A glaze material with super white antibacterial properties and preparation method thereof
Through the Ti-Ag-Cu-Li-Zn element combination and one-time sintering process, the problems of dark color and complex process of ceramic glaze materials are solved, the ultra-white antibacterial effect and aesthetics of ceramic materials are achieved, and the process flow is simplified.
Patent Information
- Application Number
- CN202211721831.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-30
AI Technical Summary
Existing ceramic glaze materials perform well in antibacterial properties, but are dark in color, affecting the appearance, and require secondary sintering, which increases process complexity.
Using Ti-Ag-Cu-Li-Zn element combination, by adjusting the content of Ti and Zn, combined with cuprous oxide, an ultra-white antibacterial glaze material is prepared, using a one-time sintering process, using albite, quartz stone and diaspore The stone increases the whiteness, and achieves uniform coating and sintering of the glaze layer through spraying and ball milling steps.
It achieves the ultra-white color and high-efficiency antibacterial performance of ceramic materials, simplifies the process, avoids the complexity of secondary sintering, and significantly improves the aesthetics and antibacterial effect of the product.
Smart Images

Figure CN116023028B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sanitary ware, and particularly relates to a glaze material with super white and antibacterial properties and a preparation method thereof. Background Art
[0002] Sanitaryware is a crucial component of modern buildings, including plumbing equipment, toilets, and ceramic sinks and bathroom cabinets. Toilets and wash basins are the most common sanitaryware items, and these are typically made of ceramic. Ceramic refers to a class of inorganic, non-metallic materials made from natural or synthetic compounds through forming and high-temperature sintering. They possess advantages such as a high melting point, high hardness, excellent wear resistance, and oxidation resistance.
[0003] Because the color of the surface of the toilet and wash basin directly affects the first impression of the user or buyer. Among the ceramic materials of toilet seats, the applicant originally invented an antibacterial and wear-resistant glaze and its preparation method (CN202110859393.1). The ceramic material is used to solve the problem that the toilet seat is used to receive excrement. The wear resistance and density of its surface can effectively prevent the growth of bacteria remaining on the surface of the sanitary ware after flushing if the surface of the sanitary ware has a killing effect. Since the raw materials of the glaze layer material are to add zircon, spodumene, gallstone and other substances, the final fired glaze layer is black and dark, which is not conducive to the appearance of the product. The color of the toilet seat or ceramic wash basin directly affects whether the product is accepted by the public. Consumers usually prefer ultra-white products. In addition, the method in this technical solution involves the problem of secondary sintering. This application overcomes this defect, and the method provided can be completed by one sintering. Summary of the Invention
[0004] The present invention overcomes the defects of the prior art and provides a glaze material with super leucorrhea and antibacterial properties and a preparation method thereof. The glaze material has super leucorrhea skin feel and antibacterial properties.
[0005] The purpose of the present invention is achieved by at least one of the following technical solutions.
[0006] A super-white glaze material with antibacterial properties comprises the following substances, calculated by parts: 20-30 parts of hornblende, 40-50 parts of smithsonite, 80-100 parts of cuprite, 80-100 parts of white clay, 120-140 parts of talc, 1000-1200 parts of albite, 800-900 parts of quartz, 100-200 parts of spodumene, 680-830 parts of diaspore and 300-470 parts of titanium dioxide.
[0007] Preferably, the following substances are included, by parts: 25 parts of hornblende, 45 parts of smithsonite, 100 parts of cuprite, 90 parts of white mud, 130 parts of talc, 1100 parts of albite, 850 parts of quartz, 150 parts of spodumene, 870 parts of clay, 700 parts of diaspore and 350 parts of titanium dioxide.
[0008] In the present invention, the element combination of Ti-Ag-Cu-Li-Zn is adopted, and copper exists in the form of cuprous oxide. At the same time, the doped Ag can assist the antibacterial effect of cuprous oxide. In order to improve the whiteness of the color, in this application, by adjusting the content of Ti and Zn, the antibacterial metal elements are proportioned, so that the product has an ultra-white effect while having antibacterial properties.
[0009] A method for preparing an ultra-white glaze material with antibacterial properties comprises the following steps: firstly, half of a measured amount of albite, quartz, white mud and diaspore are mixed and ball-milled for later use; then, the other half of the measured amount of albite, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and ball-milled with water; then, the mixture is sprayed onto a ceramic body; then, a reserved slurry is sprayed on the mixture, and the mixture is calcined to obtain the glaze material.
[0010] The specific steps include:
[0011] (1) Take half of the measured amount of albite, quartz, white mud and diaspore, add water and ball mill to obtain slurry for later use;
[0012] (2) The other half of the sodium feldspar, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and then ball-milled into a slurry; the mass ratio of the water added to the raw materials is: 1 to 1.5:1;
[0013] (3) First, spray the slurry obtained in step (2) onto the ceramic body, and then spray the slurry obtained in step (1) onto it, and calcine at 900-1100° C. for 1-3 hours to obtain the ceramic body.
[0014] Further preferably, in step (1) and step (2), the ball milling time is 1 to 4 hours.
[0015] Further preferably, in step (3), the calcination temperature is 980° C.; and the calcination time is 3 hours.
[0016] Further preferably, in step (3), the spraying is performed 3 to 5 times.
[0017] Compared with the prior art, the advantages of the present invention are:
[0018] (1) The present application adjusts the element combination of Ti-Ag-Cu-Li-Zn, and copper exists in the form of cuprous oxide. At the same time, the doped Ag can assist the antibacterial effect of cuprous oxide. In the combination of the four elements, albite, quartz stone and diaspore with the effect of increasing whiteness are sprayed on the top layer of the product to increase whiteness.
[0019] (2) The present application overcomes the defect of the prior art that secondary calcination is required. By adjusting the ratio of raw materials, the product only needs to be sprayed, and then sintered once to obtain the target product. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a picture of the product obtained in Example 2.
[0021] Figure 2 This is a picture of the product obtained in Example 4. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific examples. The examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are commercially available unless otherwise specified.
[0023] Example 1
[0024] Take 20 parts of hornstone, 40 parts of smithsonite, 80 parts of cuprite, 80 parts of white mud, 120 parts of talc, 1000 parts of albite, 800 parts of quartz, 100 parts of spodumene, 680 parts of diaspore, and 300 parts of titanium dioxide in proportion to the weight of the mixture. The mass of the weighted substance is 3220 kg.
[0025] (1) Take half of the measured amount of albite, quartz, white mud and diaspore, add water and ball mill for 2 hours to obtain a slurry for later use;
[0026] (2) The other half of the sodium feldspar, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and then ball milled for 2 hours to form a slurry; the mass ratio of the water added to the raw materials is 1:1;
[0027] (3) First, spray the slurry obtained in step (2) onto the ceramic body (3 times, wait for it to dry thoroughly after each spraying before the next spraying), and then spray the slurry obtained in step (1) onto the ceramic body 3 times, wait for it to dry thoroughly after each spraying before the next spraying), and calcine at 1100°C for 1 hour to obtain the product.
[0028] Example 2
[0029] Take 25 parts of hornblende, 45 parts of smithsonite, 100 parts of cuprite, 90 parts of white mud, 130 parts of talc, 1100 parts of albite, 850 parts of quartz, 150 parts of spodumene, 870 parts of clay, 700 parts of diaspore, and 350 parts of titanium dioxide in proportion to the total mass of 4410 kg.
[0030] (1) Take half of the measured amount of albite, quartz, white mud and diaspore, add water and ball mill for 2 hours to obtain a slurry for later use;
[0031] (2) The other half of the measured amount of albite, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and then ball milled for 2 hours to form a slurry; the mass ratio of the water added to the raw materials is: 1.5:1;
[0032] (3) First, spray the slurry obtained in step (2) onto the ceramic body (5 times), and then spray the slurry obtained in step (1) onto the ceramic body (5 times), and calcine at 980°C for 3h to obtain the product.
[0033] Example 3
[0034] Calculate the weight of 30 parts of hornblende, 50 parts of smithsonite, 100 parts of cuprite, 100 parts of white mud, 140 parts of talc, 1200 parts of albite, 900 parts of quartz, 200 parts of spodumene, 830 parts of diaspore, and 470 parts of titanium dioxide. The total mass is 4020 kg.
[0035] (1) Take half of the measured amount of albite, quartz, white mud and diaspore, add water and ball mill for 2 hours to obtain a slurry for later use;
[0036] (2) The other half of the sodium feldspar, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and then ball milled for 2 hours to form a slurry; the mass ratio of the water added to the raw materials is 1:1;
[0037] (3) First, spray the slurry obtained in step (2) onto the ceramic body (4 times), and then spray the slurry obtained in step (1) onto the ceramic body (4 times), and calcine at 900°C for 3h to obtain the product.
[0038] Example 4
[0039] Calculate the weight of 25 parts of hornblende, 45 parts of smithsonite, 100 parts of cuprite, 45 parts of white mud, 130 parts of talc, 550 parts of albite, 425 parts of quartz, 150 parts of spodumene, 870 parts of clay, 350 parts of diaspore, and 350 parts of titanium dioxide. The total mass is 3040 kg.
[0040] (1) mixing argentite, smithsonite, cuprite, white mud, talc, albite, quartz, spodumene, clay, diaspore and titanium dioxide, adding water and then ball milling for 2 hours to form a slurry; the mass ratio of the water added to the raw materials is: 1.5:1;
[0041] (2) Spray the slurry obtained in step (1) onto the ceramic body (5 times) and calcine at 980° C. for 3 h to obtain the ceramic body.
[0042] The ceramic sheets prepared in Examples 1 to 4 were used to perform microbial antibacterial tests. The test results are shown in Tables 1 and 2.
[0043] Table 1
[0044]
[0045] Table 2
[0046]
[0047]
[0048] From the data in Table 1 and Table 2, it can be concluded that after 24 hours of incubation, the ceramic plate sample in Example 1 has an antibacterial rate of 77% against Escherichia coli AS1.90 and an antibacterial rate of 99% against Staphylococcus aureus AS1.89.
[0049] After culturing the ceramic plate sample in Example 2 for 24 hours, the antibacterial rate of Escherichia coli AS1.90 was 81%, and the antibacterial rate of Staphylococcus aureus AS1.89 was 99%.
[0050] After culturing the ceramic plate sample in Example 3 for 24 hours, the antibacterial rate of Escherichia coli AS1.90 was 76%, and the antibacterial rate of Staphylococcus aureus AS1.89 was 99%.
[0051] After culturing the ceramic plate sample in Example 4 for 24 hours, the antibacterial rate of Escherichia coli AS1.90 was 84%, and the antibacterial rate of Staphylococcus aureus AS1.89 was 99%.
[0052] The whiteness comparison of the products obtained in Example 2 and Example 4 is as follows: Figure 1 and Figure 2 As shown, after comparison, the color difference between the two is obvious. Figure 1 The product shows super white color, Figure 2 It is white with yellow.
Claims
1. A super white glaze material with antibacterial properties, characterized in that: The following substances are included by weight: 20-30 parts of hornblende, 40-50 parts of smithsonite, 80-100 parts of cuprite, 80-100 parts of white mud, 120-140 parts of talc, 1000-1200 parts of albite, 800-900 parts of quartz, 100-200 parts of spodumene, 680-830 parts of diaspore and 300-470 parts of titanium dioxide; The method for preparing the ultra-white glaze material with antibacterial properties specifically comprises the following steps: (1) Take half of the measured amount of albite, quartz, white mud and diaspore, add water and ball grind to obtain slurry for use; (2) The other half of the albite, quartz, white mud and diaspore are mixed with hornblende, smithsonite, cuprite, talc, spodumene and titanium dioxide, and then ball-milled into a slurry; the mass ratio of the water added to the raw materials is 1-1.5:1; (3) First, spray the slurry obtained in step (2) onto the ceramic body, and then spray the slurry obtained in step (1) onto the ceramic body, and calcine at 900-1100° C. for 1-3 hours to obtain the ceramic body.
2. The ultra-white glaze material with antibacterial properties according to claim 1 is characterized in that: In step (1) and step (2), the ball milling time is 1 to 4 hours.
3. The ultra-white glaze material with antibacterial properties according to claim 1, characterized in that: In step (3), the calcination temperature is 980° C. and the calcination time is 3 h.
4. The ultra-white glaze material with antibacterial properties according to claim 1, characterized in that: In step (3), the spraying is performed 3 to 5 times.