Resin composition for hollow blow molding and preparation method and application thereof

Through the combination of hexene copolymerized polyethylene resin and additives, the problems of low HDPE resin yield and insufficient performance are solved, and a resin composition suitable for hollow blow molding is prepared, which improves the low-temperature impact performance and modulus and meets the needs of large hollow Containers and plastic pallets are in demand.

CN116063771BActive Publication Date: 2024-10-25CHINA PETROLEUM & CHEMICAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111276406.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-25
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Domestic HDPE resins for large hollow molding have few grades, low output, low melt index, and poor melt fluidity, making it difficult to meet market demand. In addition, large hollow products have deficiencies in low-temperature impact performance and stacking resistance.

Method used

Hexene copolymerized polyethylene resin is combined with additives. By reacting ethylene and 1-hexene at 90-95°C in the presence of a chromium catalyst, a resin composition with low melt index and good low-temperature impact performance is prepared, which is suitable for Hollow blow molding, especially large hollow containers and plastic pallets.

Benefits of technology

The low-temperature impact performance and modulus of the resin composition are improved, and the resin composition has good rigidity and toughness balance properties, meets the processing requirements of large hollow containers and plastic pallets, and improves the performance balance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003330051640000081
    Figure BDA0003330051640000081
Patent Text Reader

Abstract

The present invention provides a resin composition for hollow blow molding, a preparation method and an application thereof, wherein the resin composition comprises a hexene copolymer polyethylene resin and an auxiliary agent; wherein, as measured according to GB / T 3682-2000, at 190°C and 21.6kg, the melt flow rate of the hexene copolymer polyethylene resin is 2.1-2.3g / 10min; and the molecular weight distribution Mw / Mn of the hexene copolymer polyethylene resin is 13-17, and the density is 0.950-0.960g / cm 3 The resin composition of the present invention has a low melt index, good low-temperature impact performance, high modulus, and good rigidity-toughness balance, and is suitable for blowing hollow containers and plastic pallets, especially large hollow containers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hollow blow molding, and in particular relates to a resin composition for hollow blow molding and a preparation method and application thereof. Background Art

[0002] Large hollow containers are mainly made of high-density polyethylene (HDPE) resin. Currently, large hollow container products have been widely used to contain various hazardous and non-hazardous chemicals, oils and other liquids, and are gradually replacing metal containers. However, there are few domestic HDPE resin brands for large hollow molding, and the output is low, which is far from meeting market demand.

[0003] The existing large hollow materials in China are mainly 1158 powder from Qilu Branch, TR550 powder from Shanghai Jinfei and HD5420GA from Dushanzi, while high-performance large barrel special materials are completely dependent on imports. On the one hand, the melting index of HDPE large hollow special materials is low, its melt fluidity is poor, the raw material production is very difficult, and the production capacity is low; on the other hand, large hollow products are mainly used in the packaging and transportation of dangerous goods, which requires very strict performance of large hollow raw materials, and it is difficult to ensure the balance of product performance during raw material production. Therefore, domestic synthetic resin manufacturers have encountered thorny problems in the development and production of HDPE large hollow special materials.

[0004] The large hollow products on the market have insufficient low-temperature impact performance, breakage in drop tests, and poor stacking resistance. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a resin composition for hollow blow molding and a preparation method and application thereof to address the technical problems existing in the prior art. The resin composition of the present invention has a low melt index, good low-temperature impact performance, high modulus, and good rigidity-toughness balance, and is suitable for blowing hollow containers and plastic pallets, especially large hollow containers.

[0006] The objective of the present invention is achieved through the following technical solution.

[0007] In a first aspect, the present invention provides a resin composition for hollow blow molding, wherein the resin composition comprises a hexene copolymer polyethylene resin and an additive; wherein, as measured according to GB / T 3682-2000, at 190°C and 21.6kg, the melt flow rate (melt index) of the hexene copolymer polyethylene resin is 2.1 to 2.3 g / 10min; and the molecular weight distribution Mw / Mn of the hexene copolymer polyethylene resin is 13 to 17, and the density is 0.950 to 0.960 g / cm 3 .

[0008] The present invention adopts a specific hexene copolymer polyethylene resin and adds an auxiliary agent to obtain a resin composition for hollow blow molding, which has a low melt index, good low-temperature impact performance, high modulus, and good rigidity-toughness balance, and is suitable for blowing hollow containers and plastic pallets, especially large hollow containers.

[0009] In the present invention, the term "large hollow container" refers to a hollow container with a volume of 20L or more, for example, a hollow container with a volume of 200L.

[0010] According to the resin composition provided by the present invention, the density of the hexene copolymer polyethylene resin is 0.950-0.956 g / cm 3 .

[0011] According to the resin composition provided by the present invention, the content of 1-hexene repeating units in the hexene copolymer polyethylene resin is 0.1 to 0.2 mol%, preferably 0.13 to 0.18 mol%.

[0012] According to the resin composition provided by the present invention, the hexene copolymer polyethylene resin is prepared by a method comprising the following steps: ethylene and 1-hexene are reacted at a temperature of 90 to 95° C. in the presence of a diluent and a chromium catalyst.

[0013] In the present invention, C3-C6 alkanes can be used as diluents. In some embodiments, the diluent is isobutane. The diluent can be recycled, thereby reducing costs and reducing waste gas emissions.

[0014] In some embodiments, relative to ethylene feed amount of 25 t / h, the amount of the diluent used is 23-35 kg / h, preferably 25-30 kg / h.

[0015] In some embodiments, the molar ratio of ethylene to 1-hexene is 1000:5-10.

[0016] In some embodiments, the amount of the chromium catalyst is 0.05-1 wt %, preferably 0.1-0.8 wt %, more preferably 0.2-0.6 wt %, and most preferably 0.4-0.5 wt %, based on the weight of ethylene.

[0017] In some embodiments, the reaction to prepare hexene copolymer polyethylene resin is carried out in a Phillips loop slurry unit.

[0018] In the present invention, the specifications of ethylene, 1-hexene and isobutane are as follows:

[0019] Ethylene: purity ≥99.20%, C2H2 content ≤5ppm, CO content ≤1ppm, O2 ≤2ppm, H2O ≤1ppm, COS ≤0.02ppm.

[0020] 1-Hexene: purity ≥98.50%, water ≤25ppm, CO content ≤5ppm, monoolefins ≥98.5%, isomerized alpha olefins ≤1%, normal non-alpha olefins ≤1%, normal alpha olefins ≥96%, peroxides ≤1ppm, sulfur ≤1ppm.

[0021] Isobutane: purity ≥95.0%, acetylene ≤2ppm, total sulfur ≤1ppm, total olefins ≤100ppm, water ≤20ppm, O2 ≤5ppm.

[0022] According to the resin composition provided by the present invention, the auxiliary agent includes a primary antioxidant, an auxiliary antioxidant and an acid absorbent.

[0023] The primary antioxidant may be a phenolic antioxidant. Examples of phenolic antioxidants suitable for use in the present invention include, but are not limited to, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0024] The auxiliary antioxidant may be a phosphite antioxidant. Examples of phosphite antioxidants suitable for use in the present invention include, but are not limited to, bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite and tris[2,4-di-tert-butylphenyl]phosphite.

[0025] Examples of acid absorbers suitable for use in the present invention include, but are not limited to, zinc stearate and calcium stearate.

[0026] According to the resin composition provided by the present invention, the resin composition comprises 100 parts by weight of hexene copolymer polyethylene resin, 0.01 to 0.2 parts by weight of a primary antioxidant, 0.01 to 0.2 parts by weight of an auxiliary antioxidant and 0.01 to 0.2 parts by weight of an acid absorber.

[0027] In some embodiments, the resin composition includes 100 parts by weight of hexene copolymer polyethylene resin, 0.05 to 0.07 parts by weight of a primary antioxidant, 0.03 to 0.05 parts by weight of an auxiliary antioxidant, and 0.03 to 0.05 parts by weight of an acid absorbent.

[0028] In the present invention, the resin composition may be in the form of particles.

[0029] According to the resin composition provided by the present invention, the low-temperature simply supported beam impact performance of the resin composition at -20°C can reach 44.5 kJ / m 2 , the modulus can reach 1280MPa.

[0030] In a second aspect, the present invention provides a method for preparing a resin composition, wherein the preparation method comprises the following steps: mixing, extruding and granulating a hexene copolymer polyethylene resin and an auxiliary agent.

[0031] According to the preparation method provided by the present invention, the hexene copolymer polyethylene resin is prepared by the following steps: ethylene and 1-hexene are reacted at a temperature of 90 to 95° C. in the presence of a diluent and a chromium catalyst.

[0032] In the present invention, C3-C6 alkanes can be used as diluents. In some embodiments, the diluent is isobutane.

[0033] In some embodiments, relative to ethylene feed amount of 25 t / h, the amount of the diluent is 23-35 kg / h, preferably 25-30 kg / h. In some embodiments, the molar ratio of ethylene to 1-hexene is 1000:5-10.

[0034] In some embodiments, the amount of the chromium catalyst is 0.05-1 wt %, preferably 0.1-0.8 wt %, more preferably 0.2-0.6 wt %, and most preferably 0.4-0.5 wt %, based on the weight of ethylene.

[0035] In the present invention, the reaction for preparing hexene copolymer polyethylene resin is carried out in a Phillips loop slurry device.

[0036] According to the preparation method provided by the present invention, a mixing extruder or a twin-screw extruder can be used for extrusion and granulation.

[0037] In a third aspect, the present invention provides application of the resin composition in hollow blow molding, especially in the field of large hollow blow molding.

[0038] Similarly, the term "large hollow blow molding" refers to a blow molding process for preparing large hollow containers with a volume of 20L or more.

[0039] In a fourth aspect, the present invention provides a hollow container, wherein the hollow container is formed of a resin composition.

[0040] In a fifth aspect, the present invention further provides a plastic pallet, wherein the plastic pallet is formed from a resin composition.

[0041] Compared with the prior art, the present invention has the following characteristics:

[0042] (1) The resin composition of the present invention has a low melt index, good low-temperature impact resistance, and high modulus, and is suitable for blowing hollow containers and plastic pallets, especially large hollow containers, and has a good rigidity-toughness balance.

[0043] (2) The present invention is to produce a high low-temperature impact-resistant and high-modulus hexene copolymer polyethylene resin by reacting ethylene and 1-hexene in the presence of a chromium-based catalyst, and further adjusting the formula, the type and amount of the catalyst, the diluent and the amount, the reaction temperature and at least one of the raw material specifications, and controlling the molecular weight and density, so as to meet the requirements of downstream processing (especially large hollow blow molding process). DETAILED DESCRIPTION

[0044] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.

[0045] Molecular weight and its distribution

[0046] Gel permeation chromatography was used, with 1,2,4-trichlorobenzene (containing 0.025 wt % antioxidant 2,6-dibutyl-p-cresol) as the solvent and mobile phase, the column temperature was 150° C., the flow rate was 1.0 ml / min, and narrow distribution polystyrene standards were used for universal calibration.

[0047] Melt Index (Melt Flow Rate)

[0048] The melt index is measured according to GB / T 3682-2000 under the following conditions: 190°C, 21.6 kg, in g / 10 min.

[0049] density

[0050] Density is measured according to GB / T 1033.2-2010, in g / cm 3 .

[0051] Tensile strength at break and tensile elongation at yield

[0052] The tensile strength at break and tensile elongation at yield were measured according to GB / T1040.2-2006, and the units are MPa and %, respectively.

[0053] Flexural modulus

[0054] The flexural modulus is measured according to GB / T9341-2008 and the unit is MPa.

[0055] Simple supported beam notched impact strength

[0056] The notched impact strength of the beam was measured according to ISO 179-1:2000 at a temperature of -20°C in kJ / m 2 .

[0057] In the following examples and comparative examples, NTR-973 chromium catalyst produced by Shanghai Nachuan Company was used and activated by fluidized bed before use.

[0058] The specifications of ethylene are as follows: purity ≥99.20%, C2H2 content ≤5ppm, CO content ≤1ppm, O2 ≤2ppm, H2O ≤1ppm, COS ≤0.02ppm.

[0059] 1-Hexene: purity ≥ 98.50%, water ≤ 25ppm, CO content ≤ 5ppm, monoolefins ≥ 98.5%, isomeric alpha olefins ≤ 1%, normal non-alpha olefins ≤ 1%, normal alpha olefins ≥ 96%, peroxides ≤ 1ppm, sulfur ≤ 1ppm;

[0060] The specifications of isobutane are as follows: purity ≥ 95.0%, acetylene ≤ 2ppm, total sulfur ≤ 1ppm, total olefins ≤ 100ppm, water ≤ 20ppm, O2 ≤ 5ppm.

[0061] Example 1

[0062] 1. Preparation of hexene copolymer polyethylene resin

[0063] The diluent isobutane is always in a circulating state. The monomer ethylene is injected into the loop reactor and an activated chromium catalyst is added for reaction. The ethylene feed rate is 25 t / h, the 1-hexene feed rate is 125 kg / h, the isobutane feed rate is 26.9 kg / h, the catalyst feed rate is 112 kg / h, and the reaction temperature is 94°C. The melt flow rate of the obtained hexene copolymer polyethylene is 2.27 g / 10 min and the density is 0.955 kg / m 3 , molecular weight distribution is 14.2, and the 1-hexene repeating unit content is shown in Table 1.

[0064] 2. Resin composition for hollow blow molding

[0065] 100 parts by weight of hexene copolymer polyethylene resin, 0.05 parts by weight of primary antioxidant 1010, 0.03 parts by weight of auxiliary antioxidant 626 and 0.03 parts by weight of zinc stearate were mixed evenly, added into a mixer to extrude particles into cooling water to obtain a granular resin composition.

[0066] When the mixer is mixing, adjust the temperature of the second section barrel of the mixer to 230°C, the temperature of the third section barrel to 235°C, the temperature of the fourth section barrel to 240°C, the temperature of the fifth section barrel to 245°C, the temperature of the sixth section barrel to 250°C, and the temperature of the seventh section barrel to 260°C; the temperature of the heat transfer oil of the heating mixer is 260°C, and the temperature of the particle cooling water is adjusted to 68°C, and the particle cooling water flow rate is 680m 3 / h.

[0067] Example 2

[0068] 1. Preparation of hexene copolymer polyethylene resin

[0069] The diluent isobutane is always in a circulating state, the monomer ethylene is injected into the loop reactor, and the activated chromium catalyst is added for reaction, wherein the ethylene feed rate is 24t / h, the 1-hexene feed rate is 168kg / h, the isobutane feed rate is 26.9kg / h, the catalyst feed rate is 115kg / h, the reaction temperature is 90°C, and the melt flow rate of the obtained hexene copolymer polyethylene resin is 2.23g / 10min and the density is 0.951kg / m 3 , molecular weight distribution is 13.9, and the 1-hexene repeating unit content is shown in Table 1.

[0070] 2. Resin composition for hollow blow molding

[0071] 100 parts by weight of hexene copolymer polyethylene resin, 0.07 parts by weight of primary antioxidant 1010, 0.05 parts by weight of auxiliary antioxidant 626 and 0.04 parts by weight of zinc stearate were mixed evenly, added into a mixer to extrude particles into cooling water to obtain a granular resin composition.

[0072] When the mixer is mixing, adjust the temperature of the second section barrel of the mixer to 230°C, the temperature of the third section barrel to 235°C, the temperature of the fourth section barrel to 240°C, the temperature of the fifth section barrel to 245°C, the temperature of the sixth section barrel to 250°C, and the temperature of the seventh section barrel to 260°C; the temperature of the heat transfer oil of the heating mixer is 260°C, and the temperature of the particle cooling water is adjusted to 68°C, and the particle cooling water flow rate is 680m 3 / h.

[0073] Example 3

[0074] 1. Preparation of hexene copolymer polyethylene resin

[0075] The diluent isobutane is always in a circulating state. The monomer ethylene is injected into the loop reactor and an activated chromium catalyst is added for reaction. The ethylene feed rate is 23 t / h, the 1-hexene feed rate is 138 kg / h, the isobutane feed rate is 26.9 kg / h, the catalyst feed rate is 115 kg / h, the reaction temperature is 92°C, and the melt flow rate of the obtained hexene copolymer polyethylene is 2.25 g / 10 min and the density is 0.953 kg / m 3 , molecular weight distribution is 15.7, and the 1-hexene repeating unit content is shown in Table 1.

[0076] 2. Resin composition for hollow blow molding

[0077] 100 parts by weight of hexene copolymer polyethylene resin, 0.06 parts by weight of primary antioxidant 1010, 0.03 parts by weight of auxiliary antioxidant 626 and 0.05 parts by weight of zinc stearate were uniformly mixed, added into a mixer to extrude particles into cooling water to obtain a granular resin composition.

[0078] When the mixer is mixing, adjust the temperature of the second section barrel of the mixer to 230°C, the temperature of the third section barrel to 235°C, the temperature of the fourth section barrel to 240°C, the temperature of the fifth section barrel to 245°C, the temperature of the sixth section barrel to 250°C, and the temperature of the seventh section barrel to 260°C; the temperature of the heat transfer oil of the heating mixer is 260°C, and the temperature of the particle cooling water is adjusted to 68°C, and the particle cooling water flow rate is 680m 3 / h.

[0079] Example 4

[0080] 1. Preparation of hexene copolymer polyethylene resin

[0081] The diluent isobutane is always in a circulating state. The monomer ethylene is injected into the loop reactor and an activated chromium catalyst is added for reaction. The ethylene feed rate is 24 t / h, the 1-hexene feed rate is 240 kg / h, the isobutane feed rate is 26.9 kg / h, the catalyst feed rate is 116 kg / h, the reaction temperature is 95°C, and the melt flow rate of the ethylene-hexene copolymer polyethylene obtained is 2.19 g / 10 min and the density is 0.954 kg / m 3 , molecular weight distribution is 16, 1-hexene repeating unit content is shown in Table 1.

[0082] 2. Resin composition for hollow blow molding

[0083] 100 weight parts of hexene copolymer polyethylene resin, 0.06 weight parts of primary antioxidant 1010, 0.04 weight parts of auxiliary antioxidant 626 and 0.05 weight parts of zinc stearate were mixed evenly, added into a mixer to extrude particles into cooling water to obtain a granular resin composition.

[0084] When the mixer is mixing, adjust the temperature of the second section barrel of the mixer to 230°C, the temperature of the third section barrel to 235°C, the temperature of the fourth section barrel to 240°C, the temperature of the fifth section barrel to 245°C, the temperature of the sixth section barrel to 250°C, and the temperature of the seventh section barrel to 260°C; the temperature of the heat transfer oil of the heating mixer is 260°C, and the temperature of the particle cooling water is adjusted to 68°C, and the particle cooling water flow rate is 680m 3 / h.

[0085] Table 1 1-hexene repeating unit content in the hexene copolymer polyethylene resin of Examples 1 to 4

[0086] Example 1 Example 2 Example 3 Example 4 1-Hexene comonomer content mol% 0.13 0.16 0.14 0.17

[0087] The melt index, density, tensile strength at break, tensile elongation at yield, flexural modulus and notched impact strength of the resin compositions of Examples 1 to 4 were measured. The results are shown in Table 2.

[0088] Table 2 Properties of the resin compositions of Examples 1 to 4

[0089]

[0090] As can be seen from Table 2, the resin composition of the present invention has a low melt index, good low-temperature impact performance, high modulus, and good rigidity-toughness balance, and meets the requirements for blowing hollow containers and plastic pallets, especially large hollow containers.

[0091] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A resin composition for hollow blow molding, characterized in that: The resin composition comprises a hexene copolymer polyethylene resin and an auxiliary agent; wherein, measured according to GB / T 3682-2000, at 190°C and 21.6kg, the melt flow rate of the hexene copolymer polyethylene resin is 2.1-2.3 g / 10 min; and the molecular weight distribution Mw / Mn of the hexene copolymer polyethylene resin is 13-17, and the density is 0.950-0.960 g / cm 3 , The content of 1-hexene repeating units in the hexene copolymer polyethylene resin is 0.1-0.2 mol%, The hexene copolymer polyethylene resin is prepared by a method comprising the following steps: in the presence of a diluent and a chromium catalyst, ethylene and 1-hexene are reacted at a temperature of 90-95° C., and the molar ratio of ethylene to 1-hexene is 1000:5-10.

2. The resin composition according to claim 1, characterized in that The content of 1-hexene repeating units in the hexene copolymer polyethylene resin is 0.13-0.18 mol%; and / or The density of the hexene copolymer polyethylene resin is 0.950-0.956 g / cm 3 .

3. The resin composition according to claim 1 or 2, characterized in that The diluent is C3-C6 alkane; and / or, relative to the ethylene feed amount of 25 t / h, the amount of the diluent is 23-35 kg / h; And / or, based on the weight of ethylene, the amount of the chromium catalyst used is 0.05 to 1 weight %.

4. The resin composition according to claim 3, characterized in that The diluent is isobutane; and / or, relative to the ethylene feed amount of 25 t / h, the amount of the diluent is 25-30 kg / h; And / or, based on the weight of ethylene, the amount of the chromium-based catalyst used is 0.1 to 0.8 weight %.

5. The resin composition according to claim 4, characterized in that The chromium catalyst is used in an amount of 0.2 to 0.6 weight % based on the weight of ethylene.

6. The resin composition according to claim 5, characterized in that The chromium catalyst is used in an amount of 0.4 to 0.5 weight % based on the weight of ethylene.

7. The resin composition according to any one of claims 1 to 2, characterized in that The auxiliary agents include a primary antioxidant, an auxiliary antioxidant and an acid absorbent.

8. The resin composition according to claim 7, characterized in that The main antioxidant is a phenolic antioxidant; And / or, the auxiliary antioxidant is a phosphite antioxidant; And / or, the acid absorber is zinc stearate and / or calcium stearate.

9. The resin composition according to claim 8, characterized in that The primary antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and / or n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; And / or, the auxiliary antioxidant is bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite and / or tris[2,4-di-tert-butylphenyl]phosphite.

10. The resin composition according to claim 7, characterized in that The resin composition comprises 100 parts by weight of hexene copolymer polyethylene resin, 0.01 to 0.2 parts by weight of a primary antioxidant, 0.01 to 0.2 parts by weight of an auxiliary antioxidant and 0.01 to 0.2 parts by weight of an acid absorbent.

11. The resin composition according to claim 10, characterized in that The resin composition comprises 100 parts by weight of hexene copolymer polyethylene resin, 0.05 to 0.07 parts by weight of a primary antioxidant, 0.03 to 0.05 parts by weight of an auxiliary antioxidant and 0.03 to 0.05 parts by weight of an acid absorbent.

12. The method for preparing a resin composition according to any one of claims 1 to 11, characterized in that: The preparation method comprises the following steps: mixing, extruding and granulating hexene copolymer polyethylene resin and auxiliary agents.

13. The preparation method according to claim 12, characterized in that: A mixing extruder or a twin-screw extruder is used for extrusion and granulation.

14. Use of the resin composition according to any one of claims 1 to 11 in the field of hollow blow molding and large hollow blow molding.

15. A hollow container, characterized in that: The hollow container is formed from the resin composition according to any one of claims 1 to 11.