Co-precipitation-based high-rate-performance lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof

Lithium manganese iron phosphate positive electrode material was prepared by co-precipitation method and spray drying method, forming a uniform nanorod-shaped structure and carbon coating, solving the problem of poor circulation and rate performance of existing materials, and significantly improving the electrochemical performance of lithium-ion batteries and stability.

CN118919701APending Publication Date: 2024-11-08XI AN JIAOTONG UNIV +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411309690.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The circulation and rate performance of existing lithium manganese iron phosphate cathode materials have poor circulation, resulting in a low capacity of lithium-ion batteries under 3C cycles, limiting their application in large-scale industrial production.

Method used

The co-precipitation method is used to synthesize the lithium manganese iron phosphate positive electrode material, and the precursor of the lithium manganese iron phosphate is synthesized by hydrothermal method, and carbon coating is carried out by spray drying. Then, the high temperature is calcined to form a uniform nanorod-like structure and carbon coating to optimize the material electrochemical properties.

Benefits of technology

Improve the rate performance and cycle stability of the lithium iron manganese phosphate positive electrode material. The capacity of the lithium-ion battery is maintained at 138mAh/g under 3C cycle, and the capacity after 150 cycles at 0.1C is still reached 143mAh/g, which significantly improves the electrical power of the material. Chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919701A_ABST
    Figure CN118919701A_ABST
Patent Text Reader

Abstract

The invention discloses a high-rate-performance lithium manganese iron phosphate positive electrode material based on coprecipitation as well as a preparation method and application thereof, and belongs to the technical field of lithium ion batteries. The preparation method comprises the following steps: mixing a lithium source, phosphoric acid, an iron source and a manganese source, and performing hydrothermal reaction to obtain a lithium manganese iron phosphate precursor; and mixing the lithium manganese iron phosphate precursor with a carbon source and water, carrying out carbon coating by adopting a spray drying method, and then roasting to obtain the lithium manganese iron phosphate positive electrode material. According to the invention, a hydrothermal method is adopted, so that the microstructure of the lithium iron manganese phosphate precursor is in a nanorod shape, and the transmission path of lithium ions is shortened; and a uniform carbon coating is formed on the surface of the precursor through a spray drying method and roasting, so that the conductivity of the material is further enhanced, a channel is provided for lithium ion diffusion, grain growth is inhibited, and the cycle and rate performance of the material is improved. The technical problem that the lithium manganese iron phosphate material is poor in circulation and rate capability is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a high-rate performance lithium manganese iron phosphate positive electrode material based on coprecipitation, and a preparation method and application thereof. Background Art

[0002] Faced with the rapid development of new energy fields, lithium-ion batteries have played an increasingly important role since their successful development. As a key component of lithium-ion batteries, positive electrode materials have always been the key to improving the performance of lithium-ion batteries.

[0003] Olivine-type lithium manganese iron phosphate cathode material has attracted much attention due to its high theoretical capacity, high safety and high voltage platform. At present, the common methods for preparing lithium manganese iron phosphate include high-temperature solid phase method, hydrothermal method, sol-gel method, etc. Among them, the hydrothermal method is widely used due to its advantages such as being able to synthesize excellent nanocrystals and ensuring the consistency of materials. However, the lithium manganese iron phosphate prepared by the prior art has poor cycle and rate performance due to its low electronic conductivity and lithium ion diffusion coefficient. The lithium manganese iron phosphate cathode material LiMn in the prior art 0.6 Fe 0.4 When PO4 / C is used in lithium-ion batteries, the capacity of lithium-ion batteries can only reach about 120mAh / g under a 3C cycle, which seriously affects the application of positive electrode materials and is not suitable for large-scale industrial production. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a high-rate performance lithium iron manganese phosphate positive electrode material based on co-precipitation and its preparation method and application, which solves the technical problems of poor cycle performance and rate performance of lithium iron manganese phosphate materials.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The present invention provides a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation. The general chemical formula of the lithium iron manganese phosphate positive electrode material includes LiMn x Fe 1-x PO4 / C.

[0006] Preferably, the lithium manganese iron phosphate positive electrode material has a uniform nanorod structure.

[0007] Preferably, the grain size of the lithium manganese iron phosphate positive electrode material is 200-500 nm.

[0008] The present invention provides a method for preparing a high-rate performance lithium manganese iron phosphate positive electrode material based on coprecipitation, comprising the following steps: (1) Mixing a lithium source, phosphoric acid, an iron source, a manganese source and water, and performing a hydrothermal reaction to obtain a lithium iron manganese phosphate precursor; the chemical formula of the lithium iron manganese phosphate precursor is LiMn x Fe 1-x PO4, where 0.2≤x≤0.8; (2) mixing the lithium iron manganese phosphate precursor, the carbon source and water, and carbon-coating the obtained mixture by spray drying to obtain a carbon-coated lithium iron manganese phosphate precursor; wherein the amount ratio of the lithium iron manganese phosphate precursor, the carbon source and the water is 100 g: (2-6) g: (200-300) mL; (3) calcining the carbon-coated lithium manganese iron phosphate precursor to obtain a lithium manganese iron phosphate positive electrode material with high rate performance.

[0009] Preferably, in step (1), the mass concentration of the phosphoric acid is 75% to 90%, and the molar ratio of the lithium source, phosphoric acid, manganese source and iron source is 3:1:x:1-x; wherein 0.2≤x≤0.8.

[0010] Preferably, the lithium source includes lithium hydroxide monohydrate or lithium chloride; the iron source includes ferrous sulfate heptahydrate or ferrous chloride; and the manganese source includes manganese sulfate or manganese chloride.

[0011] Preferably, in step (1), the temperature of the hydrothermal reaction is 150-200° C. and the time is 15-24 h.

[0012] Preferably, in step (2), the carbon source comprises one or more of sucrose, glucose, starch and xylitol; and the mass of the carbon source is 2% to 6% of the total mass of the lithium manganese iron phosphate precursor and the carbon source.

[0013] Preferably, in step (2), in the spray drying method, the mass of the solid component accounts for 30% to 40% of the total mass of the mixture, the temperature of the spray dryer used is 150 to 180° C., and the spray feed rate is 10 to 20 mL / min.

[0014] Preferably, in step (3), the calcination temperature is 600-800° C. and the calcination time is 3-5 h.

[0015] Preferably, in step (3), the heating rate to the calcination temperature is 4-8°C / min; the calcination is carried out under a protective atmosphere; the protective atmosphere is one or more of argon, nitrogen and helium.

[0016] The present invention provides the application of the high-rate performance lithium iron manganese phosphate positive electrode material described in the above technical solution in a lithium ion battery.

[0017] Compared with the prior art, the present invention has the following beneficial effects: Lithium iron manganese phosphate positive electrode material LiMn disclosed in the present invention x Fe 1-x PO4 / C, where 0.2≤x≤0.8, by adjusting the value of x, the larger the x value, the higher the energy density, and the performance optimization of lithium manganese iron phosphate positive electrode material is achieved. Experiments show that when x is 0.6, the performance, energy density and cycle life of the material are more balanced. It has a uniform nanorod structure, the particles of the structure are uniform, the dispersion is good, and the size of the material is significantly reduced. Experimental verification shows that the grain size of the material is 200-500nm, which makes the transmission path of lithium ions in the material shorter, thereby improving the rate performance of the material. At the same time, this structure maintains the consistency of the material phase, further enhancing its stability in the electrochemical cycle.

[0018] The present invention discloses a preparation method of a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation. First, a lithium iron manganese phosphate precursor is synthesized by a hydrothermal method. The high temperature and high pressure environment makes the lithium iron manganese phosphate microstructure present a uniform nanorod shape, reduces the size, shortens the transmission path of lithium ions, ensures the consistency of the final positive electrode material phase, and improves the rate performance of the positive electrode material. It has been experimentally verified that when the lithium iron manganese phosphate positive electrode material prepared by the preparation method is used for lithium ion batteries, the capacity of the lithium ion battery is still maintained at 138mAh / g under the cycle of 3C, indicating that it has good rate performance. Secondly, the present invention adopts a spray drying method for carbon coating, and the lithium iron manganese phosphate precursor is mixed with a carbon source and then spray granulated, so that the carbon coating is uniform and does not destroy the nanorod structure of the lithium iron manganese phosphate precursor, thereby improving the cycle stability of the material. It has been experimentally verified that when the lithium iron manganese phosphate positive electrode material prepared by the preparation method is used for lithium ion batteries, after 150 cycles at 0.1C, its capacity can still reach 143mAh / g, indicating that it has good cycle performance. Finally, after high-temperature calcination, a uniform carbon coating is formed on the surface of lithium manganese iron phosphate, which further enhances the conductivity of the material, provides a channel for lithium ion diffusion, inhibits grain growth, and improves the material's cycle and rate performance.

[0019] Furthermore, during the carbon coating process, too high or too low a carbon content may lead to a decrease in performance. The present invention uses a carbon source with a mass proportion of 2% to 6% of the total mass of the lithium manganese iron phosphate precursor and the carbon source, which effectively improves the electrochemical performance of the material.

[0020] Furthermore, by controlling the temperature of the spray dryer and the spray feed rate within a certain range, and further optimizing the parameters of the calcination temperature, time and heating rate, the performance of the lithium manganese iron phosphate cathode material is optimized. The optimization of these parameters not only improves the crystallinity and purity of the material, but also further enhances its electrochemical performance.

[0021] Furthermore, the preparation process of the present invention is simple, low-cost, environmentally friendly, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The lithium iron manganese phosphate positive electrode material LiMn after calcination in Example 1 of the present invention 0.6 Fe 0.4 SEM image of PO4 / C; Figure 2 The positive electrode material LiMn prepared in Comparative Example 1 of the present invention 0.6 Fe 0.4 SEM image of PO4 / C; Figure 3 The lithium iron manganese phosphate positive electrode material LiMn prepared in Example 1 of the present invention 0.6 Fe 0.4 Cycling performance diagram of PO4 / C when used in lithium-ion batteries; Figure 4 The lithium iron manganese phosphate positive electrode material LiMn prepared in Comparative Example 1 of the present invention 0.6 Fe 0.4 Cycling performance diagram of PO4 / C when used in lithium-ion batteries; Figure 5 The lithium iron manganese phosphate positive electrode material LiMn prepared by the methods of Example 1 and Comparative Example 1 0.6 Fe 0.4 Rate performance diagram of PO4 / C when used in lithium-ion batteries. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0025] The present invention is further described in detail below in conjunction with the accompanying drawings: The present invention provides a method for preparing a high-rate performance lithium manganese iron phosphate positive electrode material based on coprecipitation, comprising the following steps: Mixing a lithium source, phosphoric acid, an iron source, a manganese source and water to perform a hydrothermal reaction to obtain a lithium manganese iron phosphate precursor; The lithium iron manganese phosphate precursor, a carbon source and water are mixed, and the obtained mixture is carbon-coated by a spray drying method to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor is calcined to obtain a lithium manganese iron phosphate positive electrode material with high rate performance.

[0026] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.

[0027] The invention mixes a lithium source, phosphoric acid, an iron source, a manganese source and water, and performs a hydrothermal reaction to obtain a lithium manganese iron phosphate precursor.

[0028] In the present invention, the lithium source preferably includes lithium hydroxide monohydrate or lithium chloride; the iron source preferably includes ferrous sulfate heptahydrate or ferrous chloride; the manganese source preferably includes manganese sulfate or manganese chloride; and the mass concentration of the phosphoric acid is preferably 85%.

[0029] In the present invention, the molar ratio of the lithium source, phosphoric acid, manganese source and iron source is preferably 3:1:x:1-x, wherein 0.2≤x≤0.8, more preferably x=0.4~0.7, and further preferably x=0.5~0.6.

[0030] In the present invention, the mixing of the lithium source, phosphoric acid, iron source, manganese source and water is preferably to dissolve the lithium source in water, then add phosphoric acid dropwise, and then add the iron source and manganese source in sequence, stir to form a mixture, and place the resulting mixture in a hydrothermal kettle for hydrothermal reaction; wherein, by adding phosphoric acid dropwise, phosphate ions can be slowly introduced, thereby controlling the reaction rate and avoiding excessive local concentration or rapid temperature increase due to rapid mixing; by adding the iron source and manganese source in sequence, it can be ensured that these raw materials are evenly distributed in the solution, which helps to form a uniform precursor precipitation; by controlling the order of adding the raw materials (such as dissolving the lithium source first, then adding phosphoric acid, iron source and manganese source) and the mixing method, the performance of the lithium iron manganese phosphate precursor can be optimized, which helps to improve its purity, uniformity and crystallinity, thereby improving the cycle and high rate performance of the lithium iron manganese phosphate material.

[0031] In the present invention, the reaction temperature of the hydrothermal reaction is preferably 150-200°C, more preferably 160-190°C, more preferably 170-180°C, and the reaction time is preferably 15-24h, more preferably 15-20h, more preferably 17-20h; wherein, conducting the hydrothermal reaction within this temperature range can ensure that the reaction achieves a higher efficiency, so that the ions in the raw materials can fully react to form the expected lithium manganese iron phosphate precursor; at the same time, appropriate reaction temperature and time also help to reduce the occurrence of side reactions and improve the purity of the product.

[0032] Within this temperature and time range, the lithium iron manganese phosphate precursor can also form a product with good crystal structure and performance. A higher reaction temperature can promote the growth of crystals and the improvement of the structure, while an appropriate reaction time helps to control the growth rate of the crystals and avoid performance degradation caused by excessive growth. After completing the hydrothermal reaction, the present invention preferably filters and dries the resulting product in sequence to obtain a lithium iron manganese phosphate precursor; the present invention has no special limitations on filtering and drying, and can be carried out according to processes well known in the art; in an embodiment of the present invention, the drying temperature is specifically 60°C.

[0033] In the present invention, the chemical formula of the lithium manganese iron phosphate precursor is LiMn x Fe 1-x PO4, wherein 0.2≤x≤0.8, more preferably x=0.4~0.7, further preferably x=0.5~0.6.

[0034] After obtaining the lithium iron manganese phosphate precursor, the present invention mixes the lithium iron manganese phosphate precursor with the carbon source and water, and carbon-coates the obtained mixture by spray drying to obtain the carbon-coated lithium iron manganese phosphate precursor.

[0035] In the present invention, the carbon source preferably includes one or more of sucrose, glucose, starch and xylitol; when the carbon source is two or more of the above, the present invention has no special limitation on the ratio of different types of carbon sources, which can be adjusted according to actual needs; the mass of the carbon source is preferably 2% to 6% of the total mass of the lithium manganese iron phosphate precursor and the carbon source, further preferably 3% to 5%, and more preferably 3.5% to 4.5%.

[0036] In the spray drying method of step (2) of the present invention, the mass of the solid component accounts for 30% to 40% of the total mass of the entire mixture, more preferably 30% to 35%, and more preferably 32% to 33%. The mass of the water in the present invention is preferably such that the mixture reaches the above solid content. In the present invention, in the spray drying method, the temperature of the spray dryer used is preferably 150 to 180°C, more preferably 160 to 170°C, and the spray feed rate of the spray drying is preferably 10 to 20 mL / min, more preferably 10 to 15 mL / min.

[0037] After obtaining the carbon-coated lithium iron manganese phosphate precursor, the present invention bakes the carbon-coated lithium iron manganese phosphate precursor to obtain a lithium iron manganese phosphate positive electrode material with high rate performance.

[0038] In the present invention, the calcination temperature is preferably 600-800°C, more preferably 650-750°C, and further preferably 650-700°C; the time is preferably 3-5h, and more preferably 3-4h; the heating rate of the temperature rise to the calcination temperature is preferably 4-8°C / min, more preferably 5-7°C / min, and further preferably 5.5-6.5°C / min; the calcination is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably one or more of argon, nitrogen and helium.

[0039] The present invention provides a high-rate performance lithium iron manganese phosphate positive electrode material prepared by the preparation method described in the above technical solution, wherein the chemical formula of the lithium iron manganese phosphate positive electrode material is LiMn x Fe 1-x PO4 / C, wherein 0.2≤x≤0.8, more preferably 0.4≤x≤0.7, and even more preferably 0.5≤x≤0.6.

[0040] The present invention provides the application of the high-rate performance lithium iron manganese phosphate positive electrode material described in the above technical solution in a lithium ion battery. The present invention has no special limitation on the application method, and the application can be carried out according to methods well known in the art.

[0041] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0042] Example 1 0.219 mol of lithium hydroxide monohydrate was dissolved in 50 mL of deionized water, and 0.073 mol of phosphoric acid (mass concentration of phosphoric acid was 85%) was added dropwise to the above solution, and stirred to form a white suspension; 0.0288 mol of ferrous sulfate heptahydrate and 0.0432 mol of manganese sulfate were added in sequence, and stirred to form a light green suspension. The obtained suspension was placed in a 100 mL hydrothermal kettle, and placed in an oven at 180°C for reaction for 20 hours to obtain a precipitate. After filtering the precipitate, it was dried in a blast drying oven at 60°C to obtain lithium iron manganese phosphate precursor LiMn 0.6 Fe 0.4 PO4; The lithium iron manganese phosphate precursor and glucose (glucose accounts for 5% of the total mass of the lithium iron manganese phosphate precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 150° C. and the spray drying feed rate is 10 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium iron manganese phosphate precursor was placed in an argon-protected tubular furnace and heated to 700°C at a heating rate of 5°C / min for 3 h to obtain a lithium iron manganese phosphate cathode material, denoted as LiMn 0.6 Fe 0.4 PO4 / C.

[0043] Example 2 0.219 mol of lithium hydroxide monohydrate was dissolved in 50 mL of deionized water, and 0.073 mol of phosphoric acid (mass concentration of phosphoric acid is 75%) was added dropwise to the above solution, and stirred to form a white suspension; 0.036 mol of ferrous sulfate heptahydrate and 0.036 mol of manganese sulfate were added in sequence, and stirred to form a light green suspension. The obtained suspension was placed in a 100 mL hydrothermal kettle, placed in an oven at 180 ° C for 24 hours to obtain a precipitate, and the precipitate was filtered and dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.5 Fe 0.5 PO4; The lithium iron manganese phosphate precursor and glucose (glucose accounts for 4% of the total mass of the lithium iron manganese phosphate precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 160° C. and the spray drying feed rate is 15 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium iron manganese phosphate precursor was placed in an argon-protected tube furnace and heated to 700°C at a heating rate of 4°C / min for 3 h to obtain the lithium iron manganese phosphate positive electrode material LiMn 0.5Fe 0.5 PO4 / C.

[0044] Example 3 0.219 mol of lithium hydroxide monohydrate was dissolved in 50 mL of deionized water, and 0.073 mol of phosphoric acid (mass concentration of phosphoric acid is 80%) was added dropwise to the above solution, and stirred evenly to form a white suspension; 0.0216 mol of ferrous sulfate heptahydrate and 0.0504 mol of manganese sulfate were added in sequence, and stirred thoroughly to form a light green suspension. The obtained suspension was placed in a 100 mL hydrothermal kettle, placed in a 200 ° C oven for reaction for 20 hours to obtain a precipitate, which was filtered and dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.7 Fe 0.3 PO4; The lithium iron manganese phosphate precursor and sucrose (sucrose accounts for 6% of the total mass of the lithium iron manganese phosphate precursor and sucrose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 150° C. and the spray drying feed rate is 10 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 750°C at a heating rate of 8°C / min for 3 hours to obtain the lithium manganese iron phosphate positive electrode material LiMn 0.7 Fe 0.3 PO4 / C.

[0045] Example 4 0.438 mol of lithium hydroxide monohydrate was dissolved in 110 mL of deionized water, and 0.146 mol of phosphoric acid (mass concentration of phosphoric acid is 88%) was added dropwise to the above solution, and stirred evenly to form a white suspension; 0.0576 mol of ferrous sulfate heptahydrate and 0.0864 mol of manganese sulfate were added in sequence, and stirred thoroughly to form a light green suspension. The obtained suspension was placed in a 250 mL hydrothermal kettle, placed in an oven at 180 ° C for 24 hours to obtain a precipitate, and the precipitate was filtered and dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.6 Fe 0.4 PO4; The lithium iron manganese phosphate precursor and sucrose (sucrose accounts for 4% of the total mass of the lithium iron manganese phosphate precursor and sucrose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 180° C. and the spray drying feed rate is 15 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 650°C at a heating rate of 5°C / min for 5 h to obtain the lithium manganese iron phosphate positive electrode material LiMn 0.6 Fe 0.4 PO4 / C.

[0046] Example 5 0.438 mol of lithium hydroxide monohydrate was dissolved in 110 mL of deionized water, and 0.146 mol of phosphoric acid (mass concentration of phosphoric acid is 82%) was added dropwise to the above solution, and stirred evenly to form a white suspension; 0.0576 mol of ferrous sulfate heptahydrate and 0.0864 mol of manganese sulfate were added in sequence, and stirred thoroughly to form a light green suspension. The obtained suspension was placed in a 250 mL hydrothermal kettle, placed in a 150 ° C oven for reaction for 24 hours to obtain a precipitate, and the precipitate was filtered and dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.6 Fe 0.4 PO4; The lithium iron manganese phosphate precursor and starch (starch accounts for 4% of the total mass of the lithium iron manganese phosphate precursor and starch) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 180° C. and the spray drying feed rate is 20 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 800°C at a heating rate of 5°C / min for 5 h to obtain the lithium manganese iron phosphate positive electrode material LiMn 0.6 Fe 0.4 PO4 / C.

[0047] Example 6 0.219 mol of lithium hydroxide monohydrate was dissolved in 50 mL of deionized water, and 0.073 mol of phosphoric acid (mass concentration of phosphoric acid was 85%) was added dropwise to the above solution, and stirred to form a white suspension; 0.0288 mol of ferrous sulfate heptahydrate and 0.0432 mol of manganese sulfate were added in sequence, and stirred to form a light green suspension. The obtained suspension was placed in a 100 mL hydrothermal kettle, placed in an oven at 180 ° C for 15 hours to obtain a precipitate, which was filtered and dried in a blast drying oven at 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.6 Fe 0.4 PO4; The lithium iron manganese phosphate precursor and glucose (glucose lithium iron manganese phosphate accounts for 5% of the total mass of the precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 150°C, and the spray drying feed rate is 10mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 600°C at a heating rate of 5°C / min and calcined for 5 h to obtain a lithium manganese iron phosphate cathode material, denoted as LiMn 0.6 Fe 0.4 PO4 / C.

[0048] Example 7 0.438 mol of lithium hydroxide monohydrate was dissolved in 110 mL of deionized water, and 0.146 mol of phosphoric acid (mass concentration of phosphoric acid is 85%) was added dropwise to the above solution, and stirred evenly to form a white suspension; 0.028008 mol of ferrous sulfate heptahydrate and 0.1152 mol of manganese sulfate were added in sequence, and stirred thoroughly to form a light green suspension. The obtained suspension was placed in a 250 mL hydrothermal kettle, placed in a 150 ° C oven for reaction for 24 hours to obtain a precipitate, and the precipitate was filtered and dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.8 Fe 0.2 PO4; The lithium iron manganese phosphate precursor and glucose (glucose accounts for 4% of the total mass of the lithium iron manganese phosphate precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 150° C. and the spray drying feed rate is 10 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 650°C at a heating rate of 5°C / min for 5 h to obtain the lithium manganese iron phosphate positive electrode material LiMn 0.8 Fe 0.2 PO4 / C.

[0049] Example 8 0.438 mol of lithium hydroxide monohydrate was dissolved in 110 mL of deionized water, and 0.146 mol of phosphoric acid (mass concentration of phosphoric acid is 90%) was added dropwise to the above solution, and stirred evenly to form a white suspension; 0.1152 mol of ferrous sulfate heptahydrate and 0.0288 mol of manganese sulfate were added in sequence, and stirred thoroughly to form a light green suspension. The obtained suspension was placed in a 250 mL hydrothermal kettle, placed in an oven at 180 ° C for 20 hours to obtain a precipitate, which was filtered and dried in a blast drying oven at 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.2 Fe 0.8 PO4; The lithium iron manganese phosphate precursor and glucose (glucose accounts for 4% of the total mass of the lithium iron manganese phosphate precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 40% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 160° C. and the spray drying feed rate is 12 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium iron manganese phosphate precursor was placed in an argon-protected tube furnace and heated to 750°C at a heating rate of 5°C / min for 4 hours to obtain the lithium iron manganese phosphate positive electrode material LiMn 0.2 Fe 0.8 PO4 / C.

[0050] Example 9 0.219 mol lithium chloride was dissolved in 50 mL deionized water, and 0.073 mol phosphoric acid (mass concentration of phosphoric acid is 90%) was added dropwise to the above solution, and stirred to form a white suspension; 0.0288 mol ferrous chloride and 0.0432 mol manganese chloride were added in sequence, and stirred to form a light green suspension. The obtained suspension was placed in a 100 mL hydrothermal kettle, and placed in a 170 ° C oven for reaction for 22 hours to obtain a precipitate. After filtering the precipitate, it was dried in a blast drying oven at a temperature of 60 ° C to obtain lithium iron manganese phosphate precursor LiMn 0.6 Fe 0.4 PO4; The lithium iron manganese phosphate precursor and glucose (glucose accounts for 2% of the total mass of the lithium iron manganese phosphate precursor and glucose) are mixed in deionized water so that the mass of the solid component accounts for 30% of the total mass of the entire mixture, and carbon-coated by spray drying. The working temperature of the spray dryer is 170° C. and the spray drying feed rate is 13 mL / min to obtain a carbon-coated lithium iron manganese phosphate precursor; The carbon-coated lithium manganese iron phosphate precursor was placed in an argon-protected tube furnace and heated to 700°C at a heating rate of 5°C / min for 4 hours to obtain the lithium manganese iron phosphate positive electrode material LiMn 0.6 Fe 0.4 PO4 / C.

[0051] Comparative Example 1 Preparation of LiMn iron manganese phosphate cathode material by high temperature solid phase method 0.6 Fe 0.4 PO4 / C: 0.012 mol of ferrous oxalate dihydrate, 0.018 mol of manganese carbonate, 0.03 mol of lithium carbonate and 0.03 mol of ammonium dihydrogen phosphate were mixed, sucrose was added in an amount of 3% of the sum of the mass of the carbon source, phosphorus source, iron source and manganese source, 15 g of ethanol was added as a solvent, and the mixture was ball-milled in a planetary ball mill at a ball-to-material ratio of 10:1 and a speed of 600 r / min for 10 h to form a uniform first slurry; The obtained first slurry was placed in a blast oven and dried at 60°C, and then placed in an argon-protected tubular furnace for sintering. The sintering temperature was set to 350°C, the heating rate was 5°C / min, and the holding time was 6h to obtain a mixed powder; The mixed powder was mixed with sucrose, the amount of sucrose added was 3% of the sum of the mass of sucrose and the mixed powder, 10 g of ethanol was added as a solvent, and the mixture was ball-milled in a planetary ball mill at a ball-to-material ratio of 10:1 and a speed of 600 r / min for 2 h to form a uniform second slurry; The second slurry was dried in a blast oven at 60°C, and then placed in an argon protected tubular furnace for sintering. The sintering temperature was set to 700°C, the heating rate was 5°C / min, and the holding time was 20h to obtain lithium manganese iron phosphate positive electrode material LiMn 0.6 Fe 0.4 PO4 / C.

[0052] Performance and testing 1) Figure 1 The lithium iron manganese phosphate positive electrode material LiMn after calcination in Example 1 0.6 Fe 0.4 SEM image of PO4 / C; Figure 2 The positive electrode material LiMn prepared in Comparative Example 1 0.6 Fe 0.4 SEM image of PO4 / C; Figure 1 and Figure 2 It can be seen that the lithium manganese iron phosphate positive electrode material prepared by the hydrothermal method and spray drying carbon coating in Example 1 presents a uniform nanorod structure. Compared with the high-temperature solid phase method in Comparative Example 1, the particles are more uniform and have better dispersion. In Example 1, the particles are nanosized and uniformly carbon coated to shorten the lithium ion transmission path and improve the electrical conductivity, thereby exhibiting good electrochemical properties.

[0053] 2) 0.24 g of lithium manganese iron phosphate positive electrode material LiMn prepared in Example 1 and Comparative Example 1 0.6 Fe 0.4PO4 / C, polyvinylidene fluoride powder and conductive agent super P were put into a mortar in a mass ratio of 8:1:1 and ground for 30 minutes to obtain a mixture; then 900 μL of N-methylpyrrolidone was added to the mixture for stirring to obtain a mixed slurry; finally, the mixed slurry was evenly spread on a carbon-coated aluminum foil and dried to obtain a positive electrode sheet; the positive electrode sheet was assembled into a CR2032 battery in a glove box, the negative electrode material was a lithium sheet with a diameter of 13 mm, the diaphragm was Celgard2400, and the electrolyte was 1 mol LiPF6 dissolved in a EC:DEC:DMC solution with a volume ratio of 1:1:1.

[0054] The performance of the assembled lithium-ion battery was tested at a rate of 0.1C at 25°C (the voltage range of charge and discharge was 2.5-4.5V). The cycle performance diagrams of the lithium iron manganese phosphate positive electrode materials prepared in Example 1 and Comparative Example 1 are shown as follows: Figure 3 , Figure 4 As shown. Figure 3 It can be seen that the lithium manganese iron phosphate positive electrode material LiMn prepared in Example 1 0.6 Fe 0.4 When PO4 / C is used in lithium-ion batteries, after 150 cycles at 0.1C, its capacity can still reach 143mAh / g. Figure 4 It can be seen that the lithium manganese iron phosphate positive electrode material LiMn prepared in Comparative Example 1 0.6 Fe 0.4 When PO4 / C is used in lithium-ion batteries, its capacity is only 123 mAh / g after 150 cycles at 0.1C.

[0055] The performance of the lithium manganese iron phosphate positive electrode materials prepared in Example 1 and Comparative Example 1 was tested at a rate of 0.1C-0.5C-1C-2C-3C-2C-1C-0.5C-0.1C at 25°C (the charge and discharge voltage range was 2.5-4.5V). The rate performance results are as follows: Figure 5 shown by Figure 5 It can be seen that the lithium manganese iron phosphate positive electrode material LiMn prepared in Example 1 and Comparative Example 1 0.6 Fe 0.4 When PO4 / C is used in lithium-ion batteries, the capacities of the lithium-ion batteries are maintained at 138 mAh / g and 127 mAh / g respectively under a cycle of 3C. Example 1 has better cycle performance and rate performance.

[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. The above content is only to illustrate the technical idea of ​​the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution according to the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A high-rate performance lithium manganese iron phosphate cathode material based on co-precipitation, It is characterized in that Chemical formula of lithium iron manganese phosphate positive electrode material: LiMn x Fe 1-x PO 4 / C, where 0.2≤x≤0.

8.

2. A high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 1, It is characterized in that The chemical formula of lithium manganese iron phosphate positive electrode material: LiMn x Fe 1-x PO 4 / C, where x=0.4~0.

7.

3. A high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 1, It is characterized in that The chemical formula of lithium manganese iron phosphate positive electrode material: LiMn x Fe 1-x PO 4 / C, where x=0.5~0.

6.

4. A high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 1, It is characterized in that The lithium manganese iron phosphate positive electrode material has a uniform nanorod structure with a grain size of 200-500nm.

5. A method for preparing a high-rate performance lithium manganese iron phosphate positive electrode material based on coprecipitation according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Mixing a lithium source, phosphoric acid, an iron source, a manganese source and water, and performing a hydrothermal reaction to obtain a lithium iron manganese phosphate precursor; the chemical formula of the lithium iron manganese phosphate precursor is LiMn x Fe 1-x PO 4 , where 0.2≤x≤0.8; the temperature of the hydrothermal reaction is 150~200℃, and the time is 15~24h; (2) mixing the lithium iron manganese phosphate precursor, a carbon source and water, and carbon-coating the obtained mixture by spray drying to obtain a carbon-coated lithium iron manganese phosphate precursor; (3) calcining the carbon-coated lithium manganese iron phosphate precursor to obtain a lithium manganese iron phosphate positive electrode material with high rate performance.

6. A method for preparing a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 5, It is characterized in that In step (1), the lithium source includes lithium hydroxide monohydrate or lithium chloride; the iron source includes ferrous sulfate heptahydrate or ferrous chloride; the manganese source includes manganese sulfate or manganese chloride; The mass concentration of phosphoric acid is 75% to 90%, and the molar ratio of the lithium source, phosphoric acid, manganese source and iron source is 3:1:x:1-x, wherein 0.2≤x≤0.

8.

7. A method for preparing a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 5, It is characterized in that In step (2), the carbon source includes one or more of sucrose, glucose, starch or xylitol; the mass of the carbon source is 2% to 6% of the total mass of the lithium manganese iron phosphate precursor and the carbon source.

8. The method for preparing a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 5, It is characterized in that In step (2), in the spray drying method, the mass of the solid component accounts for 30% to 40% of the total mass of the mixture, the temperature of the spray dryer used is 150 to 180° C., and the spray feed rate is 10 to 20 mL / min.

9. The method for preparing a high-rate performance lithium iron manganese phosphate positive electrode material based on coprecipitation according to claim 5, It is characterized in that In step (3), the calcination temperature is 600-800°C and the calcination time is 3-5 hours.

10. Use of the high-rate performance lithium iron manganese phosphate positive electrode material according to any one of claims 1 to 4 in lithium-ion batteries.

Citation Information

Cited By

  • Preparation method and application of lithium manganese iron phosphate positive electrode material with uniformly mixed iron and manganese

    CN120097305A

  • Phosphate spherical material and preparation method thereof, compound positive electrode material and preparation method thereof, and lithium ion battery

    CN121107387A

  • A phosphate spherical material and its preparation method, a composite cathode material and its preparation method, and a lithium-ion battery.

    CN121107387B

  • Phosphate positive electrode material, preparation method thereof and battery

    CN121292393A

  • Positive electrode material, secondary battery, and electronic device

    WO2026153200A1