performed, specifically: ultrasonic treatment for 60 minutes, standing for 20 minutes, and repeated 4 times to obtain a mixture solution 2, in which the mass ratio of paclitaxel to magnetic nanoparticles was 1:5; the mixture solution 2 was stood for 24 hours, and then the composite particles in the container were adsorbed to the bottom by a magnet, the supernatant was poured off, ultrapure water was added thereto for washing, the operation was repeated 3 times, and dried to obtain.
[0030] Example 2
[0031] A magnetic drug-loaded nanoparticle used in a drug-coated balloon, wherein the preparation method comprises the following steps:
[0032] (1) Dissolving ferrous trisulfide and dopamine with a particle size of 100 nm in a Tris buffer solution and ultrasonically dispersing them uniformly to prepare solution 1 and solution 2, mixing solution 1 and solution 2, and then subjecting them to intermittent ultrasonic treatment to prepare a mixture solution 1, specifically: ultrasonic treatment for 50 min each, standing for 10 min, and repeating 3 times; the mass ratio of ferrous trisulfide to dopamine in the mixture solution 1 is 1:2;
[0033] (2) Rapamycin was dissolved in an ethanol solution at a concentration of 1 mg / mL, and then the mixture solution 1 in step (1) was added thereto for intermittent ultrasonic treatment, specifically: ultrasonic treatment for 50 min each, standing for 10 min, repeated 3 times, to obtain a mixture solution 2, wherein the mass ratio of rapamycin to magnetic nanoparticles in the mixture solution 2 was 1:4; the mixture solution 2 was allowed to stand for 24 h, and then the composite particles in the container were adsorbed to the bottom with a magnet, the supernatant was discarded, ultrapure water was added thereto for washing, the operation was repeated 3 times, and dried to obtain.
[0034] Example 3
[0035] A magnetic drug-loaded nanoparticle used in a drug-coated balloon, wherein the preparation method comprises the following steps:
[0036] (1) dissolving nano-NdFeB and tannic acid with a particle size of 200 nm in a Tris buffer solution respectively and uniformly dispersing them by ultrasonication to obtain solution 1 and solution 2, mixing solution 1 and solution 2, and then subjecting the mixture solution 1 to intermittent ultrasonic treatment, specifically: ultrasonic treatment for 70 min each, standing for 15 min, and repeating 5 times; the mass ratio of nano-NdFeB to tannic acid in the mixture solution 1 is 1:5;
[0037] (2) dissolving doxorubicin in an ethanol solution at a concentration of 1 mg / mL, then adding the mixture solution 1 in step (1) thereto, and performing intermittent ultrasonic treatment, specifically: ultrasonic treatment for 70 min each, standing for 20 min, repeating 5 times, to obtain a mixture solution 2, wherein the mass ratio of doxorubicin to magnetic nanoparticles in the mixture solution 2 is 1:6; the mixture solution 2 is allowed to stand for 24 h, and then the composite particles in the container are adsorbed to the bottom by a magnet, the supernatant is discarded, ultrapure water is added thereto for washing, the operation is repeated 3 times, and dried to obtain.
[0038] Test example
[0039] 1. Taking the magnetic drug-loaded nanoparticles prepared in Example 1 as an example, a Fe3O4-EGCG-PTX solution was prepared and the solution was subjected to UV spectrophotometric analysis. The specific results are shown in Figure 1 (a).
[0040] The characteristic absorption peak of EGCG is 276nm, and the ultraviolet characteristic absorption peak of paclitaxel is 228nm. Figure 1 The UV absorption spectra of Fe3O4-EGCG-PTX and Fe3O4-EGCG are shown in Figure 2. Figure 1 (a) shows that an obvious absorption peak appears at 228nm between wavelengths of 200 and 400nm, while no absorption peak is detected at the characteristic absorption peak of EGCG at 276nm. This result indicates that the grafting of paclitaxel is successful. In order to eliminate the influence of paclitaxel, the Fe3O4-EGCG complex was prepared by the method in Example 1 alone, and a Fe3O4-EGCG solution was prepared for ultraviolet spectrophotometric analysis. The specific results are shown in Figure 1 In (b), there is still no obvious absorption peak at 276 nm. The possible reason is that the grafted EGCG content is relatively low and the absorption peak at 276 nm is relatively weak, which is covered by the Fe3O4 absorption peak.
[0041] 2. Taking the magnetic drug-loaded nanoparticles prepared in Example 1 as an example, a Fe3O4-EGCG-PTX solution was prepared. At the same time, a Fe3O4-EGCG complex was prepared by the method in Example 1, and a Fe3O4-EGCG solution was prepared. The above two solutions and the Fe3O4 solution were subjected to infrared spectroscopy analysis. The specific analysis results are shown in Figure 2 .
[0042] Figure 2 The infrared spectra of Fe3O4-EGCG-PTX, Fe3O4-EGCG and Fe3O4 are shown in Figure 2. Figure 2 From the analysis of (a), we can see that 592cm -1 and 632cm -1The peak at 1370cm represents the Fe-O bond. By comparing the infrared spectra of Fe3O4 and Fe3O4-EGCG-PTX, it can be seen that -1 The deformation vibration of CH3 is 1246cm -1 The stretching vibration of CN is 710 cm -1 It is the deformation vibration of CH or CC=O out of plane.
[0043] It is difficult to find the characteristic peak of EGCG functional group in the infrared spectrum of Fe3O4-EGCG-PTX composite. Therefore, the infrared spectrum analysis was performed again after EGCG was grafted onto Fe3O4 nanoparticles and compared with Fe3O4 nanoparticles. The difference between the two is mainly at the wave number of 700 cm -1 -1700cm -1 Therefore, the absorption peak here is magnified, see Figure 2 (b) By comparing the infrared spectra of Fe3O4 and Fe3O4-EGCG, it can be seen that 875cm -1 The position may be the =CH deformation vibration of 1,3 disubstituted benzene, 1214cm -1 The -CO stretching vibration of the ester may be at 1147 cm -1 and 1062cm -1 The above results indicate that EGCG and PTX were successfully grafted onto Fe3O4.
[0044] 3. Observe the microscopic morphology of Fe3O4 nanoparticles and Fe3O4-EGCG-PTX nanoparticles. The specific results are shown in Figure 3 , Figure 3 (a) is the microscopic morphology of Fe3O4 nanoparticles. Figure 3 (b) is the microscopic morphology of Fe3O4-EGCG-PTX nanoparticles. It can be seen from the figure that the actual particle size of the Fe3O4 nanoparticles used is between 10-20nm. The Fe3O4 nanoparticles used are round, but their dispersion is poor, and some nanoparticles are agglomerated and overlapped. The dispersion of Fe3O4-EGCG-PTX nanoparticles is improved compared with Fe3O4, without excessive particle overlap. The particles are oval, with a particle size between 10-20nm. A dark film can be observed at the edge, which is the attachment of EGCG and PTX on the surface of Fe3O4 nanoparticles. The result of TEM observation of particle size is much smaller than that of nanoparticle size potentiometer. This is because Fe3O4 nanoparticles are easy to agglomerate in solution, and the measured particle size is water and particle size.
[0045] IV. Pass Figure 1It can be seen that the characteristic absorption peak of EGCG is 276 nm, and the UV absorbance values of EGCG at different concentrations at 276 nm are shown in Table 1;
[0046] Table 1 Absorbance values of EGCG at different concentrations at 276 nm
[0047]
[0048] GraphPad 8.0.2 and OriginPro 8.5 software were used for curve fitting to obtain the EGCG concentration (C, μg / mL) and absorbance (A) curve. The linear regression equation was A = 0.04312C-0.0364, r = 0.96882. Figure 4 .
[0049] The calculation formulas for drug loading and encapsulation efficiency are as follows:
[0050] Drug loading / % = drug content in particles / particle weight × 100%
[0051] = (EGCG dosage - EGCG amount in solution) / particle weight × 100%
[0052] =(w-v×c) / m×100%;
[0053] Encapsulation rate / % = (EGCG dosage - mass of EGCG in solution) / EGCG dosage × 100%
[0054] =(w-v×c) / w×100%;
[0055] Wherein w is the total amount of EGCG dosed when preparing nanoparticles, v is the volume of the solution, c is the concentration of EGCG in the solution, and m is the weight of the particles.
[0056] After the preparation of Fe3O4-EGCG-PTX nanoparticles, the particles were placed in a centrifuge tube and centrifuged at 8000r / min without washing. The magnetic nanoparticles were separated and placed in an oven for drying. The supernatant was diluted to an appropriate concentration and then UV analysis was performed. The absorbance was measured and then brought into the linear regression equation to calculate the concentration. The final measured EGCG loading was 18.89% and the encapsulation efficiency was 6.8%.
[0057] 5. The zeta potential of ferric oxide, ferric oxide treated with epigallocatechin gallate, ferric oxide treated with gallic acid, and ferric oxide treated with tannic acid were measured. The specific measurement results are shown in Figure 5 .
[0058] pass Figure 5It can be seen that the zeta potential of ferric oxide treated with epigallocatechin gallate, gallic acid and tannic acid is lower than that of ferric oxide, which proves that polyphenols such as epigallocatechin gallate, gallic acid and tannic acid are successfully grafted on the surface of ferric oxide. Figure 3 It can be seen that the dispersibility of ferrosoferric oxide is enhanced due to the grafting of the above-mentioned polyphenols.
Claims
1. A method for preparing magnetic drug-loaded nanoparticles for drug-coated balloons, characterized in that: The following steps are involved: (1) Dissolving the magnetic nanoparticles and the antioxidant agent in a solvent respectively to prepare a solution 1 and a solution 2, and mixing the solution 1 and the solution 2 to prepare a mixture solution 1; (2) dissolving the agent, and then adding the mixture solution 1 in step (1) thereto, mixing well to obtain a mixture solution 2, allowing the mixture solution 2 to stand to form a precipitate, filtering and washing the precipitate, and drying to obtain; Wherein, the antioxidant agent in step (1) is one of epigallocatechin gallate, tannic acid, gallic acid, apple polyphenols, pomegranate polyphenols, tea polyphenols, chlorogenic acid or cocoa polyphenols; The mixing method in step (1) or step (2) is intermittent ultrasonication, specifically: ultrasonic treatment for 50-70 minutes, standing for 10-20 minutes, and repeating 3-5 times.
2. The preparation method according to claim 1, characterized in that In step (1), the mass ratio of the magnetic nanoparticles to the antioxidant agent in the mixture solution 1 is 1:1-5.
3. The preparation method according to claim 1 or 2, characterized in that: The magnetic nanoparticles in step (1) are ferroferric oxide, ferrous sulfide or nano-NdFeB nanoparticles, and the particle size of the magnetic nanoparticles is 10-200 nm.
4. The preparation method according to claim 1, characterized in that: The solvent in step (1) is Tris buffer solution.
5. The preparation method according to claim 1, characterized in that: The drug in step (2) is paclitaxel, rapamycin, doxorubicin, aspirin or a statin.
6. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the medicinal agent to the magnetic nanoparticles in the second mixed solution is 1:4-6.
7. A magnetic drug-loaded nanoparticle for use in a drug-coated balloon, characterized in that: The method is prepared by any one of claims 1 to 6.