A lithium iron phosphate positive electrode material and its preparation method and application

By regulating the amount of titanium doping and carbon coating, the preparation process of lithium iron phosphate cathode materials is optimized, which solves the problems of poor conductivity and cycle stability, achieves high capacity and good cycle performance, simplifies the process, and is suitable for industrial production.

CN115974041BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310218802.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-10-22
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Lithium iron phosphate cathode material has poor conductivity, low capacity, and poor cycle stability. The existing process is complex, dangerous, and high-energy-consuming, making it difficult to use in industrial mass production.

Method used

By rationally regulating the relationship between the titanium doping amount, the carbon coating amount and the compaction density of the positive electrode piece, wet grinding and spray drying processes are used to control the parameter I in the range of 0.4 to 1.6 to improve the conductivity and resistance of the material. Pressure capacity, reduce particle agglomeration, ensure capacity and cycle life.

Benefits of technology

It improves the capacity and cycle retention rate of the lithium iron phosphate cathode material, simplifies the preparation process, reduces the production cycle, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974041B_ABST
    Figure CN115974041B_ABST
Patent Text Reader

Abstract

The present invention provides a lithium iron phosphate positive electrode material and a preparation method and application thereof, and relates to the technical field of lithium ion batteries. Specifically, the method comprises the following steps: fully mixing iron phosphate, a lithium source and a carbon source, and then sequentially performing wet grinding and spray drying; fully mixing the dried material with a titanium source and then calcining, and obtaining a lithium iron phosphate positive electrode material after calcination; by testing the compaction density of the pole piece made of the lithium iron phosphate positive electrode material and the mass ratio of the raw materials, substituting into a specific relationship to calculate the parameter I, and limiting 0.4<I<1.6. The present invention aims at the defects of the lithium iron phosphate material in the prior art, such as poor conductivity, low capacity, and poor cycle stability, and improves the conductivity of the material by reasonably regulating the relationship between the titanium doping amount, the carbon coating amount, and the compaction of the pole piece, reduces the agglomeration between particles, increases the compressive strength of the material, and ensures that the capacity of the lithium iron phosphate material is normally exerted without affecting its cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium iron phosphate (LiFePO4) has been a hot topic in the research and development of positive electrode materials for lithium-ion batteries since its reversible lithium insertion and removal properties were first discovered in 1997, due to its advantages such as good safety performance, long cycle life, wide sources of raw materials, and no environmental pollution. It is recognized as one of the most promising positive electrode materials for lithium-ion power batteries. At present, lithium iron phosphate has entered the practical stage, but lithium iron phosphate still has some application problems, the most important of which is the poor charge and discharge rate performance; and the main reasons for its poor charge and discharge rate performance are low lithium ion conduction rate and low electronic conductivity of materials. In order to improve the electronic or ionic conductivity of lithium iron phosphate, the commonly used technical routes are carbon coating and bulk doping. In the actual synthesis of lithium iron phosphate materials, several methods are often used at the same time, and several mechanisms coexist. Therefore, the method of using ion doping and carbon coating composite modification at the same time is an effective way to improve the electrochemical properties of lithium iron phosphate.

[0003] CN201710971049.5 discloses a method for preparing a titanium-doped lithium iron phosphate positive electrode material: a lithium source compound, a phosphorus source compound, an iron source compound and metal titanium are used as raw materials, mixed evenly, and then melted at high temperature in a furnace, quenched into particles by water, and then ground and dispersed together with a carbon source compound to make the particle size reach a fineness index of D90≤0.2μm, and then powdered by spray drying, and calcined in an atmosphere furnace at 600-800°C for 40-300 minutes, and then cooled to obtain a lithium iron phosphate positive electrode material; by adopting a high-temperature melting method, the uniformity of the lithium iron phosphate positive electrode material is improved; metal titanium powder is introduced, and the Fe in the melt is melted at high temperature. 3+ Reduction to Fe 2+ , and make the generated Ti 4+ Doping into the lithium iron phosphate structure improves the electronic conductivity of the lithium iron phosphate cathode material by forming vacancies; reducing the specific surface area by grinding, dispersion and carbon coating to increase the tap density of the lithium iron phosphate cathode material. However, this invention has the defects of complex process flow, danger and high energy consumption, and is difficult to be used for industrial mass production.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a method for preparing a lithium iron phosphate positive electrode material. In view of the defects of the lithium iron phosphate material provided in the prior art, such as poor conductivity, low capacity, and poor cycle stability, the present invention improves the conductivity of the material, reduces the agglomeration between particles, and increases the compressive resistance of the material by reasonably regulating the relationship between the titanium doping amount, the carbon coating amount, and the compaction of the positive electrode sheet prepared from the lithium iron phosphate positive electrode material, while ensuring that the capacity of the lithium iron phosphate material is normally exerted without affecting its cycle life.

[0006] The second object of the present invention is to provide a lithium iron phosphate positive electrode material prepared by the preparation method of the lithium iron phosphate positive electrode material.

[0007] The third object of the present invention is to provide a use of the lithium iron phosphate positive electrode material in the field of lithium ion batteries.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical scheme is specially adopted: a preparation method of a lithium iron phosphate positive electrode material comprises the following steps: fully mixing iron phosphate, a lithium source and a carbon source, and then sequentially performing wet grinding and spray drying; fully mixing the dried material with a titanium source and then calcining, and obtaining a lithium iron phosphate positive electrode material after calcination; wherein the compaction density of the positive electrode sheet prepared by the lithium iron phosphate positive electrode material is 1 P , with the mass ratio of the carbon source to the iron phosphate being 1 C , with the mass ratio of the titanium source to the iron phosphate being I T , the parameter I is calculated by the following formula: I = I C *(100I P ) 2 / (8.28I P / I T ), the parameter I is: 0.4<I<1.6.

[0009] Preferably, the lithium source comprises at least one of lithium hydroxide, lithium carbonate or lithium nitrate;

[0010] Preferably, the carbon source comprises at least one of lactic acid, glucose, polyethylene glycol or citric acid;

[0011] Preferably, the titanium source comprises titanium dioxide.

[0012] Preferably, the molar ratio of lithium in the lithium source to iron in the iron phosphate is 0.95 to 1.05;

[0013] Preferably, the mass ratio of the carbon source to the iron phosphate is 0.04 to 0.1;

[0014] Preferably, the mass ratio of the titanium source to the iron phosphate is 0.003 to 0.006;

[0015] Preferably, the iron-to-phosphorus ratio of the ferric phosphate is 0.99 to 1.01.

[0016] Preferably, the compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material is P 2.2g / cm 3 ~2.4g / cm 3 .

[0017] Preferably, the wet grinding is performed until the particle size of the material is 300nm to 500nm;

[0018] Preferably, after the wet grinding and before the spray drying, the method includes: adjusting the solid content of the material to 30% to 50%.

[0019] Preferably, the spray pressure of the spray drying is 0.2 MPa to 0.3 MPa, and the temperature of the spray drying is 100° C. to 150° C.

[0020] Preferably, the calcination comprises: firstly heating the temperature to 700°C to 750°C at a rate of 2°C / min to 5°C / min, and then keeping the temperature for 6h to 10h.

[0021] The lithium iron phosphate positive electrode material prepared by the preparation method of the lithium iron phosphate positive electrode material; and the use of the lithium iron phosphate positive electrode material in the field of lithium ion batteries, including but not limited to lithium battery positive electrodes, lithium ion batteries or electrical equipment prepared based on the lithium iron phosphate positive electrode material.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: by controlling the mass ratio of each raw material and the compaction density of the prepared positive electrode sheet, and calculating the parameter I within a limited range, the prepared lithium iron phosphate positive electrode material has the advantages of high capacity and good cycle retention rate; at the same time, the preparation process is simple, the cycle is short, and it is easy to synthesize, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is the first charge and discharge curve of the lithium iron phosphate positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0025] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0026] The present invention is carried out through the following specific implementation methods: A method for preparing a lithium iron phosphate positive electrode material comprises the following steps: fully mixing iron phosphate, a lithium source and a carbon source, and then sequentially performing wet grinding and spray drying; fully mixing the dried material with a titanium source and then calcining, and obtaining a lithium iron phosphate positive electrode material after calcination; wherein the compaction density of the positive electrode sheet prepared with the lithium iron phosphate positive electrode material is 1 P , with the mass ratio of the carbon source to the iron phosphate being 1 C , with the mass ratio of the titanium source to the iron phosphate being I T , the parameter I is calculated by the following formula: I = I C *(100I P ) 2 / (8.28I P / I T ), the parameter I is: 0.4<I<1.6.

[0027] Carbon has excellent electrical conductivity. The present invention coats conductive carbon during the synthesis of lithium iron phosphate to simply and effectively improve the electrical conductivity of lithium iron phosphate. Adding a small amount of carbon can, on the one hand, enhance the electronic conductivity between particles through direct contact between carbon and lithium iron phosphate, and on the other hand, can inhibit the growth of lithium iron phosphate particles to a certain extent, reduce the particle size, shorten the diffusion path of lithium ions during charging and discharging, and indirectly improve the rate characteristics of lithium iron phosphate. However, as the carbon coating increases, the specific surface area of ​​the material increases, and the particles agglomerate seriously, resulting in a decrease in the compaction density of the positive electrode sheet and more fragile particles, an increase in battery side reactions, and serious capacity decay. The doping of titanium ions can effectively inhibit the agglomeration of lithium iron phosphate particles, and the higher the doping amount, the fewer agglomerated particles in the positive electrode material; however, relatively speaking, a small amount of titanium doping will not change the crystal structure of lithium iron phosphate. When the doping amount is too large, part of the titanium occupies the position of iron, producing a mixed phase Li4P2O7, which causes the positive electrode material cycle retention rate to decay significantly.

[0028] The present invention has concluded through a large amount of experimental data that there is a quantitative relationship between the compaction density of the positive electrode sheet made of lithium iron phosphate positive electrode material and the mass of each raw material component. By setting, calculating and controlling the parameter I, when the parameter I is limited to 0.4-1.6, the prepared lithium iron phosphate positive electrode material meets the advantages of strong conductivity, high capacity, good stability, etc. In actual production, the parameter I can be increased or decreased by adjusting the titanium doping amount, carbon coating amount, positive electrode sheet compaction density and other parameter values. As a preferred embodiment, the value of the parameter I includes but is not limited to 0.41, 0.45, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.55, 1.59, etc.

[0029] As a preferred embodiment, the preparation method includes the following steps: fully mixing iron phosphate, a lithium source and a carbon source, and then sequentially performing wet grinding, adjusting the solid content of the slurry, spray drying, and air flow milling; uniformly mixing the crushed material and the titanium source by high-speed ultracentrifugation, and then calcining in a nitrogen protective atmosphere; finally, cooling and sieving the calcined material to obtain a lithium iron phosphate positive electrode material.

[0030] As a preferred embodiment, the compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material is P The measuring method comprises: mixing the lithium iron phosphate positive electrode material with a conductive agent and a binder to prepare a positive electrode slurry, applying the positive electrode slurry to a current collector, and obtaining a positive electrode sheet after drying, rolling and die-cutting; measuring the surface density and thickness of the positive electrode sheet, and calculating the compaction density;

[0031] As a more preferred embodiment, among the components of the positive electrode slurry, the conductive glue includes but is not limited to carbon black, carbon nanotubes, graphite, etc.; the adhesive includes but is not limited to PVDF, PTFE, etc.; the current collector includes but is not limited to aluminum foil, copper foil, etc.; the surface density can be measured by conventional methods in the art, and the compacted density is obtained by dividing the surface density by the thickness.

[0032] As a preferred embodiment, the molar ratio of lithium in the lithium source to iron in the iron phosphate includes but is not limited to 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.01, 1.02, 1.03, 1.04, and 1.05.

[0033] As a preferred embodiment, the mass ratio of the carbon source to the ferric phosphate includes but is not limited to 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, and 0.1.

[0034] As a preferred embodiment, the mass ratio of the titanium source to the iron phosphate includes but is not limited to 0.003, 0.004, 0.005, and 0.006.

[0035] As a preferred embodiment, the wet grinding is performed to a particle size of the material including but not limited to 300, 320, 340, 360, 380, 400, 420, 440, 460, 480, 500 (nm).

[0036] As a preferred embodiment, after the wet grinding and before the spray drying, the process includes adjusting the solid content of the material to include but is not limited to 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, and 50%.

[0037] As a preferred embodiment, the spray pressure of the spray drying includes but is not limited to 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3 (MPa), and the temperature of the spray drying includes but is not limited to 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150 (℃).

[0038] As a preferred embodiment, the calcination includes: first heating to 700, 705, 710, 715, 720, 725, 730, 735, 740, 745, 750 (°C) at a rate of 2.5°C / min, and then keeping warm for 6, 7, 8, 9, 10 (h).

[0039] Example 1

[0040] Lithium hydroxide and iron phosphate are added to the grinding machine silo at a molar ratio of 1:1; then lactic acid and iron phosphate are also added to the grinding machine at a mass ratio of 9%:1 for wet grinding. The ground slurry is spray dried at 120°C and a pressure of 0.4MPa, and the dried material is jet milled. The crushed material is then mixed with TiO2 (TiO2 and iron phosphate are added at a mass ratio of 0.4%:1) and mixed evenly by ultracentrifugation at a high speed of 16000rpm / min. Finally, the mixed material is placed in a nitrogen atmosphere and heated to 725°C at a rate of 2.5°C / min, calcined for 8h, cooled, and sieved to obtain the final positive electrode material. The prepared positive electrode material is compacted at 2.3g / cm 3 Made into pole pieces.

[0041] Example 2

[0042] It is basically the same as Example 1, except that the mass ratio of lactic acid to iron phosphate is 10%:1; the mass ratio of TiO2 to iron phosphate is 0.5%:1.

[0043] Example 3

[0044] The method is basically the same as Example 1, except that the mass ratio of lactic acid to iron phosphate is 4%:1.

[0045] Example 4

[0046] The method is basically the same as Example 1, except that the calcination condition is to increase the temperature to 750° C. at a rate of 2.5° C. / min in a nitrogen atmosphere and calcine for 6 hours.

[0047] Example 5

[0048] The method is basically the same as Example 1, except that the calcination condition is to increase the temperature to 700° C. at a rate of 2.5° C. / min in a nitrogen atmosphere and calcine for 10 h.

[0049] Example 6

[0050] The method is basically the same as Example 1, except that the spray drying conditions are 150° C. and 0.2 MPa.

[0051] Example 7

[0052] The same as Example 1, except that the prepared positive electrode material was compacted at 2.2 g / cm 3 Made into pole pieces.

[0053] Example 8

[0054] The same as Example 1, except that the prepared positive electrode material was compacted at 2.4 g / cm 3 Made into pole pieces.

[0055] Comparative Example 1

[0056] It is basically the same as Example 1, except that the mass ratio of lactic acid to iron phosphate is 12%:1; the mass ratio of TiO2 to iron phosphate is 0.8%:1.

[0057] Comparative Example 2

[0058] The method is basically the same as Example 1, except that the mass ratio of lactic acid to ferric phosphate is 15%:1.

[0059] Comparative Example 3

[0060] It is basically the same as Example 1, except that the mass ratio of TiO2 and iron phosphate is 1%:1.

[0061] Comparative Example 4

[0062] The same as Example 1, except that the prepared positive electrode material was compacted at 1.8 g / cm 3 Made into pole pieces.

[0063] Comparative Example 5

[0064] The same as Example 1, except that the prepared positive electrode material was compacted at 3.0 g / cm 3 Made into pole pieces.

[0065] Table 1

[0066]

[0067]

[0068] Test example

[0069] The positive electrode materials prepared in the above-mentioned embodiments and comparative examples were respectively used to prepare button batteries. The positive electrode material, carbon black conductive agent, binder PVDF and NMP with a mass ratio of 95:2.5:2.5:5 were mixed evenly to prepare the positive electrode slurry of the battery; the slurry was coated on an aluminum foil with a thickness of 20 to 40 μm, and the positive electrode sheet was obtained after vacuum drying and rolling; the lithium metal sheet was used as the negative electrode, and the electrolyte ratio was 1.15 mol / L LiPF6EC:DMC (1:1 vol%).

[0070] Figure 1 The constant current charge and discharge curve of the button cell prepared in Example 1 is shown in FIG. 1 , and the charge and discharge test is performed at 0.1C.

[0071] The electrical performance test was conducted using a blue battery test system at 25°C with a test voltage range of 2.0V to 3.75V; the capacity and 50-week capacity retention rate were tested. The test results are shown in Table 1.

[0072] Table 2

[0073]

[0074] Among them, in each embodiment of the present invention: 0.4<I<1.6; at the same time when I P ,I C ,I T When it conforms to the preferred value range of the present invention, the I value also has the following trend characteristics: when 0.4<I<1, as the I value decreases, the capacity of the positive electrode material shows a downward trend; when I=1, the capacity and cycle performance of the positive electrode material are optimal; when 1<I<1.6, as the I value increases, the cycle retention rate of the positive electrode material decreases significantly.

[0075] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The method comprises the following steps: fully mixing iron phosphate, a lithium source and a carbon source, and then sequentially performing wet grinding and spray drying; fully mixing the dried material with a titanium source and then calcining the mixture to obtain a lithium iron phosphate positive electrode material; the titanium source is titanium dioxide; The compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material is 1 P , with the mass ratio of the carbon source to the iron phosphate being 1 C , with the mass ratio of the titanium source to the iron phosphate being I T ; said I P In g / cm 3 count; The parameter I is calculated by the following formula: I = I C *(100I P ) 2 ∕ (8.28I P ∕ I T ), the value of the parameter I is: 0.4<I<1.4; The compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material is P 2.2g / cm 3 ~2.4g / cm 3 .

2. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The lithium source includes at least one of lithium hydroxide, lithium carbonate or lithium nitrate; And / or, the carbon source comprises at least one of lactic acid, glucose, polyethylene glycol or citric acid.

3. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The molar ratio of lithium in the lithium source to iron in the iron phosphate is 0.95-1.05; And / or, the mass ratio of the carbon source to the iron phosphate is C 0.04~0.1; And / or, the mass ratio of the titanium source to the iron phosphate is T It is 0.003~0.

006.

4. The method for preparing a lithium iron phosphate positive electrode material according to claim 1, characterized in that: The compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material is P The measurement method includes: mixing the lithium iron phosphate positive electrode material with a conductive agent and a binder to prepare a positive electrode slurry, applying the positive electrode slurry to a current collector, and obtaining a positive electrode sheet after drying, rolling, and die-cutting; measuring the surface density and thickness of the positive electrode sheet, and calculating the compaction density.

5. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The wet grinding is performed until the particle size of the material is 300nm~500nm.

6. The method for preparing a lithium iron phosphate positive electrode material according to claim 1, characterized in that: After the wet grinding and before the spray drying, the method includes adjusting the solid content of the material to 30% to 50%.

7. The method for preparing a lithium iron phosphate positive electrode material according to claim 1, characterized in that: The spray drying spray pressure is 0.2MPa-0.3MPa, and the spray drying temperature is 100°C-150°C.

8. The method for preparing a lithium iron phosphate positive electrode material according to claim 1, characterized in that: The calcination comprises: firstly heating the temperature to 700°C-750°C at a speed of 2°C / min-5°C / min, and then keeping the temperature for 6h-10h.

9. The lithium iron phosphate positive electrode material obtained by the method for preparing the lithium iron phosphate positive electrode material according to any one of claims 1 to 8.

10. Use of the lithium iron phosphate positive electrode material according to claim 9 in the field of lithium ion batteries.