A carbide composite powder precursor and its preparation method and application
Through the mixing of iron group metal organic alkoxide solution and carbide and temperature gradient calcination, the problem of controlling the carbon content of the carbide precursor is solved, and a carbide composite powder precursor with a more uniform structure and excellent performance is prepared for hardening. The modification of cemented carbide materials improves the performance of cemented carbide materials.
Patent Information
- Application Number
- CN202310060680.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-17
AI Technical Summary
It is difficult to accurately control the amount of carbon in the preparation of carbide precursors using the existing technology, resulting in large errors in the carbon content in the carbide precursors and unable to meet the production needs of high-quality cemented carbide materials.
The carbide composite powder precursor is prepared by mixing, drying and calcining the iron group metal organic alkoxide solution with the carbide. The precise preparation of the carbide composite powder precursor is achieved through wet grinding in a ball mill and temperature gradient calcination under hydrogen protection.
This method can achieve precise control of the carbon content of carbide precursors, improve the microstructure and physical properties of cemented carbide materials, and improve the wettability of the hard phase and bonding phase of cemented carbide and steel-bonded cemented carbide. , to prepare better materials.
Smart Images

Figure CN116043088B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of cemented carbide and steel-bonded cemented carbide materials, and belongs to the technical field of alloy material preparation. Background Art
[0002] The preparation and research of carbide precursors have always been a hot topic in the preparation technology of metal composite materials, and are also the key technology to solve the development of metal composite materials. At present, a type of carbide precursor is mainly prepared by mixing a metal salt solution with a liquid or gaseous carbon source and reducing and calcining it. However, this method of preparing carbide precursors has a large error fluctuation in the carbon content of the final prepared carbide precursor due to the difficulty in accurately controlling the carbon content; it cannot meet the demand for preparing a type of high-quality alloy using the traditional cemented carbide material production process route. Summary of the invention
[0003] The purpose of the present invention is to provide a carbide composite powder precursor and its preparation method and application method in view of the technical problems in the above background technology. A carbide composite powder precursor is prepared by mixing, drying and calcining an iron group metal organic alcohol salt solution with a carbide. The carbide composite powder precursor replaces the hard phase in cemented carbide or is used independently as a type of composite powder in the preparation process of cemented carbide to solve the problem of surface modification of hard phase carbides in cemented carbide.
[0004] The solution provided by the present invention is as follows:
[0005] A method for preparing a carbide composite powder precursor comprises the following steps:
[0006] Carbide and iron group metal organic alkoxide solution are ball-milled and mixed in proportion, and dried to obtain a mixture of iron group metal organic alkoxide and carbide; finally, the mixture is calcined to obtain a carbide composite powder precursor.
[0007] Further preferably, the ratio of the iron group metal organic alkoxide solution to the carbide is 50 ml / Kg to 3000 ml / Kg.
[0008] More preferably, the mass concentration of the iron group metal in the iron group metal organic alkoxide solution is ≥5 g / L; the carbide comprises one or two of WC and TiC. The chemical formula of the iron group metal organic alkoxide is Me y (OEt) x , Me represents Co, Ni, Fe.
[0009] Further preferably, the carbide is a carbide with a Fisher particle size of 0.2 μm to 100 μm and a combined carbon content of ≥5.9 wt%.
[0010] Further preferably, when the carbide is WC, its Fischer-Tropsch particle size is 0.2 μm to 100 μm, wherein the combined carbon is ≥5.9 wt%; when the carbide is TiC, its Fischer-Tropsch particle size is 0.5 μm to 100 μm, wherein the combined carbon is ≥18.5 wt%.
[0011] Further preferably, the weight ratio of the carbide to the ball milling medium in the ball milling mixing process is 1:1 to 1:20; the ball milling medium is a steel ball or a cemented carbide ball or a steel rod or a cemented carbide rod, and the size of the ball is ∮5 to ∮15 mm, and the rod is ∮5×15 to ∮15×20 mm. The ball mill wet milling process can fully mix the iron group metal organic alkoxide solution with the carbide, effectively crush the carbide, and fully adsorb the iron group metal organic alkoxide on the surface of the carbide.
[0012] Further preferably, when the mixture of the iron group metal organic alkoxide and the carbide is calcined, the calcination is performed with a temperature gradient under hydrogen protection conditions. The calcination with a temperature gradient under hydrogen protection conditions can fully reduce the iron group metal organic alkoxide to iron group element metal ions, which are uniformly adsorbed on the surface of the carbide to obtain a carbide composite powder precursor.
[0013] More preferably, the temperature gradient adopts different temperature increase gradients according to the type of carbide.
[0014] When the carbide is WC, its temperature gradient is as follows:
[0015] The temperature is raised from room temperature to 150-190°C at a heating rate of 1°C-20°C / min, and then kept at 150-190°C for 30-120 min.
[0016] Then, the temperature is raised to 210-290°C at a heating rate of 1°C-20°C / min, and then kept at 210-290°C for 30-180 min.
[0017] Then, the temperature is raised to 320-380°C at a heating rate of 1°C-20°C / min, and then kept at 320-380°C for 30-360 min.
[0018] Then, the temperature is raised to 420-480°C at a heating rate of 1°C-10°C / min, and then kept at 420-480°C for 60-240 min.
[0019] Then, the temperature is raised to 650-780°C at a heating rate of 1°C-20°C / min, and then kept at 650-780°C for 60-240 min.
[0020] Then, the temperature is raised to 850-980°C at a heating rate of 2-20°C / min, and then kept at 850-980°C for 30-120 minutes.
[0021] Then the temperature is lowered from 850 to 980° C. to room temperature at a cooling rate of 10 to 25° C. / min to obtain a WC-containing carbide composite powder precursor.
[0022] When the carbide is TiC, its temperature gradient is as follows:
[0023] The temperature is raised from room temperature to 150-190°C at a heating rate of 1°C-20°C / min, and then kept at 150-190°C for 30-120 min.
[0024] Then, the temperature is raised to 210-290°C at a heating rate of 1°C-20°C / min, and then kept at 210-290°C for 30-180 min.
[0025] Then, the temperature is raised to 320-380°C at a heating rate of 1°C-20°C / min, and then kept at 320-380°C for 30-360 min.
[0026] Then, the temperature is raised to 420-480°C at a heating rate of 1°C-10°C / min, and then kept at 420-480°C for 60-240 min.
[0027] Then, the temperature is raised to 650-780°C at a heating rate of 1°C-20°C / min, and then kept at 650-780°C for 60-240 min.
[0028] Then, the temperature is increased to 1000-1080°C at a heating rate of 2-20°C / min, and then kept at 1000-1080°C for 30-120 minutes.
[0029] Then the temperature is lowered from 1000-1080° C. to room temperature at a cooling rate of 10-25° C. / min to obtain a carbide composite powder precursor containing TiC.
[0030] Based on the same technical idea, the present invention also provides a carbide composite powder precursor, and the carbide composite powder precursor is prepared by the above-mentioned preparation method.
[0031] Based on the same technical idea, the present invention also provides an application method of a carbide composite powder precursor, and the carbide composite powder precursor is used as a hard phase of cemented carbide and steel-bonded cemented carbide or as an independent type of composite powder in the preparation process of cemented carbide.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention proposes a new idea for preparing a carbide precursor, that is, preparing a carbide composite powder precursor by mixing carbide powder with an iron group metal organic alcohol salt solution. The preparation method of the present invention adopts a combined firing of solid materials, and the preparation steps are simple, and the carbon content of the carbide precursor can be accurately controlled.
[0034] The present invention fully mixes the iron group metal organic alkoxide solution and carbide by wet grinding in a ball mill, and then obtains the iron group metal organic alkoxide and carbide mixture by vacuum stirring drying or spray drying, and then calcines at an appropriate temperature under hydrogen protection conditions to obtain a carbide composite powder precursor with multiple uses. The carbide composite powder precursor prepared by the present invention can be used as a hard phase of cemented carbide and steel-bonded cemented carbide or independently used as a type of composite powder in the preparation process of cemented carbide, and the hard phase surface of the cemented carbide is modified to prepare a cemented carbide and steel-bonded cemented carbide with more uniform microstructure and better physical performance indicators. When the carbide composite powder precursor prepared by the preparation method of the present invention is used as a hard phase in a cemented carbide material, it can improve the wettability of the hard phase and the bonding phase of the cemented carbide material during the sintering process, thereby obtaining a type of cemented carbide material with better microstructure and physical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a scanning electron microscope image of the TiC+Co composite powder precursor prepared in Example 1;
[0036] Figure 2 for Figure 1 Energy spectrum diagram of TiC grains in (where A1 is TiC grain surface scan, B1 is TiC grain surface scan energy spectrum, and C1 is TiC grain surface scan energy spectrum data statistics);
[0037] Figure 3 This is a scanning electron microscope image of the TiC+Ni composite powder precursor prepared in Example 2;
[0038] Figure 4 for Figure 3 Energy spectrum diagram of TiC grains in (A2 is the TiC grain surface scan, B2 is the TiC grain surface scan energy spectrum, and C2 is the TiC grain surface scan energy spectrum data statistics);
[0039] Figure 5 This is a scanning electron microscope image of the TiC+Co+Ni composite powder precursor prepared in Example 3;
[0040] Figure 6 for Figure 5 Energy spectrum diagram of TiC grains in (A3 is the TiC grain surface scan, B3 is the TiC grain surface scan energy spectrum, and C3 is the TiC grain surface scan energy spectrum data statistics);
[0041] Figure 7 This is a scanning electron microscope image of the WC+Co+Ni composite powder precursor prepared in Example 4;
[0042] Figure 8 for Figure 7 Energy spectrum diagram of WC grains in the middle (A4 is the WC grain surface scan, B4 is the WC grain surface scan energy spectrum, and C4 is the WC grain surface scan energy spectrum data statistics);
[0043] Fig. 9 This is a metallographic photograph of a cemented carbide material prepared using the TiC+Co composite powder precursor prepared in Example 1 as the hard phase;
[0044] Fig.10 This is a metallographic photograph of the cemented carbide material prepared with TiC as the hard phase. DETAILED DESCRIPTION
[0045] In order to facilitate the understanding of the present invention, the present invention is described in more comprehensive and detailed manner below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0046] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0047] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0048] Example 1
[0049] In this embodiment, the chemical formula of a cobalt metal organic alkoxide solution is Co x (OEt) y ; A method for preparing a TiC-Co composite powder precursor by mixing a cobalt metal organic alkoxide solution with titanium carbide powder, drying and calcining the mixture is completed by the following steps:
[0050] 1. Ingredients:
[0051] ①. Weigh the cobalt metal organic alkoxide solution:
[0052] A cobalt metal organic alkoxide solution with a Co mass concentration of 30 g / L was selected, and 300 ml of the cobalt metal organic alkoxide solution was weighed per kilogram of titanium carbide powder.
[0053] ②. Weigh titanium carbide powder:
[0054] A titanium carbide powder having a carbon content of 18.75 wt % and a Fisher particle size greater than 0.5 μm but less than 8 μm is selected and weighed to 1 kg.
[0055] ③. Weigh the hard alloy baseball grinding medium:
[0056] Select three sizes of cemented carbide rods of ∮5×15, ∮10×15 and ∮15×20 mm, and weigh 6 kg of cemented carbide rods according to the configuration of cemented carbide rod weight of 1:1:1 and the weight ratio of titanium carbide powder to cemented carbide rod of 1:6.
[0057] ④. Weigh the organic fat forming agent:
[0058] PEG4000 was selected as the molding agent, and 30 g of PEG4000 was weighed per kilogram of titanium carbide powder.
[0059] ⑤. Weigh the ethanol solution:
[0060] Weigh 300 ml of ethanol solution per kilogram of titanium carbide powder.
[0061] 2. Mixing:
[0062] The cobalt metal organic alkoxide solution, titanium carbide powder, hard alloy baseball milling medium, organic fat forming agent and ethanol solution obtained in step 1 are put into a ball mill for ball milling. The speed of the ball mill is 60r / min and the ball milling time is 60h to obtain a mixture slurry of the cobalt metal organic alkoxide solution and titanium carbide.
[0063] 3. Drying:
[0064] The mixture slurry obtained in step 2 is dried by vacuum stirring or spray drying at a drying temperature of 80° C. to 110° C. to obtain a mixture of cobalt metal organic alkoxide solution and titanium carbide.
[0065] 4. Calcination:
[0066] The mixed material obtained in step 3 is placed in a boat, and then calcined under hydrogen protection conditions.
[0067] The temperature was raised from room temperature to 150°C at a heating rate of 15°C / min, and then kept at 150°C for 60 min.
[0068] The temperature was then raised to 270°C at a heating rate of 10°C / min, and then kept at 270°C for 90 min.
[0069] The temperature was then raised to 350°C at a heating rate of 10°C / min, and then kept at 350°C for 180 min.
[0070] The temperature was then raised to 450°C at a heating rate of 5°C / min, and then kept at 450°C for 180 min.
[0071] The temperature was then raised to 650°C at a heating rate of 10°C / min, and then kept at 650°C for 180 min.
[0072] The temperature was then raised to 1050°C at a heating rate of 10°C / min, and then kept at 1050°C for 90 min.
[0073] The temperature was then lowered from 1050°C to room temperature at a cooling rate of 20°C / min to obtain a TiC-Co composite powder precursor.
[0074] The composite powder precursor prepared in this embodiment was tested, and the structure was as follows Figure 1 and Figure 2 shown.
[0075] The TiC-Co composite powder precursor prepared in this embodiment is used as the hard phase. The cemented carbide material is prepared according to the ratio of 50wt% TiC-Co composite powder precursor, 50wt% Fe and other 50wt%. The cemented carbide material is tested and the results show that: hardness: 85.0HRA; flexural strength: 2400MPa; density: 6.15g / cm 3 ; Metallographic photos such as Fig. 9 As shown. With TiC as the hard phase, cemented carbide material is prepared according to the ratio of TiC 50wt%, Fe and other 50wt%. The cemented carbide material is tested and the results show that: hardness: 82.0HRA; bending strength: 1600MPa; density: 6.05g / cm 3 ; Metallographic photos such as Fig.10 shown.
[0076] By comparing the test results of cemented carbide materials prepared with two different hard phases, it can be known that the TiC-Co composite powder precursor prepared in this embodiment as the hard phase can improve the bending strength of the cemented carbide material by more than 40%; the metallographic photograph shows that the structure is also more uniform, indicating that the TiC-Co composite powder precursor effectively improves the wettability of the interface between the hard phase and the bonding phase, enhances the solubility of TiC grains in the iron group elements, generates a better interface bonding between the hard phase and the bonding phase, and enables the bonding phase to obtain better solid solution strengthening.
[0077] This embodiment has the following beneficial effects:
[0078] ①. This embodiment proposes for the first time a method for preparing a TiC-Co composite powder precursor, in which a cobalt metal organic alkoxide solution and titanium carbide powder are fully mixed by wet grinding with a ball mill, and then a mixture of cobalt metal organic alkoxide solution and titanium carbide powder is obtained by vacuum stirring drying or spray drying, and then calcined at an appropriate temperature under hydrogen protection conditions to obtain a TiC-Co composite powder precursor.
[0079] ② This embodiment uses three sizes of cemented carbide rods of ∮5×15, ∮10×15 and ∮15×20 mm, which are configured according to the weight of the cemented carbide rods at a ratio of 1:1:1 and the weight ratio of titanium carbide powder to cemented carbide rods at a ratio of 1:6. Ball milling for 60 hours at a ball mill speed of 60 r / min can make the cobalt metal organic alcohol salt solution and the titanium carbide powder mixed evenly, and the titanium carbide powder is fully crushed, so that the cobalt metal ions are fully adsorbed on the surface of the titanium carbide grains.
[0080] ③ In this embodiment, 30 g of PEG4000 is used as a molding agent and vacuum stirring drying or spray drying is performed at a drying temperature of 80°C to 110°C, which helps to avoid oxygenation of the mixture and obtain a composite powder mixture with more uniform composition.
[0081] ④ This embodiment adopts staged temperature-controlled calcination under hydrogen protection conditions, which can fully reduce the cobalt metal ions and uniformly adsorb them on the surface of titanium carbide to obtain a TiC-Co composite powder precursor.
[0082] ⑤ This embodiment proposes for the first time a method for surface modification of titanium carbide powder. Replacing the hard phase TiC in the cemented carbide material with the TiC-Co composite powder precursor prepared in this embodiment can effectively improve the wettability between the hard phase and the bonding phase of the cemented carbide material during the sintering process, thereby obtaining a type of cemented carbide material with better microstructure and physical properties.
[0083] ⑥ The present invention can obtain a TiC-Co composite powder precursor powder.
[0084] Example 2
[0085] The difference between this embodiment and embodiment 1 is that the chemical formula of the iron metal organic alkoxide solution is Nix(OEt)y; the mass concentration of Ni in the nickel metal organic alkoxide solution in step 1① is 80g / L; the other steps are the same as those in embodiment 1. The composite powder precursor prepared in this embodiment is tested, and the structure is as follows Figure 3 and Figure 4 shown.
[0086] Example 3
[0087] The difference between this embodiment and specific embodiment 1 is that the chemical formula of the iron group metal organic alkoxide solution is (Co x1 Ni x2 )(OEt) y ; X1+X2=1; the mass concentration of cobalt+nickel metal in the (cobalt+nickel) metal organic alkoxide solution in step 1① is 100g / L; the other steps are the same as those in specific embodiment 1. The composite powder precursor prepared in this embodiment is tested, and the structure is as follows Figure 5 and Figure 6 shown.
[0088] Example 4
[0089] The chemical formula of the (cobalt + nickel) metal organic alkoxide solution in this embodiment is (Co x1 Ni x2 )(OEt)y; the X1+X2=1; the (cobalt+nickel) metal organic alcohol salt solution is mixed with tungsten carbide powder, dried, and calcined to prepare a WC-Co+Ni composite powder precursor according to the following steps:
[0090] 1. Ingredients:
[0091] ①. Weigh (cobalt + nickel) metal organic alkoxide solution:
[0092] A (cobalt + nickel) metal organic alkoxide solution with a cobalt + nickel metal mass concentration of 120 g / L was selected, and 700 ml of the (cobalt + nickel) metal organic alkoxide solution was weighed per kilogram of titanium carbide powder.
[0093] ②. Weigh tungsten carbide powder:
[0094] Select tungsten carbide powder with a carbon content of 6.15 wt % and a Fisher particle size greater than 0.2 μm but less than 5 μm, and weigh 1 kg.
[0095] ③. Weigh the hard alloy baseball grinding medium:
[0096] Select three sizes of cemented carbide rods of ∮5×15, ∮10×15 and ∮15×20 mm, and weigh 6 kg of cemented carbide rods according to the configuration of cemented carbide rod weight of 1:1:1 and the weight ratio of titanium carbide powder to cemented carbide rod of 1:6.
[0097] ⑤. Weigh the organic fat forming agent:
[0098] PEG4000 was selected as the molding agent, and 60 g of PEG4000 was weighed per kilogram of titanium carbide powder.
[0099] ⑤. Weigh the ethanol solution:
[0100] Weigh 300 ml of ethanol solution per kilogram of titanium carbide powder.
[0101] 2. Mixing:
[0102] The (cobalt + nickel) metal organic alkoxide solution obtained in step 1, tungsten carbide powder, carbide baseball grinding medium, organic fat forming agent, and ethanol solution are put into a ball mill for ball milling. The speed of the ball mill is 45r / min, and the ball milling time is 40h to obtain a mixture slurry of (cobalt + nickel) metal organic alkoxide solution and titanium carbide.
[0103] 3. Drying:
[0104] The mixture slurry obtained in step 2 is dried by vacuum stirring or spray drying at a drying temperature of 80° C. to 110° C. to obtain a mixture of (cobalt+nickel) metal organic alcohol salt solution and tungsten carbide.
[0105] 4. Calcination:
[0106] The mixed material obtained in step 3 is placed in a boat, and then calcined under hydrogen protection conditions.
[0107] The temperature was raised from room temperature to 150°C at a rate of 15°C / min, and then kept at 150°C for 60 min.
[0108] The temperature was then raised to 270°C at a heating rate of 10°C / min, and then kept at 270°C for 90 min.
[0109] The temperature was then raised to 350°C at a heating rate of 10°C / min, and then kept at 350°C for 180 min.
[0110] The temperature was then raised to 450°C at a heating rate of 5°C / min, and then kept at 450°C for 180 min.
[0111] The temperature was then raised to 700°C at a heating rate of 10°C / min, and then kept at 700°C for 180 min.
[0112] The temperature was then raised to 950°C at a heating rate of 10°C / min, and then kept at 950°C for 90 min.
[0113] The temperature was then cooled from 950°C to room temperature at a cooling rate of 20°C / min to obtain a WC-Co+Ni composite powder precursor.
[0114] The composite powder precursor prepared in this embodiment was tested, and the structure was as follows Figure 7 and Figure 8 shown.
[0115] This embodiment has the following beneficial effects:
[0116] ①. This embodiment proposes for the first time a method for preparing a WC-Co+Ni composite powder precursor. The (cobalt+nickel) metal organic alkoxide solution and tungsten carbide powder are fully mixed by wet grinding with a ball mill, and then a mixture of (cobalt+nickel) metal organic alkoxide solution and titanium tungsten carbide powder is obtained by vacuum stirring drying or spray drying, and then calcined at an appropriate temperature under hydrogen protection conditions to obtain a WC-Co+Ni composite powder precursor.
[0117] ②. This embodiment uses three sizes of cemented carbide rods: ∮5×15, ∮10×15 and ∮15×20 mm. The cemented carbide rods are configured at a weight ratio of 1:1:1 and the weight ratio of tungsten carbide powder to cemented carbide rods is 1:6. Ball milling for 40 hours at a ball mill speed of 45r / min can make the (cobalt + nickel) metal organic alcohol salt solution and tungsten carbide powder mixed evenly, and the tungsten carbide powder is fully crushed, so that the (cobalt + nickel) metal ions are fully adsorbed on the surface of tungsten carbide grains.
[0118] ③. This embodiment uses 60 grams of PEG4000 as a molding agent and performs vacuum stirring drying or spray drying at a drying temperature of 80°C to 110°C, which helps to avoid oxygenation of the mixture and obtain a composite powder mixture with more uniform composition.
[0119] ④. This embodiment adopts temperature-controlled calcination in stages under hydrogen protection conditions, which can fully reduce the (cobalt + nickel) metal ions and uniformly adsorb them on the surface of titanium carbide to obtain a WC-Co + Ni composite powder precursor.
[0120] ⑤. This embodiment proposes for the first time a method for surface modification of tungsten carbide powder. Replacing the hard phase WC in the cemented carbide material with the WC-Co+Ni composite powder precursor prepared in this embodiment can effectively improve the wettability between the hard phase and the bonding phase of the cemented carbide material during the sintering process, thereby obtaining a type of cemented carbide material with better microstructure and physical properties.
[0121] ⑥ The present invention can obtain a WC-Co+Ni composite powder precursor powder.
[0122] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a carbide composite powder precursor, characterized in that: The following steps are involved: The carbide and the iron group metal organic alkoxide solution are ball-milled and mixed in proportion, and after drying, a mixture of the iron group metal organic alkoxide and the carbide is obtained; finally, the mixture is calcined to obtain a carbide composite powder precursor; The chemical formula of the iron group metal organic alkoxide is Me y (OEt) x , Me represents Co, Ni, Fe; The carbide includes one or two of WC and TiC; The temperature gradient adopts different temperature rising gradients according to the type of carbide; When the carbide is WC, its temperature gradient is as follows: Heat from room temperature to 150-190°C at a rate of 1°C-20°C / min, and then keep at 150-190°C for 30-120 min; Then, the temperature is raised to 210-290°C at a heating rate of 1°C-20°C / min, and then kept at 210-290°C for 30-180 min; Then, the temperature was raised to 320-380°C at a heating rate of 1°C-20°C / min, and then kept at 320-380°C for 30-360 min; Then, the temperature is raised to 420-480°C at a heating rate of 1°C-10°C / min, and then kept at 420-480°C for 60-240 min; Then, the temperature is raised to 650-780°C at a heating rate of 1°C-20°C / min, and then kept at 650-780°C for 60-240 min; Then, the temperature is raised to 850-980°C at a heating rate of 2-20°C / min, and then kept at 850-980°C for 30-120 min; Then, the temperature is lowered from 850-980°C to room temperature at a cooling rate of 10-25°C / min to obtain a WC-containing carbide composite powder precursor; When the carbide is TiC, its temperature gradient is as follows: Heat from room temperature to 150-190°C at a rate of 1°C-20°C / min, and then keep at 150-190°C for 30-120 min; Then, the temperature is raised to 210-290°C at a heating rate of 1°C-20°C / min, and then kept at 210-290°C for 30-180 min; Then, the temperature was raised to 320-380°C at a heating rate of 1°C-20°C / min, and then kept at 320-380°C for 30-360 min; Then, the temperature is raised to 420-480°C at a heating rate of 1°C-10°C / min, and then kept at 420-480°C for 60-240 min; Then, the temperature is raised to 650-780°C at a heating rate of 1°C-20°C / min, and then kept at 650-780°C for 60-240 min; Then, the temperature is raised to 1000-1080°C at a heating rate of 2-20°C / min, and then kept at 1000-1080°C for 30-120 min; The temperature is then lowered from 1000-1080°C to room temperature at a cooling rate of 10-25°C / min to obtain a carbide composite powder precursor containing TiC.
2. The preparation method according to claim 1, characterized in that The ratio of the iron group metal organic alkoxide solution to the carbide is 50 ml / Kg to 3000 ml / Kg.
3. The preparation method according to claim 2, characterized in that: The mass concentration of the iron group metal in the iron group metal organic alkoxide solution is ≥5 g / L.
4. The preparation method according to claim 3, characterized in that: The carbide has a Fisher particle size of 0.2 μm to 100 μm and a combined carbon content of ≥5.9 wt%.
5. The preparation method according to claim 4, characterized in that: When the carbide is WC, its Fischer-Tropsch particle size is 0.2 μm to 100 μm, wherein the combined carbon is ≥5.9 wt %; when the carbide is TiC, its Fischer-Tropsch particle size is 0.5 μm to 100 μm, wherein the combined carbon is ≥18.5 wt %.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The weight ratio of the carbide to the ball milling medium during the ball milling mixing process is 1:1-1:20; the ball milling medium is a steel ball or a cemented carbide ball or a steel rod or a cemented carbide rod, the size of the ball is ∮5-∮15mm, and the size of the rod is ∮5×15-∮15×20mm.
7. The preparation method according to claim 6, characterized in that: When the mixture of the iron group metal organic alkoxide and the carbide is calcined, the calcination is carried out in a temperature gradient under the protection of hydrogen.
8. A carbide composite powder precursor, characterized in that: The carbide composite powder precursor is prepared by the preparation method according to any one of claims 1 to 7.
9. An application of a carbide composite powder precursor, characterized in that: The carbide composite powder precursor according to claim 8 is used as the hard phase of cemented carbide and steel-bonded cemented carbide or independently as a type of composite powder in the preparation process of cemented carbide.