Car composition
The high emission values of heterophasic propylene copolymers are addressed by combining low ethylene content heterophasic propylene copolymers produced using metallocene catalysts with recycled polypropylene-polyethylene blends, plastomers and talc in automotive interior applications. and the problem of limited performance of recycled materials, achieving a balance of low emissions and high mechanical properties.
Patent Information
- Application Number
- CN202180057074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-13
- Filing Date
- 2021-08-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-08-11
AI Technical Summary
Existing heterophasic propylene copolymers have high emission values in automotive interior applications, and recycled polyolefin materials have limited mechanical properties and odor and emissions issues, limiting their use in automotive applications.
A new composition using a low ethylene content heterophasic propylene copolymer produced with a metallocene catalyst, combined with recycled polypropylene-polyethylene blends, plastomers and talc, to reduce emission values and maintain mechanical properties .
It effectively reduces the emission value of the composition, maintains mechanical properties, especially stiffness and impact properties, and promotes the use of recycled materials, complying with the strict requirements of the automotive industry.
Smart Images

Figure CN116134087B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a novel composition suitable for automotive products, especially automotive interior products, comprising a heterophasic propylene copolymer with low ethylene content produced by a metallocene catalyst, a recycled polypropylene-polyethylene blend, a plastomer and talc. The present invention also relates to an automotive product comprising the composition. Background Art
[0002] It is well known that heterophasic propylene copolymers are used in the automotive industry mainly due to their low specific gravity and good properties. In some specific areas, such as automotive interior applications, low emissions are an important issue. The main disadvantage of the solutions currently on the market is that they have rather high emissions, which are essentially driven by the polypropylene component. Usually, heterophasic propylene copolymers are characterized by a rather high amount of oligomers, which is the main reason for higher carbon compound emission values, such as high VOC values or FOG values. These values can be reduced to a certain extent due to washing steps, but these steps complicate the production process and are not environmentally friendly. Some heterophasic propylene copolymers with quite low emission values are known, although these copolymers suffer from low melting temperature and / or low stiffness.
[0003] Accordingly, it is an object of the present invention to provide a heterophasic propylene copolymer composition suitable for reducing emission values of compositions suitable for automotive articles, especially automotive interior articles, without compromising mechanical properties, especially stiffness and impact properties.
[0004] A fundamental problem for the polymer industry is recycling. Currently, there is a somewhat limited market for recyclates, especially those from household waste, often referred to as PCR ("post-consumer resin"). Starting from household waste, the sorting and separation processes employed do not allow the production of pure polymers, i.e. there will always be some contaminants present, or these processes may even result in blends of different polymers. When it comes to polyolefins, which constitute the vast majority of the polymer fraction of collected household waste, it is almost impossible to make a perfect separation of polypropylene and polyethylene. Recycled polyolefin materials, especially post-consumer resins, are often cross-contaminated with non-polyolefin materials (such as polyethylene terephthalate, polyamide, polystyrene) or non-polymer substances (such as wood, paper, glass or aluminum). To make matters worse, these post-consumer recycled polyolefin materials are easily available on a multi-ton scale, but unfortunately, they have limited mechanical properties and often have serious odor and / or emission problems.
[0005] In addition to demanding requirements on the mechanical properties of its components, the automotive industry also has stringent requirements on odor and emissions, which are likely to become more stringent in the future. This greatly limits the use of recyclates in automotive applications.
[0006] However, there is a profound need to allow the reuse and re-use of post-consumer polyolefin recyclates in manufactured products without causing health and safety hazards.
[0007] The present invention is based on the surprising finding that complex heterophasic polypropylene copolymers can be at least partially replaced by polypropylene-polyethylene blends derived from post-consumer recycled polyolefin streams. Summary of the invention
[0008] The finding of the present invention is to provide a composition comprising a heterophasic propylene copolymer produced with a metallocene catalyst and having a low total ethylene content, a recycled polypropylene-polyethylene blend, a plastomer, talc and optionally a high density polyethylene (HDPE).
[0009] Therefore, the present invention relates to a composition comprising
[0010] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0011] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0012] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0013] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0014] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0015] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0016] in
[0017] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition;
[0018] Among them further
[0019] - A multiphase composition (HECO) comprising
[0020] (a) a propylene homopolymer as a matrix, and
[0021] (b) an ethylene-propylene rubber dispersed in the matrix,
[0022] The heterophasic propylene copolymer (HECO) has
[0023] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0024] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0025] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0026] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0027] (v) a total ethylene content measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0028] - The polypropylene-polyethylene blend (B) comprises:
[0029] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0030] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0031] Wherein the polypropylene-polyethylene blend (B) has:
[0032] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0033] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %; and one or more of the following:
[0034] iii) 0.1 ppm to 100 ppm of limonene content determined by using solid phase microextraction (HS-SPME-GC-MS);
[0035] iv) a content of one or more fatty acids determined by using solid phase microextraction (HS-SPME-GC-MS) of 0.1 to 100 ppm;
[0036] v) a content of one or more polyamides determined by NMR of 0 to 1.5% by weight;
[0037] vi) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight;
[0038] - The plastic body has a mass of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0039] Alternatively, the present invention relates to a composition comprising
[0040] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0041] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0042] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0043] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0044] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0045] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0046] in
[0047] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition;
[0048] Among them further
[0049] - A multiphase composition (HECO) comprising
[0050] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0051] (b) an ethylene-propylene rubber dispersed in the matrix,
[0052] The heterophasic propylene copolymer (HECO) has
[0053] (i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0054] (ii) the crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0055] (iii) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0056] (iv) a total ethylene content measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0057] - The polypropylene-polyethylene blend (B) comprises:
[0058] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0059] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0060] Wherein the polypropylene-polyethylene blend (B) has:
[0061] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0062] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %; and one or more of the following:
[0063] iii) 0.1 ppm to 100 ppm of limonene content determined by using solid phase microextraction (HS-SPME-GC-MS);
[0064] iv) a content of one or more fatty acids determined by using solid phase microextraction (HS-SPME-GC-MS) of 0.1 to 100 ppm;
[0065] v) a content of one or more polyamides determined by NMR of 0 to 1.5% by weight;
[0066] vi) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight;
[0067] - The plastic body has a mass of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0068] Therefore, the present invention particularly relates to a composition comprising
[0069] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0070] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0071] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0072] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0073] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0074] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0075] in
[0076] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition;
[0077] Among them further
[0078] - A multiphase composition (HECO) comprising
[0079] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0080] (b) an ethylene-propylene rubber dispersed in the matrix,
[0081] The heterophasic propylene copolymer (HECO) has
[0082] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0083] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0084] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0085] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0086] (v) a total ethylene content measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0087] - The polypropylene-polyethylene blend (B) comprises:
[0088] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0089] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0090] Wherein the polypropylene-polyethylene blend (B) has:
[0091] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0092] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %; and one or more of the following:
[0093] iii) 0.1 ppm to 100 ppm of limonene content determined by using solid phase microextraction (HS-SPME-GC-MS);
[0094] iv) a content of one or more fatty acids determined by using solid phase microextraction (HS-SPME-GC-MS) of 0.1 to 100 ppm;
[0095] v) a content of one or more polyamides determined by NMR of 0 to 1.5% by weight;
[0096] vi) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight;
[0097] - The plastic body has a mass of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0098] Further preferred embodiments of the compositions according to the invention are defined in the dependent claims.
[0099] Furthermore, the present invention relates to an automotive article, in particular to an automotive article comprising at least 95% by weight of a composition, preferably consisting of a composition, comprising
[0100] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0101] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0102] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0103] (D) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition; and
[0104] (E) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0105] in
[0106] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition;
[0107] Among them further
[0108] - A multiphase composition (HECO) comprising
[0109] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0110] (b) an ethylene-propylene rubber dispersed in the matrix,
[0111] The heterophasic propylene copolymer (HECO) has
[0112] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0113] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0114] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0115] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0116] (v) a total ethylene content measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0117] - The polypropylene-polyethylene blend (B) comprises:
[0118] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0119] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0120] Wherein the polypropylene-polyethylene blend (B) has:
[0121] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0122] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %;
[0123] - The plastic body has a mass of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0124] Hereinafter, the present invention will be described in more detail.
[0125] definition
[0126] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0127] Although any methods and materials similar or equivalent to those described herein can be used in practice to test the present invention, preferred materials and methods are described herein. In describing and claiming the present invention, the following terms will be used in accordance with the definitions set forth below. Unless otherwise expressly indicated, the use of the terms "a", "an", etc. means one or more.
[0128] For the purposes of this specification, the term "recycled waste" or "recycled material" is used to denote materials recovered from both post-consumer waste and industrial waste, rather than virgin polymers. Post-consumer waste refers to items that have completed at least a first use cycle (or life cycle), i.e., have been used for their first purpose. In contrast, industrial waste refers to manufacturing waste, or conversion waste, which does not usually reach the consumer.
[0129] The term "virgin" refers to newly produced materials and / or articles prior to first use, which have not yet been recycled. Virgin and post-consumer materials can be easily distinguished based on the presence or absence of contaminants such as limonene and / or fatty acids and / or paper and / or wood. Polypropylene-polyethylene blends can also be distinguished with respect to their origin by the presence of polystyrene and / or polyamide. Residual content means content above the detection limit.
[0130] Polymer blend refers to a mixture of two or more polymer components. Generally, the blend can be prepared by mixing two or more polymer components. Suitable mixing procedures known in the art are post-polymerization blending. Post-polymerization blending can be dry blending of polymer components (such as polymer powders and / or compounded polymer pellets) or melt blending performed by melt mixing polymer components.
[0131] Many different types of polyethylene or polypropylene can be found in "recycled material".
[0132] Propylene random copolymer is a copolymer of propylene monomer units and comonomer units, wherein the comonomer units are randomly distributed on the polypropylene chain. "Polypropylene-polyethylene blend" refers to a composition comprising both polypropylene and polyethylene, also including propylene copolymers and ethylene copolymers. Since it is impossible to directly measure each of these components, the content of polypropylene and polyethylene defined in the present invention is determined by C2 and C3 content, as measured by calibration with iPP and HDPE.
[0133] The term "plastomer" refers to a natural or synthetic polymer that possesses both elastic and plastic properties.
[0134] The term "XCS" refers to the xylene cold soluble content (XCS wt. %) measured according to ISO 16152 at 25°C.
[0135] The term "XCI" refers to the xylene cold insoluble content (XCI wt. %) determined according to ISO 16152 at 25°C.
[0136] Unless otherwise indicated, "%" means % by weight.
[0137] The heterophasic propylene copolymers with a propylene homopolymer as matrix and produced in the presence of a metallocene catalyst are characterized by a melting temperature below 160°C but above 150°C. Furthermore, the heterophasic propylene copolymers with a propylene homopolymer as matrix and produced in the presence of a metallocene catalyst contain 2,1 regio defects in the matrix phase. In contrast, the heterophasic propylene copolymers with a propylene homopolymer as matrix and produced in the presence of a Ziegler-Natta catalyst have a much higher melting temperature, i.e. above 160°C, and do not show 2,1 regio defects.
[0138] The presence of multiphase properties can be easily determined by the number of glass transition points. Reactor blends are blends produced from two or more reactors connected in series or in a reactor with two or more reaction chambers. Reactor blends can also be produced by blending in solution. Reactor blends are contrasted with compounds produced by melt extrusion. DETAILED DESCRIPTION
[0139] Composition
[0140] As mentioned above, the composition of the present invention must contain a multiphase composition (HECO), a polypropylene-polyethylene blend (B), a plastomer (P), talc (T) and optionally a high-density polyethylene (HDPE). It is particularly preferred that the composition of the present invention consists of the aforementioned components and optionally other additives. However, the composition of the present invention should preferably not contain additional polymers.
[0141] Therefore, the composition of the present invention preferably comprises
[0142] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0143] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0144] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0145] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0146] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0147] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0148] in
[0149] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90 wt.-% of the total composition, preferably at least 90.0 wt.-% of the total composition.
[0150] Therefore, it is particularly preferred that the composition of the present invention comprises
[0151] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0152] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0153] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0154] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0155] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0156] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0157] in
[0158] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90 wt%, preferably at least 95 wt% of the total composition.
[0159] Still more preferably, the composition of the present invention consists of
[0160] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0161] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0162] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0163] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0164] (E) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0165] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0166] (G) 1.0 to 5.0 wt % of additive (A), based on the total composition.
[0167] Still more preferably, the composition of the present invention consists of
[0168] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0169] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0170] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0171] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0172] (E) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0173] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0174] (G) 1.0 to 5.0 wt % of additive (A), based on the total composition.
[0175] Preferably, the composition according to the invention has a melt flow rate MFR2 (230° C., 2.16 kg), measured according to ISO 1133, in the range of 10.0 to 30.0 g / 10 min.
[0176] Therefore, it is preferred that the composition of the present invention has a melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min, and comprises
[0177] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0178] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0179] (C) 0.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0180] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0181] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0182] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0183] in
[0184] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition,
[0185] and
[0186] - Optionally, the weight ratio between the first heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably in the range of 0.3 to 6.0.
[0187] Still more preferably, the composition of the invention has a melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min and consists of
[0188] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0189] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0190] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0191] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0192] (E) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0193] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0194] (G) 1.0 to 5.0 wt. % of additive (A), based on the total composition;
[0195] Wherein optionally, the weight ratio between the heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably in the range of 0.3 to 6.0.
[0196] Still more preferably, the composition of the present invention comprises
[0197] (A) 16.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0198] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0199] (C) 0.0 to 12.0 wt %, preferably 2 to 12 wt %, of high density polyethylene (HDPE), based on the total composition;
[0200] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0201] (E) 2.0 to 12.0 wt. % of a plastomer (P), based on the total composition; and
[0202] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition;
[0203] in
[0204] The heterophasic composition (HECO), the polypropylene-polyethylene blend (B), the high density polyethylene (HDPE), the plastomer (P) and the talc (T) together constitute at least 90% by weight of the total composition,
[0205] and
[0206] - the weight ratio between the heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably in the range of 0.3 to 6.0,
[0207] The composition also has
[0208] - melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min;
[0209] - flexural modulus measured according to ISO 178 in the range of 1600 to 2400 MPa;
[0210] -4.5 to 45.0 kJ / m 2 range, preferably 5.0 to 40.0 kJ / m 2 Notched Charpy Impact Strength (NIS) measured at +23°C according to ISO 179 1eA; and
[0211] -1.8 to 8.0 kJ / m 2 range, preferably 2.0 to 7.0 kJ / m 2 The Charpy Notched Impact Strength (NIS) was measured at -20°C according to ISO 179 1eA.
[0212] Particularly preferably, the composition of the present invention consists of the following
[0213] (A) 16.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0214] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0215] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0216] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0217] (E) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0218] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0219] (G) 1.0 to 5.0 wt. % of additive (A), based on the total composition;
[0220] wherein the weight ratio between the heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably in the range of 0.3 to 6.0,
[0221] The composition also has
[0222] - melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min;
[0223] - flexural modulus measured according to ISO 178 in the range of 1600 to 2400 MPa;
[0224] -4.5 to 45.0 kJ / m 2 range, preferably 5.0 to 40 kJ / m 2 Notched Charpy Impact Strength (NIS) measured at +23°C according to ISO 179 1eA; and
[0225] -1.8 to 8.0 kJ / m 2 range, preferably 2.0 to 7.0 kJ / m 2 The Charpy Notched Impact Strength (NIS) was measured at -20°C according to ISO 179 1eA.
[0226] The composition according to the invention can be prepared by compounding the components in a suitable melt-mixing device for preparing polymer compounds, which particularly includes extruders, such as single screw extruders and co-rotating or counter-rotating twin screw extruders. Other suitable melt-mixing devices include planetary extruders and single screw co-kneaders. Especially preferred are co-rotating twin screw extruders including high intensity mixing and kneading sections. Suitable melt temperatures for preparing the composition are in the range of 170 to 300° C., preferably in the range of 200 to 260° C.
[0227] The compositions according to the present invention, in particular the compositions described in the preceding embodiments, are preferably characterized by low VOC emission values measured according to VDA278 of less than 100 μg / gram of composition, more preferably in the range of 10 to 90 μg / gram of composition, most preferably in the range of 15 to 75 μg / gram of composition.
[0228] The compositions according to the present invention, in particular the compositions described in the preceding embodiments, are further preferably characterized by low FOG emission values measured according to VDA278 of less than 320 μg / gram of composition, more preferably in the range of 25 to 300 μg / gram of composition, most preferably in the range of 30 to 280 μg / gram of composition.
[0229] Hereinafter, the components present in the composition of the present invention are described in more detail.
[0230] Heterophasic propylene copolymer (HECO)
[0231] A heterophasic propylene copolymer (HECO) is a heterophasic system as understood by a person skilled in the art. That is, a heterophasic propylene copolymer (HECO) comprises a matrix, which is a propylene homopolymer, in which the ethylene-propylene rubber is dispersed. In other words, the expression "heterophasic" means that the ethylene-propylene rubber is (finely) dispersed in the matrix. In other words, the ethylene-propylene rubber forms inclusions in the matrix. Thus, the matrix contains (finely) dispersed inclusions, which are not part of the matrix, and the inclusions are ethylene-propylene rubber. The term "inclusions" according to the present invention should preferably mean that the matrix and the inclusions form different phases in the heterophasic propylene copolymer, which inclusions are visible, for example, by high-resolution microscopy, such as electron microscopy or scanning force microscopy.
[0232] The heterophasic propylene copolymer (HECO) according to this invention has been produced by a metallocene catalyst, in particular by a metallocene catalyst as defined in more detail below. Thus, the heterophasic propylene copolymer (HECO) according to this invention has a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10 °C / min) in the range of 150 to 159 °C, preferably in the range of 153 to 158 °C, and / or a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10 °C / min) in the range of 0.05 to 0.90 %, preferably in the range of 0.25 to 0.85 %. 13 2,1 regio defects in the matrix (i.e. propylene homopolymer) determined by C-NMR.
[0233] Furthermore, the heterophasic propylene copolymer (HECO) according to this invention is characterized by a rather low ethylene content. Ethylene is the only comonomer in the heterophasic propylene copolymer (HECO). Thus, the total ethylene content of the heterophasic propylene copolymer (HECO) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis is in the range of 1.5 to 6.5 mol-%, more preferably in the range of 1.7 to 6.0 mol-%, such as in the range of 1.9 to 5.8 mol-%, wherein ethylene is the only comonomer in the heterophasic composition (HECO).
[0234] Furthermore, the heterophasic propylene copolymer (HECO) according to this invention is further characterized by a rather low amount of ethylene-propylene rubber, which is reflected by a rather low amount of soluble fraction (SF) measured by CRYSTEX analysis. That is, the heterophasic propylene copolymer (HECO) according to this invention has
[0235] (a) the crystalline fraction (CF) determined according to the CRYSTEXQC method ISO 6427 annex B is present in an amount in the range of 79.0 to 91.0 wt.-%, preferably in the range of 80.5 to 90.5 wt.-%, like in the range of 81.0 to 90.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0236] (b) soluble fraction (SF) determined according to the CRYSTEX QC method ISO 6427, appendix B, present in an amount in the range of 9.0 to 21.0 wt.-%, preferably in the range of 9.5 to 19.5 wt.-%, like in the range of 10.0 to 19.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO).
[0237] The crystalline fraction (CF) is dominated by the matrix of the heterophasic composition (HECO), i.e. the propylene homopolymer, while the soluble fraction (SF) is dominated by the rubber component of the heterophasic composition (HECO), i.e. the ethylene-propylene rubber of the heterophasic composition (HECO). Therefore, it is preferred that the heterophasic composition (HECO) comprises
[0238] (a) from 79.0 to 91.0 wt.-%, more preferably from 80.5 to 90.5 wt.-% of a propylene homopolymer, based on the total heterophasic composition (HECO); and
[0239] (b) 9.0 to 21.0 wt. %, more preferably 9.5 to 19.5 wt. %, based on the total heterophasic composition (HECO), of ethylene-propylene rubber.
[0240] Furthermore, the heterophasic composition (HECO) has a melt flow rate MFR2 (230° C., 2.16 kg), measured according to ISO 1133, in the range of 20.0 to 120 g / 10 min.
[0241] Furthermore, it is preferred that the ethylene content (C2(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis is in the range of 22.0 to 39.0 mol %, more preferably in the range of 25.0 to 35.0 mol %.
[0242] Still further, the ethylene content (C2(CF)) of the crystalline fraction of the heterogeneous composition (HECO) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis is in the range of 0.0 to 0.7 mol %, more preferably in the range of 0.0 to 0.5 mol %.
[0243] In addition, it is preferred that the matrix and the rubber, namely the crystalline fraction (CF) and the soluble fraction (SF), have specific molecular weights.
[0244] (i) the intrinsic viscosity (IV(SF)) of the soluble fraction of the heterophasic composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) is in the range of 1.80 to 3.20 dl / g, more preferably in the range of 2.00 to 3.00 dl / g, such as in the range of 2.20 to 2.80 dl / g;
[0245] (ii) the intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterophasic composition (HECO), measured according to ISO 1628-1 (in decalin at 135°C) is in the range of 0.80 to 1.80 dl / g, more preferably in the range of 1.00 to 1.60 dl / g; and
[0246] (iii) the ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the multiphase composition (HECO) [IV(SF) / IV(CF)] is in the range of 1.50 to 2.80, more preferably in the range of 1.60 to 2.70, such as in the range of 1.70 to less than 2.60.
[0247] Thus, the multiphase composition (HECO) comprises
[0248] (a) a propylene homopolymer as a matrix, and
[0249] (b) an ethylene-propylene rubber dispersed in the matrix,
[0250] The heterophasic propylene copolymer (HECO) has
[0251] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0252] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0253] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0254] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0255] (v) Total ethylene content measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol%.
[0256] In a preferred embodiment, the multiphase composition (HECO) comprises
[0257] (a) a propylene homopolymer as a matrix, and
[0258] (b) an ethylene-propylene rubber dispersed in the matrix,
[0259] The heterophasic propylene copolymer (HECO) has
[0260] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0261] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0262] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0263] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0264] (v) a total ethylene content in the range of 1.5 to 6.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0265] (vi) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %, and optionally
[0266] (vii) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol%.
[0267] In a still more preferred embodiment, the multiphase composition (HECO) comprises
[0268] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0269] (b) an ethylene-propylene rubber dispersed in the matrix,
[0270] The heterophasic propylene copolymer (HECO) has
[0271] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0272] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0273] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0274] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0275] (v) a total ethylene content in the range of 1.5 to 6.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0276] (viii) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %, and optionally
[0277] (ix) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol%.
[0278] In a still more preferred embodiment, the multiphase composition (HECO) comprises
[0279] (a) a propylene homopolymer as a matrix, and
[0280] (b) an ethylene-propylene rubber dispersed in the matrix,
[0281] The heterophasic propylene copolymer (HECO) has
[0282] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0283] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0284] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0285] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0286] (v) an intrinsic viscosity (IV(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 1.80 to 3.20 dl / g;
[0287] (vi) an intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterogeneous composition (HECO) in the range of 0.80 to 1.80 dl / g;
[0288] (vii) a ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the heterogeneous composition (HECO) [IV(SF) / IV(CF)] in the range of 1.50 to 2.80;
[0289] (viii) a total ethylene content in the range of 1.5 to 6.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0290] (ix) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %, and optionally
[0291] (x) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol%.
[0292] In a still more preferred embodiment, the multiphase composition (HECO) comprises
[0293] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0294] (b) an ethylene-propylene rubber dispersed in the matrix,
[0295] The heterophasic propylene copolymer (HECO) has
[0296] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0297] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0298] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0299] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0300] (v) an intrinsic viscosity (IV(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 1.80 to 3.20 dl / g;
[0301] (vi) an intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 0.80 to 1.80 dl / g;
[0302] (vii) a ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the heterogeneous composition (HECO) [IV(SF) / IV(CF)] in the range of 1.50 to 2.80;
[0303] (viii) a total ethylene content in the range of 1.5 to 6.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0304] (ix) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %, and optionally
[0305] (x) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol%.
[0306] In a specific embodiment, the multiphase composition (HECO) comprises
[0307] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0308] (b) an ethylene-propylene rubber dispersed in the matrix,
[0309] The heterophasic propylene copolymer (HECO) has
[0310] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 150 to 159°C;
[0311] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0312] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0313] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0314] (v) an intrinsic viscosity (IV(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 1.80 to 3.20 dl / g;
[0315] (vi) an intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 0.80 to 1.80 dl / g;
[0316] (vii) a ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the heterogeneous composition (HECO) [IV(SF) / IV(CF)] in the range of 1.50 to 2.80;
[0317] (viii) a total ethylene content in the range of 1.5 to 6.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0318] (ix) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %, and optionally
[0319] (x) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol%.
[0320] In a very specific embodiment, the multiphase composition (HECO) comprises
[0321] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0322] (b) an ethylene-propylene rubber dispersed in the matrix,
[0323] The heterophasic propylene copolymer (HECO) has
[0324] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 153 to 158°C;
[0325] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0326] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 80.5 to 90.5 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0327] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.5 to 19.5 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0328] (v) an intrinsic viscosity (IV(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 2.30 to 2.80 dl / g;
[0329] (vi) an intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 1.00 to 1.40 dl / g;
[0330] (vii) a ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the heterogeneous composition (HECO) [IV(SF) / IV(CF)] in the range of 1.65 to 2.65;
[0331] (viii) a total ethylene content in the range of 1.7 to 4.5 mol % as measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis;
[0332] (ix) an ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 25.0 to 35.0 mol %, and optionally
[0333] (x) Ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.5 mol%.
[0334] In the following, the polymerization of the heterophasic composition (HECO) is described in detail.
[0335] The multiphase composition (HECO) according to the present invention can be produced in a cascade of two or more reactors, preferably three reactors. Polymerization processes suitable for producing the multiphase composition (HECO) according to the present invention are known in the prior art. They comprise at least two polymerization stages, wherein the polymerization is generally carried out in solution, slurry, bulk or gas phase. Typically, the polymerization process comprises additional polymerization stages or reactors. In a particularly preferred embodiment, the polymerization process comprises at least one bulk reactor and optionally at least two gas phase reactors arranged in the following order. The process may also comprise a pre-reactor and a post-reactor. The pre-reactor generally comprises a pre-polymerization reactor. In this process, preferably a higher polymerization temperature is used to obtain specific polymer properties. Typical temperatures in these processes are 65° C. or higher, preferably 75° C. or higher. The higher polymerization temperatures as described above can be applied to some or all reactors of the cascade reactor, preferably to the first gas phase reactor.
[0336] A preferred multi-stage process is a "loop-gas phase" process such as that developed by Borealis (known as Another suitable slurry-gas phase process is the slurry-gas phase process of Basell. method.
[0337] As mentioned above, the heterophasic composition (HECO) according to the invention is obtained in particular in a polymerization process using a metallocene catalyst having formula (I)
[0338]
[0339] Each R 1 are independently the same or different and are hydrogen or a linear or branched C1-C6 alkyl group, wherein each phenyl group has at least one R 1 Not hydrogen,
[0340] R′ is C1-C 10 A hydrocarbon group, preferably a C1-C4 hydrocarbon group, and more preferably a methyl group, and
[0341] X is independently a hydrogen atom, a halogen atom, a C1-C6 alkoxy group, a C1-C6 alkyl group, a phenyl group or a benzyl group.
[0342] Most preferably, X is chlorine, benzyl or methyl. Preferably, the two X groups are identical. The most preferred options are two chlorides, two methyls or two benzyls, especially two chlorides.
[0343] Particularly preferred metallocene catalysts of the present invention include:
[0344] Racemic-trans-dimethylsilylene[2-methyl-4,8-bis-(4′-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride
[0345] Racemic-trans-dimethylsilanediylsilylene[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride
[0346] Racemic-trans-dimethylsilylene[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-di-tert-butyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride
[0347] or their corresponding dimethyl zirconium analogs.
[0348] The most preferred catalyst is rac-trans-dimethylsilylene[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacene-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride
[0349]
[0350] The ligands required for forming the complex of the present invention and thus forming the catalyst of the present invention can be synthesized by any method, and a skilled organic chemist can design various synthesis schemes for making necessary ligand materials. For example, WO2007 / 116034 discloses necessary chemistry. Synthesis schemes can also be generally found in WO 2002 / 02576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790 and WO 2018 / 122134. With particular reference to WO 2019 / 179959, the most preferred catalyst of the present invention is described. The examples section also provides sufficient guidance for those skilled in the art.
[0351] Catalyst
[0352] In order to form an active catalytic species, it is usually necessary to use a promoter as is known in the art.
[0353] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with the metallocene catalyst complex defined above.
[0354] The aluminoxane cocatalyst may be a catalyst of formula (III):
[0355]
[0356] wherein n is generally 6 to 20 and R has the following meanings.
[0357] Aluminoxanes are formed upon partial hydrolysis of organoaluminum compounds, such as those having the formula AlR3, AlR2Y, and Al2R3Y3, wherein R can be, for example, C1-C 10 Alkyl, preferably C1-C5 alkyl, or C 3-10 Cycloalkyl, C7-C 12 Aralkyl or alkaryl and / or phenyl or naphthyl, and wherein Y can be hydrogen, halogen, preferably chlorine or bromine, or C1-C 10 The alkoxy group is preferably a methoxy group or an ethoxy group. The oxygen-containing aluminoxane obtained is usually not a pure compound but a mixture of oligomers of the formula (III).
[0358] The preferred aluminoxane is methylaluminoxane (MAO).Since the aluminoxanes used as cocatalysts according to the invention are not pure compounds due to the way they are prepared, the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.
[0359] According to the present invention, a boron-containing cocatalyst may also be used instead of the aluminoxane cocatalyst, or the aluminoxane cocatalyst may be used in combination with the boron-containing cocatalyst.
[0360] Those skilled in the art will appreciate that where a boron-based cocatalyst is used, the complex is typically pre-alkylated by reacting the complex with an alkylaluminum compound such as TIBA. This procedure is well known and any suitable alkylaluminum may be used, for example Al(C1-C6 alkyl)3. Preferred alkylaluminum compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum and triisooctylaluminum.
[0361] Alternatively, when a borate cocatalyst is used, the metallocene catalyst complex is in its alkylated form, ie, for example, a dimethyl or dibenzyl metallocene catalyst complex may be used.
[0362] Boron-based cocatalysts of interest include those of formula (IV)
[0363] BY3(IV)
[0364] Wherein Y is the same or different and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkaryl group, an aralkyl group, a halogenated alkyl group or a halogenated aryl group each having 1 to 10 carbon atoms in the alkyl group and 6 to 20 carbon atoms in the aryl group, or an alkaryl group, an aralkyl group, a halogenated alkyl group or a halogenated aryl group each having fluorine, chlorine, bromine or iodine. Preferred embodiments of Y are methyl, propyl, isopropyl, isobutyl or trifluoromethyl, unsaturated groups such as aryl or halogenated aryl groups, such as phenyl, tolyl, benzyl, p-fluorophenyl, 3,5-difluorophenyl, pentachlorophenyl, pentafluorophenyl, 3,4,5-trifluorophenyl and 3,5-bis(trifluoromethyl)phenyl. Preferred options are trifluoroborane, triphenylborane, tri(4-fluorophenyl)borane, tri(3,5-difluorophenyl)borane, tri(4-fluoromethylphenyl)borane, tri(2,4,6-trifluorophenyl)borane, tri(pentafluorophenyl)borane, tri(tolyl)borane, tri(3,5-dimethyl-phenyl)borane, tri(3,5-difluorophenyl)borane and / or tri(3,4,5-trifluorophenyl)borane.
[0365] Tris(pentafluorophenyl)borane is particularly preferred.
[0366] However, preference is given to using borates, i.e. compounds containing borate 3+ ions. Such ionic promoters preferably contain non-coordinating anions, such as tetrakis(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amines or aniline derivatives, such as methylammonium, anilinium, dimethylammonium, diethylammonium, N-methylanilinium, diphenylammonium, N,N-dimethylanilinium, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridinium, p-bromo-N,N-dimethylanilinium or p-nitro-N,N-dimethylanilinium.
[0367] Preferred ionic compounds that can be used according to the present invention include:
[0368] Triethylammonium tetra(phenyl)borate,
[0369] Tributylammonium tetra(phenyl)borate,
[0370] Trimethylammonium tetra(tolyl)borate,
[0371] Tributylammonium tetra(tolyl)borate,
[0372] Tributylammonium tetrakis(pentafluorophenyl)borate,
[0373] Tripropylammonium tetrakis(dimethylphenyl)borate,
[0374] Tributylammonium tetrakis(trifluoromethylphenyl)borate,
[0375] Tributylammonium tetrakis(4-fluorophenyl)borate,
[0376] N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate,
[0377] N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate,
[0378] N,N-dimethylanilinium tetra(phenyl)borate,
[0379] N,N-diethylanilinium tetra(phenyl)borate,
[0380] N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate,
[0381] N,N-di(propyl)ammonium tetrakis(pentafluorophenyl)borate,
[0382] Di(cyclohexyl)ammonium tetrakis(pentafluorophenyl)borate,
[0383] Triphenylphosphonium tetra(phenyl)borate,
[0384] Triethylphosphonium tetra(phenyl)borate,
[0385] Diphenylphosphonium tetra(phenyl)borate,
[0386] tri(methylphenyl)phosphonium tetra(phenyl)borate,
[0387] tri(dimethylphenyl)phosphonium tetra(phenyl)borate,
[0388] Triphenylcarbeniumtetrakis(pentafluorophenyl)borate
[0389] Or ferroceniumtetrakis(pentafluorophenyl)borate.
[0390] Preferred are triphenylcarbonium tetrakis(pentafluorophenyl)borate,
[0391] N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate or
[0392] N,N-Dimethylbenzylammonium tetrakis(pentafluorophenyl)borate.
[0393] Surprisingly, it has been found that certain boron promoters are particularly preferred. Thus, preferred borates for use in the present invention include trityl ions. Thus, it is particularly preferred to use N,N-dimethylammonium-tetrapentafluorophenyl borate and Ph3CB(PhF5)4 and the like.
[0394] According to the present invention, preferred cocatalysts are aluminoxanes, more preferably methylaluminoxane, combinations of aluminoxanes with alkylaluminum, boron or borate cocatalysts, and combinations of aluminoxanes with boron-based cocatalysts.
[0395] Suitable amounts of promoter are well known to those skilled in the art.
[0396] The molar ratio of boron to the metal ion of the metallocene may be in the range of 0.5:1 to 10:1 mol / mol, preferably in the range of 1:1 to 10:1, especially in the range of 1:1 to 5:1 mol / mol.
[0397] The molar ratio of Al in the aluminoxane to the metal ion of the metallocene may be in the range of 1:1 to 2000:1 mol / mol, preferably in the range of 10:1 to 1000:1, and more preferably in the range of 50:1 to 500:1 mol / mol.
[0398] The catalyst can be used in supported or unsupported form, preferably in supported form. The particulate support material used is preferably an organic or inorganic material, such as silicon dioxide, aluminum oxide or zirconium oxide or a mixed oxide, such as silicon dioxide-alumina, in particular silicon dioxide, aluminum oxide or silicon dioxide-alumina. Preferably, a silicon dioxide support is used. The person skilled in the art knows the procedures required for supporting the metallocene catalyst.
[0399] It is particularly preferred that the support is a porous material so that the complex can be loaded into the pores of the support, for example using methods similar to those described in WO94 / 14856 (Mobil), WO95 / 12622 (Borealis) and WO2006 / 097497.
[0400] The average particle size of the silica support can generally be in the range from 10 to 100 μm. However, it has been shown that particular advantages can be achieved if the support has an average particle size of from 15 to 80 μm, preferably from 18 to 50 μm.
[0401] The average pore size of the silica support may be in the range of 10 to 100 nm, and the pore volume is 1 to 3 mL / g.
[0402] Examples of suitable support materials are silicas such as ES757 produced and sold by PQ, Sylopol 948 produced and sold by Grace or SUNSPERA DM-L-303 produced by AGC Si-Tech. Before use in the catalyst preparation, the support can optionally be calcined to achieve an optimum silanol group content.
[0403] The use of these vectors is routine in the art.
[0404] Polypropylene-polyethylene blend (B)
[0405] The polypropylene-polyethylene blend (B) according to the present invention comprises
[0406] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0407] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0408] At the same time, polypropylene-polyethylene blends (B) have
[0409] - a melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min, preferably 7.0 to 50 g / 10 min, more preferably 9.0 to 30 g / 10 min; and
[0410] - a residual ash content in the range of 0.1 to 3.0 wt.-%, preferably 0.5 to 2.7 wt.-%, more preferably 0.7 to 2.5 wt.-%.
[0411] The polypropylene-polyethylene blend (B) according to the present invention is preferably a recycled material. It is particularly preferred that the polypropylene-polyethylene blend (B) according to the present invention is derived in an amount of at least 90 wt.-% from post-consumer waste and / or post-industrial waste, more preferably from post-consumer waste.
[0412] The polypropylene-polyethylene blend (B) according to the present invention may have one or more of the following properties:
[0413] a) 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm of limonene content determined by using solid phase microextraction (HS-SPME-GC-MS);
[0414] b) a content of one or more fatty acids determined by using solid phase microextraction (HS-SPME-GC-MS) of 0.1 to 100 ppm;
[0415] c) a content of one or more polyamides determined by NMR of 0 to 1.5% by weight;
[0416] d) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight;
[0417] e) Residual ash content as described above.
[0418] It should be understood that the composition of the polypropylene-polyethylene blend (B) may vary widely, i.e. may include propylene homopolymers, propylene copolymers, ethylene homopolymers and ethylene copolymers. Since it is not possible to directly determine each of these components, the content of polypropylene and polyethylene defined in the present invention is determined by the C2 and C3 content, as determined by calibration with iPP and HDPE.
[0419] Generally, the polypropylene-polyethylene blend (B) according to the present invention may also have one or more of the following properties:
[0420] - the residual content of PET determined as described in the experimental part;
[0421] - residual talc and chalk content as described in the experimental part;
[0422] - Residual content of metals (determined by x-ray fluorescence (XRF));
[0423] - the remaining amount of paper as described in the experimental part;
[0424] - Remaining amount of wood as described in the experimental section.
[0425] The polypropylene-polyethylene blend (B) according to the present invention is preferably obtained from washing and / or aeration steps known in the art.
[0426] Plastic body
[0427] The composition according to the invention further comprises a plastomer having a density of 850 to 900 kg / m 3 In the range of 860 to 890 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0428] Preferably, the plastomer has a melt flow rate MFR2 (190° C., 2.16 kg) measured according to ISO 1133 in the range of 1.5 to 15.0 g / 10 min, preferably in the range of 2.0 to 10.0 g / 10 min.
[0429] It is particularly preferred that the plastomer has a density of 850 to 900 kg / m 3 Ethylene 1-octene copolymers having a density measured according to ISO 1183-1 in the range of 0.1 % to 0.2 % and a melt flow rate MFR2 (190° C., 2.16 kg) measured according to ISO 1133 in the range of 1.5 to 15.0 g / 10 min.
[0430] According to one embodiment, the plastomer is an ethylene 1-octene copolymer having a molecular weight of 860 to 890 kg / m3 The density measured according to ISO 1183-1 is in the range of 2.0 to 10.0 g / 10 min and the melt flow rate MFR2 (190° C., 2.16 kg) measured according to ISO 1133 is in the range of 2.0 to 10.0 g / 10 min.
[0431] In a preferred embodiment, the plastomer is prepared with at least one metallocene catalyst. The plastomer may also be prepared with more than one metallocene catalyst, or may be a blend of multiple elastomers prepared with different metallocene catalysts. In some embodiments, the plastomer is a substantially linear ethylene polymer (SLEP). SLEP and other metallocene-catalyzed plastomers are known in the art, e.g., US 5,272,236. These resins are also commercially available, e.g., Queo ® available from Borealis AG (Austria). TM Plastomers, ENGAGE available from The Dow Chemical Company (USA) TM Plastomer resin, or EXACT available from ExxonMobil (USA) TM polymer, or TAFMER available from Mitsui (Japan) TM polymer.
[0432] High-density polyethylene (HDPE)
[0433] According to a preferred embodiment of the present invention, the composition further comprises high density polyethylene (HDPE).
[0434] High density polyethylene (HDPE) preferably has a density of 940 to 970 kg / m 3 Density measured according to ISO 1183-1 within the range.
[0435] In addition, it is preferred that the high density polyethylene (HDPE) has a rather low melt flow rate. Therefore, the melt flow rate MFR2 (190°C, 2.16 kg) of the high density polyethylene (HDPE) measured according to ISO 1133 is preferably in the range of 1.0 to 30.0 g / 10 min, more preferably in the range of 2.0 to 20.0 g / 10 min.
[0436] Preferably, the high density polyethylene (HDPE) according to the present invention is a high density polyethylene known in the art. In particular, it is preferred that the high density polyethylene (HDPE) is the commercial ethylene homopolymer "HE9621-PH" of Borealis AG.
[0437] talc
[0438] Another essential component of the present invention is talc (T). It is preferred that the talc (T) has a median particle size (d ) in the range of 0.3 to 3.0 μm measured according to ISO 13317-3. 50 ) and a top cut particle size (d 95 ).
[0439] According to one embodiment, talc (T) has a median particle size (d ) in the range of 0.5 to 2.5 μm, measured according to ISO 13317-3. 50 ) and a top cut particle size (d 95 ).
[0440] According to the present invention, talc (T) does not belong to the category of alpha nucleating agents and additives (A).
[0441] Talc (T) is a prior art and commercially available product.
[0442] Additive (A)
[0443] The composition of the present invention may further comprise additives (A). Typical additives are acid scavengers, nucleating agents, antioxidants, colorants, light stabilizers, slip agents, anti-scratch agents, dispersants, processing aids, lubricants, pigments, carbon black masterbatch, and the like.
[0444] These additives are commercially available and are described, for example, in "Plastic Additives Handbook" by Hans Zweifel, 6th edition, 2009 (pp. 1141 to 1190).
[0445] Additives are usually provided in the form of masterbatches. A masterbatch is a composition in which an additive or a mixture of additives is dispersed in a polymer in a relatively high amount. Therefore, the term "additive" according to the present invention also includes a carrier material, in particular a polymer carrier material, in which the "active additive" or the "active additive mixture" is dispersed.
[0446] Automobile products
[0447] The present invention further relates to an automotive article comprising at least 90% by weight, preferably at least 95% by weight, of a composition according to the invention. The present invention particularly relates to an automotive interior article comprising at least 90% by weight, preferably at least 95% by weight, of a composition according to the invention. Still more preferably, the present invention relates to an automotive interior article consisting of a composition according to the invention. Examples of such automotive interior articles are instrument panels, center consoles, door claddings and pillar trims.
[0448] Particularly preferred embodiments
[0449] The present invention particularly relates to a composition having a melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min and consisting of
[0450] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0451] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0452] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0453] (D) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0454] (E) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0455] (F) 1.0 to 5.0 wt. % of additive (A), based on the total composition;
[0456] wherein the weight ratio between the heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably 0.3 to 6.0;
[0457] Among them further
[0458] - A multiphase composition (HECO) comprising
[0459] (a) a propylene homopolymer as a matrix, and
[0460] (b) an ethylene-propylene rubber dispersed in the matrix,
[0461] The heterophasic propylene copolymer (HECO) has
[0462] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 153 to 158°C;
[0463] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0464] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0465] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 annex B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO); and
[0466] (v) a total ethylene content measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0467] - The polypropylene-polyethylene blend (B) comprises:
[0468] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0469] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0470] Wherein the polypropylene-polyethylene blend (B) has:
[0471] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0472] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %,
[0473] - The plastic body has a mass of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:1.
[0474] The present invention particularly relates to a composition having a melt flow rate MFR2 (230° C., 2.16 kg) measured according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min and consisting of
[0475] (A) 18.0 to 60.0 wt. % of a heterogeneous composition (HECO), based on the total composition;
[0476] (B) 7.0 to 55.0 wt. % of a polypropylene-polyethylene blend (B), based on the total composition;
[0477] (C) 2.0 to 12.0 wt % of high density polyethylene (HDPE), based on the total composition;
[0478] (D) 5.0 to 15.0 wt. % of polyethylene, based on the total composition, which is the sum of the high density polyethylene (HDPE) and the polyethylene contained in the polypropylene-polyethylene blend (B);
[0479] (E) 2.0 to 12.0 wt. % of plastomer (P), based on the total composition;
[0480] (F) 7.0 to 25.0 wt. % of talc (T), based on the total composition; and
[0481] (G) 1.0 to 5.0 wt. % of additive (A), based on the total composition;
[0482] wherein the weight ratio between the heterophasic composition (HECO) and the polypropylene-polyethylene blend (B) [(HECO) / (B)] is in the range of 0.2 to 8.0, preferably 0.3 to 6.0;
[0483] Among them further
[0484] - A multiphase composition (HECO) comprising
[0485] (a) a propylene homopolymer as a matrix, wherein the propylene homopolymer has a content of 0.05 to 0.90% by weight 13 2,1 regio defects determined by C-NMR, and
[0486] (b) an ethylene-propylene rubber dispersed in the matrix,
[0487] The heterophasic propylene copolymer (HECO) has
[0488] (i) a melting temperature Tm measured by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min) in the range of 153 to 158°C;
[0489] (ii) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 20.0 to 120 g / 10 min;
[0490] (iii) crystalline fraction (CF) determined according to the CRYSTEX QC method ISO 6427 appendix B present in an amount in the range of 79.0 to 91.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0491] (iv) the soluble fraction (SF) determined according to CRYSTEX QC method ISO 6427 appendix B is present in an amount in the range of 9.0 to 21.0 wt.-% relative to the total weight of the heterophasic propylene copolymer (HECO);
[0492] (v) an intrinsic viscosity (IV(SF)) of the soluble fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 2.00 to 3.00 dl / g;
[0493] (vi) an intrinsic viscosity (IV(CF)) of the crystalline fraction of the heterogeneous composition (HECO) measured according to ISO 1628-1 (in decalin at 135°C) in the range of 1.00 to 1.50 dl / g;
[0494] (vii) a ratio between the intrinsic viscosity of the soluble fraction (SF) and the intrinsic viscosity of the crystalline fraction (CF) of the heterogeneous composition (HECO) [IV(SF) / IV(CF)] in the range of 1.50 to 2.80;
[0495] (viii) ethylene content of the soluble fraction (C2(SF)) measured by Fourier transform infrared spectroscopy (FITR) during CRYSTEX analysis in the range of 22.0 to 39.0 mol %;
[0496] (ix) an ethylene content of the crystalline fraction (C2(CF)) measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 0.0 to 0.7 mol %, and
[0497] (x) a total ethylene content measured by Fourier transform infrared spectroscopy (FTIR) during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition (HECO);
[0498] - The polypropylene-polyethylene blend (B) comprises:
[0499] B-1) at least 85.0 wt. % of polypropylene relative to the total weight of the polypropylene-polyethylene blend (B),
[0500] B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of the polypropylene-polyethylene blend (B),
[0501] Wherein the polypropylene-polyethylene blend (B) has:
[0502] i) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 75 g / 10 min; and
[0503] ii) a residual ash content measured by thermogravimetric analysis in the range of 0.1 to 3.0 wt. %; and one or more of the following:
[0504] iii) 0.1 ppm to 100 ppm of limonene content determined by using solid phase microextraction (HS-SPME-GC-MS);
[0505] iv) a content of one or more fatty acids determined by using solid phase microextraction (HS-SPME-GC-MS) of 0.1 to 100 ppm;
[0506] v) a content of one or more polyamides determined by NMR of 0 to 1.5% by weight;
[0507] vi) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight;
[0508] - The plastic body has a mass of 850 to 900 kg / m 3 ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 in the range of 1.5 to 15.0 g / 10 min and a melt flow rate MFR2 (190° C., 2.16 kg) measured according to ISO 1133 in the range of 1.5 to 15.0 g / 10 min;
[0509] - Polyethylene (HDPE) has a density of 940 to 970 kg / m 3 a density measured according to ISO 1183-1 in the range of 1.0 to 30.0 g / 10 min and a melt flow rate MFR2 (190° C., 2.16 kg) measured according to ISO 1133 in the range of 1.0 to 30.0 g / 10 min;
[0510] - talc (T) having a median particle size d in the range of 0.3 to 3.0 μm, measured according to ISO 13317-3 50 and a top cut particle size d measured according to ISO 13317-3 in the range of 0.5 to 10.0 μm 95 ;
[0511] Hereinafter, the present invention will be described by way of examples.
[0512] Example
[0513] Melt flow rate
[0514] The melt flow rate (MFR2) is determined according to ISO 1133 and is expressed in g / 10 min. The MFR2 of the heterophasic propylene copolymers is determined at a temperature of 230°C and under a load of 2.16 kg, whereas the MFR2 of the plastomers and the MFR2 of the HDPE are determined at a temperature of 190°C and under a load of 2.16 kg.
[0515] Melting temperature T m and crystallization temperature T c
[0516] Melting temperature T m Determined by differential scanning calorimetry (DSC) according to ISO 11357-3 using a TA-Instrument 2920 Dual-Cell with RSC refrigeration unit and data station. A heating and cooling rate of 10°C / min was used in a heating / cooling / heating cycle between +23°C and +210°C. Crystallization temperature (T c ) is determined by the cooling step, while the melting temperature (T m ) and melting enthalpy (H m ) is determined in the second heating step.
[0517] Crystex analysis
[0518] Crystallization and soluble fraction method
[0519] The crystalline fraction (CF) and the soluble fraction (SF) of the heterophasic propylene copolymer, the final comonomer content of the heterophasic propylene copolymer, the comonomer content of each fraction and the intrinsic viscosity of each fraction were analyzed by CRYSTEX QC, Polymer Char (Valencia, Spain) based on ISO 6427 Annex B: 1992 (E). Figure 1 A schematic diagram of the CRYSTEX QC instrument is shown in a. Figure 1 As shown in (b), the crystalline and amorphous parts were separated by temperature cycling of dissolution in 1,2,4-trichlorobenzene (1,2,4-TCB) at 160°C, crystallization at 40°C, and redissolution in 1,2,4-TCB at 160°C. Quantification of SF and CF as well as determination of ethylene content (C2) were achieved by an infrared detector (IR4), and intrinsic viscosity (iV) was determined using an online 2-capillary viscometer. The IR4 detector is a detector that detects the CH3 stretching vibration (centered at about 2960 cm -1 ) and CH x Extension vibration (2700 to 3000cm -1) at two different wavelengths, the IR absorbance at these two different bands can be used to determine the concentration and ethylene content in ethylene-propylene copolymers (EP copolymers). The IR4 detector is calibrated with a series of 8 EP copolymers with known ethylene contents ranging from 2 wt% to 69 wt% (measured by 13 C-NMR measurement), and each ethylene-propylene copolymer has multiple concentrations in the range of 2 and 13 mg / ml. For the various polymer concentrations expected during Crystex analysis, in order to simultaneously account for two characteristics, i.e., concentration and ethylene content, the following calibration equation was applied:
[0520] Equation 1:
[0521] Concentration = a + b * absorbance (CH x )+c*(absorbance(CH x ))2+d*Absorbance(CH3)+e*(Absorbance(CH3))2+f*
[0522] Absorbance (CH x )*Absorbance(CH3)
[0523] Equation 2:
[0524] CH3 / 1000C=a+b*absorbance(CH x )+c*absorbance(CH3)+d*(absorbance(CH3) / absorbance(CH x ))+
[0525] e*(absorbance(CH3) / absorbance(CH x ))2
[0526] Constants a to e for Equation 1 and constants a to f for Equation 2 are determined by using least squares regression analysis.
[0527] Equation 3:
[0528] The CH3 / 1000C is converted to ethylene content in weight % using the following relationship:
[0529] Weight % (ethylene in EP copolymer) = 100 - CH3 / 1000TC*0.3
[0530] The amounts of the soluble fraction (SF) and the crystalline fraction (CF) are related by means of the XS calibration to the "xylene cold soluble" (XCS) fraction and the "xylene cold insoluble" (XCI) fraction, respectively, determined according to the standard gravimetric method according to ISO 16152. The XS calibration is achieved by testing various EP copolymers having a xylene cold soluble (XCS) content in the range of 2 to 31 wt%. The determined XS calibration is linear (Equation 4):
[0531] Weight%XCS=1.01*weight%SF
[0532] The intrinsic viscosity (IV) of the parent heterophasic propylene copolymer and its soluble fraction (SF) and crystalline fraction (CF) was determined using an online 2-capillary viscometer and related to the corresponding IV determined by the standard method in decalin according to ISO 1628-3. Calibration was achieved using various EP copolymers with IV = 2 to 4 dl / g. The calibration curve determined between Vsp and IV measured in CRYSTEX QC and normalized by concentration (c) was linear (Equation 5):
[0533] IV(dl / g)=a*Vsp / c
[0534] The slope a=16.2. The heterophasic propylene copolymer sample to be analyzed was weighed out at a concentration of 10 mg / ml to 20 mg / ml. After automatically filling the vial with 1,2,4-TCB containing 250 mg / l of 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the sample was dissolved at 160°C until completely dissolved, usually for 60 min, with continuous stirring at 400 rpm. In order to avoid sample degradation, the polymer solution was blanketed with a N2 atmosphere during the dissolution process.
[0535] like Figure 1 As shown in a and b, a limited volume of sample solution is injected into a column filled with an inert carrier, where crystallization of the sample and separation of the soluble fraction and the crystalline fraction are carried out. This process is repeated twice. During the first injection, the entire sample is measured at high temperature to determine the IV [dl / g] and C2 [wt%] of the heterophasic propylene copolymer. During the second injection, the soluble fraction (SF) (at low temperature, 40 ° C) and the crystalline fraction (CF) (at high temperature, 160 ° C) (wt% SF, wt% C2 of SF, IV of SF) are measured using the crystallization cycle.
[0536] based on 13 C NMR spectroscopy for determination of C2 content of calibration standards
[0537] Use for 1 H and 13Quantitative measurements were recorded in solution on a Bruker Avance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz, respectively. 13 C{ 1 H} NMR spectroscopy. Nitrogen was used for all pneumatic devices, using 13 All spectra were recorded at 125°C with a C optimized 10 mm extended temperature probe. Approximately 200 mg of material was dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) along with chromium (III) acetylacetonate (Cr(acac)3) to give a 65 mM solution of the relaxant in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475). To ensure a homogeneous solution, the NMR tube was further heated in a rotary oven for at least 1 hour after the initial sample preparation in the heating block. After insertion into the magnet, the tube was rotated at 10 Hz. This setup was chosen primarily to obtain high resolution and is quantitatively required for accurate quantification of ethylene content. Standard single pulse excitation without NOE was used, with an optimized tip angle, a 1 s recycle delay, and a two-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225, Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transient values were obtained for each spectrum. For quantitative 13 C{ 1 The H} NMR spectra are processed, integrated and the relevant quantitative properties are determined from the integrals. All chemical shifts are indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This method allows for comparable references even if this structural unit is not present.
[0538] Characteristic signals corresponding to ethylene incorporation were observed (Cheng, HN, Macromolecules 17 (1984), 1950) and the comonomer fraction was calculated as the fraction of ethylene in the polymer relative to all monomers in the polymer:
[0539] fE=(E / (P+E))
[0540] The method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) was used to 13 C{ 1 The comonomer fraction was quantified by integrating multiple signals over the entire spectral region of the {H} spectrum. This method was chosen due to its robustness and ability to account for the presence of regio defects when required. The integration region was slightly adjusted to improve applicability over the entire range of comonomer contents encountered. For systems with very low ethylene content, where only isolated ethylene in the PPEPP sequence was observed, the method of Wang et al. was modified to reduce the impact of the integration of sites that were no longer present. This approach reduces the overestimation of the ethylene content for such systems and is achieved by reducing the number of sites used to determine the absolute ethylene content to less than
[0541] E=0.5(Sββ+Sβγ+Sβδ+0.5(Sαβ+Sαγ))
[0542] Using this set of sites, the corresponding integral equation becomes:
[0543] E=0.5(I H +I G +0.5(I C +I D ))
[0544] The same symbols as used in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) are used. No modifications are made to the equation for absolute propylene content. The mole percentage of comonomer incorporation is calculated from the mole fraction:
[0545] E[mol%]=100*fE
[0546] Calculate the weight percent of comonomer incorporation from the mole fraction:
[0547] E[weight%]=100*(fE*28.06) / ((fE*28.06)+((1-fE)*42.08))
[0548] Quantification of microstructure by NMR spectroscopy
[0549] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the isotacticity and regio-regularity of the matrix component of the heterophasic copolymer (HECO) on samples taken after the first gas phase reactor (GPR1).
[0550] Use for 1 H and 13Quantitative measurements were recorded in solution on a Bruker Advance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz, respectively. 13 C{ 1 H} NMR spectra. All spectra were obtained using 13 The C-optimized 10 mm extended temperature probe was recorded at 125 °C, using nitrogen for all pneumatics.
[0551] For propylene homopolymers, about 200 mg of material was dissolved in 1,2-tetrachloroethane-d2 (TCE-d2). To ensure the homogeneity of the solution, the NMR tube was further heated in a rotary oven for at least 1 hour after the initial sample preparation in the heating block. After insertion into the magnet, the tube was rotated at 10 Hz. This setting was chosen mainly for the high resolution required for quantification of stereoregularity distribution (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V.; Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251). Standard single pulse excitation was used, with NOE and a two-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 11289). A total of 8192 (8k) transient values were acquired for each spectrum.
[0552] A proprietary computer program was used to quantify 13 C{ 1 H} NMR spectra are processed, integrated and relevant quantitative properties determined from the integrals.
[0553] For propylene homopolymers, all chemical shifts are internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.
[0554] Characteristic signals corresponding to regional defects (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253; Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157; Cheng, HN, Macromolecules 17 (1984), 1950) or comonomers were observed.
[0555] The stereoregularity distribution is quantified by integration over the methyl region between 23.6-19.7 ppm, correcting for any sites not related to the stereo sequence of interest (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V., Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251).
[0556] Specifically, the quantitative effects of regio defects and comonomers on the tacticity distribution were corrected by subtracting representative regio defect and comonomer integrals from the specific integrated region of the stereo sequence.
[0557] Isotacticity is determined at the pentad level and reported as the percentage of isotactic pentad (mmmm) sequences to all pentad sequences:
[0558] [mmmm]% = 100*(mmmm / sum of all pentads)
[0559] The presence of the 2,1 erythro regio defect is indicated by the presence of two methyl sites at 17.7 and 17.2 ppm and confirmed by other characteristic sites. No characteristic signals corresponding to other types of regio defects were observed (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253).
[0560] The amount of 2,1 erythro regio defect was quantified using the average integral of two characteristic methyl sites at 17.7 and 17.2 ppm.
[0561] P 21e =(I e6 +I e8 ) / 2
[0562] The amount of 1,2 major propylene insertions was quantified based on the methyl region, with corrections made for sites not associated with the major insertion contained within this region and for major insertion sites not contained within this region.
[0563] P 12 =I CH3 +P 21e
[0564] The total amount of propene was quantified as the sum of the primary inserted propene and all other regio defects present.
[0565] P 总 =P 12 +P 21e
[0566] The mole percentage of 2,1 erythro regio defects relative to all propylene was quantified.
[0567] [21e] mol% = 100*(P 21e / P 总 )
[0568] Intrinsic viscosity
[0569] The intrinsic viscosity (iV) is measured analogously to DIN ISO 1628 / 1, October 1999, in decalin at 135° C.
[0570] density
[0571] Density was measured according to ISO 1183-1. Sample preparation was performed by compression molding according to ISO 1872-2:2007.
[0572] Particle size distribution
[0573] Median particle size d 50 and top cut particle size d 95 It is measured by gravity liquid sedimentation according to ISO 13317-3.
[0574] Flexural modulus
[0575] Flexural modulus according to ISO 178 at 23°C on 80×10×4 mm injection molded according to EN ISO 1873-2 3 Measured on a test bar in 3-point bending.
[0576] Notched Impact Strength (NIS)
[0577] Charpy notched impact strength (NIS) was measured according to ISO 179 1eA at -20°C and +23°C using 80×10×4 mm prepared according to ISO 294-1:1996. 3The measurements were performed on injection molded rod specimens.
[0578] VOC value, FOG value
[0579] Sample preparation
[0580] The VOC and FOG values were measured as described below after sample preparation consisting of injection-molded plaques according to EN ISO 19069-2: 2016. The plaques were packed in aluminum composite foils immediately after production and the foils were sealed.
[0581] For the thermal desorption analysis according to VDA 278 (October 2011), the samples were stored uncovered at room temperature (max. 23° C.) for 7 days before starting the analysis.
[0582] The production date of the injection molded plaques, the time of arrival of the samples at the laboratory, and the date of analysis were recorded.
[0583] VOC and FOC according to VDA278
[0584] The VOC values are determined from injection molded plaques according to VDA 278, October 2011. VDA 278, October 2011, Thermal desorption analysis for the characterization of organic emissions from non-metallic materials for use in vehicles, VDA Verbandder Automobilindustrie. According to VDA 278, October 2011, the VOC value is defined as "the sum of highly volatile to moderately volatile substances. They are calculated in toluene equivalent. The method described in this recommendation allows the determination and analysis of substances in the boiling / elution range up to n-pentacosane (C25)".
[0585] The FOG value is determined from injection molded plaques according to VDA 278, October 2011. According to VDA 278, October 2011, the FOG value is defined as "the sum of substances with low volatility eluting from the retention time of n-tetradecane (inclusive)". It is calculated in hexadecane equivalents. Determination and analysis of the FOG value in the n-alkanes "C 14 ” to “C 32 "Substances within the boiling range of .
[0586] Specific methods for recyclables
[0587] Amounts of iPP, polystyrene, polyethylene (and copolymers containing ethylene), poly(ethylene terephthalate) and polyamide-6
[0588] To establish different calibration curves, different standards, namely iPP and HDPE as well as iPP, PS and PA6 were blended. To quantify the content of foreign polymers, IR spectra were recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. The films were prepared using a compression molding device at 190 °C and a clamping force of 4 to 6 MPa. The film thickness of the calibration standards for iPP and HDPE was 300 μm, while for the quantification of iPP, PS and PA 6, film thicknesses of 50 to 100 μm were used. Standard transmission FTIR spectroscopy was employed, using a spectral range of 4000 to 400 cm -1 , aperture is 6mm, spectral resolution is 2cm -1 , 16 background scans, 16 spectral scans, an interferogram zero filling factor of 32 and Norton Beer strong apodization were performed.
[0589] Measure iPP at 1167cm -1 The absorbance of the band at 37° was measured and the iPP content was quantified according to the calibration curve (absorption / thickness (cm) versus iPP content (wt%)).
[0590] Measured at 1601cm -1 (PS) and 3300cm -1 The absorbance of the band at (iPP + PS + PA6) was measured and the PS and PA6 contents were quantified according to the calibration curve (absorption / thickness (cm) versus PS and PA content (wt%)). The contents of polyethylene and ethylene-containing copolymers were obtained by subtracting (iPP + PS + PA6) from 100, taking into account the content of non-polymer impurities determined in the following method. The analysis was performed in duplicate.
[0591] The amount of metal
[0592] The amount of metal was determined by X-ray fluorescence (XRF).
[0593] Amount of paper and wood
[0594] Paper and wood were tested by conventional laboratory methods including grinding, flotation, microscopy and thermogravimetric analysis (TGA).
[0595] Amount of talc and chalk
[0596] TGA is conducted according to the following procedures:
[0597] Thermogravimetric analysis (TGA) experiments were performed using a Perkin Elmer TGA8000. Approximately 10 to 20 mg of material was placed in a platinum pan. The temperature was equilibrated at 50°C for 10 minutes and then raised to 950°C at a heating rate of 20°C / min under nitrogen. The weight loss (WCO2) between about 550°C and 700°C was attributed to CO2 released from CaCO3, so the chalk content was estimated as:
[0598] Chalk content = 100 / 44×WCO2
[0599] The temperature is then lowered to 300°C at a cooling rate of 20°C / min. The gas is then switched to oxygen and the temperature is raised to 900°C again. The weight loss in this step is attributed to carbon black (Wcb). In the case where the content of carbon black and chalk is known, the ash content excluding chalk and carbon black is calculated as:
[0600] Ash content = (ash residue) – 56 / 44 × WCO2 – Wcb
[0601] The ash is the weight % measured at 900° C. in a first step carried out under nitrogen. The ash content is estimated to be identical to the talc content of the cycle studied.
[0602] Ash content
[0603] The ash content was measured by thermogravimetric analysis (TGA) according to ISO 11358-1 (20147) standard.
[0604] Limonene Measurement
[0605] Limonene quantification was performed using solid phase microextraction (HS-SPME-GC-MS) by standard addition.
[0606] 50 mg of ground sample was weighed into a 20 mL headspace vial and the vial was sealed with a silicone / PTFE lined magnetic cap after adding different concentrations of limonene and a glass coated magnetic stir bar. A known concentration of diluted limonene standard was added to the sample using a microcapillary (10 pL). 0, 2, 20 and 100 ng equivalent to 0 mg / kg, 0.1 mg / kg, 1 mg / kg and 5 mg / kg of limonene were added, in addition, 6.6 mg / kg, 11 mg / kg and 16.5 mg / kg of standard amounts of limonene were used in conjunction with some of the samples tested in this application. For quantification, ion 93 in SIM mode was used. Volatile components were enriched by headspace solid phase microextraction at 60°C for 20 minutes using a 2 cm stable curved 50 / 30 pm DVB / Carboxen / PDMS fiber. Desorption was performed directly in the heated injection port of the GCMS system at 270°C.
[0607] GCMS parameters:
[0608] Column: 30m HP 5MS 0.25*0.25
[0609] Syringe: Splitless, with 0.75 mm SPME liner, 270 °C
[0610] Temperature program: -10℃(1min)
[0611] Carrier gas: Helium 5.0, 31cm / s linear velocity, constant flow
[0612] MS: Single quadrupole, direct interface, interface temperature 280°C
[0613] Acquisition: SIM scan mode
[0614] Scan parameters: 20-300amu
[0615] SIM parameters: m / Z 93, 100 ms dwell time
[0616] Total free fatty acid content
[0617] Fatty acid quantification was performed using headspace solid phase microextraction (HS-SPME-GC-MS) by standard addition.
[0618] 50 mg of ground sample was weighed in a 20 mL headspace vial and sealed with a silicone / PTFE lined magnetic cap after adding different concentrations of limonene and a glass coated magnetic stir bar. Using a 10 μL microcapillary, a known concentration of a diluted free fatty acid mixture (acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid and octanoic acid) standard was added to the sample at three different levels. The addition of 0, 50, 100 and 500 ng is equivalent to 0 mg / kg, 1 mg / kg, 2 mg / kg and 10 mg / kg of each individual acid. All acids except propionic acid (here ion 74 was used) were quantified using ion 60 collected in SIM mode.
[0619] GCMS parameters:
[0620] Column: 20m ZB Wax plus 0.25*0.25
[0621] Syringe: Split 5:1, split liner with glass liner, 250°C
[0622] Temperature program: 40℃(1min)@6℃ / min to 120℃, @15℃ to 245℃(5min)
[0623] Carrier gas: Helium 5.0, 40 cm / s linear velocity, constant flow
[0624] MS: Single quadrupole, direct interface, interface temperature 220°C
[0625] Acquisition: SIM scan mode
[0626] Scan parameters: 46 to 250 amu 6.6 scans / second
[0627] SIM parameters: m / z 60, 74, 6.6 scans / sec
[0628] 1. Preparation of heterophasic propylene copolymer (HECO)
[0629] a) Preparation of single active site catalyst system
[0630] Catalyst complex
[0631] As described in WO 2019 / 179959, the following metallocene complexes have been used:
[0632]
[0633] Preparation of MAO-silica carrier
[0634] A steel reactor equipped with a mechanical stirrer and a filter screen was flushed with nitrogen and the reactor temperature was set to 20°C. Then, silica grade DM-L-303 (5.0 kg) from AGC Si-Tech, pre-calcined at 600°C, was added from the feed bucket and then carefully pressurized and depressurized with nitrogen using a manual valve. Toluene (22 kg) was then added. The mixture was stirred for 15 min. Then, a 30 wt % solution (9.0 kg) of MAO from Lanxess in toluene was added through the feed line at the top of the reactor within 70 min. The reaction mixture was then heated to 90°C and stirred for another two hours at 90°C. The slurry was allowed to settle and the mother liquor was filtered off. At 90°C, the catalyst was washed twice with toluene (22 kg), then settled and filtered. The reactor was cooled to 60°C and the solid was washed with heptane (22.2 kg). Finally, the MAO treated SiO2 was dried at 60° under a nitrogen stream for 2 hours and then dried under vacuum (-0.5 bar, gauge) with stirring for 5 hours. The MAO treated support was collected as a free flowing white powder which was found to contain 12.2% aluminum (by weight).
[0635] Preparation of single active site catalyst system
[0636] At 20°C, 30 wt% MAO (0.7 kg) in toluene was added to a nitrogen-sealed steel reactor by a burette. Toluene (5.4 kg) was then added under stirring. The metallocene complex (93 g) as described above under 2a) was added from a metal cylinder and then rinsed with 1 kg of toluene. The mixture was stirred for 60 minutes at 20°C. Trityl tetrakis (pentafluorophenyl) borate (91 g) was then added from a metal cylinder and subsequently rinsed with 1 kg of toluene. The mixture was stirred at room temperature for 1 h. The resulting solution was added to the stirred cake of the MAO-silica support prepared above within 1 hour. The cake was left for 12 hours, then dried for 2 hours at 60°C under a N2 stream, and dried for another 5 hours under vacuum (-0.5 bar, gauge pressure) under stirring.
[0637] The dried catalyst was sampled as a pink free-flowing powder containing 13.9% aluminum and 0.11% zirconium.
[0638] Table 1: Polymerization conditions of HECO1
[0639] HECO1 Prepolymerization temperature [℃] 18 pressure [kPa] 4867 Catalyst feed [g / h] 2.4 C3 Feed [kg / h] 72 H2 feed [g / h] 0.2 Dwell time [h] 0.36 Loop pipe (reactor 1) temperature [℃] 70 pressure [kPa] 4867 H2 / C3 Ratio [mol / kmol] 0.35 Dwell time [h] 0.29 Loop reactor split ratio (split) [weight%] 56.6 MFR2 [g / 10min] 101 GPR1 (reactor 2) temperature [℃] 80 pressure [kPa] 2500 H2 / C3 Ratio [mol / kmol] 1.7 Polymer residence time [h] 1.20 GPR Reactor Split Ratio [weight%] 31.9 <![CDATA[MFR2]]> [g / 10min] 101 GPR2 (reactor 3) temperature [℃] 70 pressure [kPa] 2500 H2 / C2 Ratio [mol / kmol] 1.7 C2 / C3 Ratio [mol / kmol] 821.7 Polymer residence time [h] 1.40 GPR Reactor Split Ratio [weight%] 11.5 <![CDATA[MFR2]]> [g / 10min] 76
[0640] Table 2: Performance of HECO, HECO2 and HECO3
[0641] HECO1 HECO2 HECO3 <![CDATA[MFR2]]> [g / 10min] 76 100 13 <2.1> Defects (matrix) [%] 0.60 0 0 Crystalline fraction (CF) [weight%] 89.3 85.3 83.7 Soluble fraction (SF) [weight%] 10.6 14.7 16.3 Ethylene content [weight%] 2.2 8.0 7.5 Ethylene content [mol %] 3.3 11.5 10.8 CF Ethylene (C2(CF)) [weight%] 0 2.4 1.5 CF Ethylene (C2(CF)) [mol %] 0 3.6 2.2 Ethylene from SF (C2(SF)) [weight%] 23.3 39.5 39.1 Ethylene from SF (C2(SF)) [mol %] 31.3 49.7 49.1 Melting temperature Tm [℃] 157 165 165 Crystallization temperature Tc [℃] 121 121 120 Intrinsic viscosity of CF (IV(CF)) [dl / g] 1.1 1.2 1.9 Intrinsic viscosity of SF (IV(SF)) [dl / g] 2.5 3.1 2.5 IV(SF) / IV(CF) [-] 2.3 2.6 1.3 Flexural modulus [MPa] 1257 1500 1220 Notched impact strength (23℃) <![CDATA[[kJ / m 2 ]]]> 3.9 4.0 6.3 Notched impact strength (-20℃) <![CDATA[[kJ / m 2 ]]]> 2.0 2.0 3.8
[0642] Table 3: Formulation and properties of comparative composition and composition of the present invention
[0643]
[0644] “HECO2” is the commercial heterophasic propylene copolymer “BJ400HP” of Borealis AG, Austria (properties see Table 2 );
[0645] “HECO3” is the commercial heterophasic propylene copolymer “BE170CF” of Borealis AG, Austria (properties see Table 2 );
[0646] "Blend (B)" is an experimental recycled polypropylene-polyethylene blend based on separately collected post-consumer plastic waste that has been subjected to a sequence of sorting, washing and compounding steps. It has a PP content of 91.2 wt%, a total ethylene content of 7.0 wt% as determined by FTIR, an ash content of 1.7 wt% and a limonene content greater than 0.1 ppm (see Table 3 for other properties).
[0647] The “plastomer” is the commercialized ethylene-1-octene copolymer “Engage 8200” of the Dow Chemical Company of the United States, which has a hardness of 870 kg / m 3Density and melt flow rate MFR2 (190°C, 2.16kg) of 5.0g / 10min;
[0648] “HDPE” is a commercial high-density polyethylene “HE9621-PH” from Borealis AG of Austria, which has a density of 964 kg / m 3 Density and melt flow rate MFR2 (190°C, 2.16kg) of 12.0g / 10min;
[0649] The talc was commercial talc "Jetfine 3CA" from Imerys, UK, having a median particle size of 1.2 μm. 50 and a top cut particle size of 3.3 μm 95 ;
[0650] An “additive” is a mixture of:
[0651] - 15.5 wt. % of a commercial medium molecular weight solid epoxy resin "NPES 902" from Nan Ya Plastics Corp (People's Republic of China), based on the total weight of the "additives",
[0652] - 8.9% by weight of commercial erucamide "Finawax-E" from Fine Organics (UK), based on the total weight of the "additive";
[0653] - 7.8% by weight, based on the total weight of the "additives", of a commercial nucleating agent "NA-21" from Adeka (France), a mixture of bis[2,2'-methylene-bis(4,6-di-tert-butylphenyl)phosphate]hydroxyaluminum and lithium myristate,
[0654] - 7.8% by weight, based on the total weight of the "additives", of Solvay's light stabilizer Cyasorb UV-3808PP5, a masterbatch of 25% by weight of n-hexadecyl-3,5-di-tert-butyl-4-hydroxybenzoate and 25% by weight of esters of 2,2,6,6-tetramethyl-4-piperidinol and higher fatty acids (mainly stearic acid) in a PP homopolymer, the latter being commercially available as Cyasorb UV-3853 from Solvay,
[0655] - 5.8% by weight of the commercial sterically hindered phenol octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate "Songnox 1076" from Songwon (Korea), based on the total weight of the "additives",
[0656] - 3.9% by weight, based on the total weight of the "additive", of the commercial phosphorus-based antioxidant tris(2,4-di-tert-butylphenyl)phosphite "Irgafos 168" from BASF SE (Germany),
[0657] 50.3% by weight, based on the total weight of the “additives”, of a carbon black masterbatch Plasblak 10PPP6331 from Cabot (Germany).
[0658] As can be seen from the data in Table 3, the HECO of the present invention can be replaced with recycled polypropylene-polyethylene blends in varying amounts without significantly compromising the mechanical and odor properties of the final composition (compare IE1 to IE3 with CE1). Despite the addition of a less stiff component, the stiffness remains almost unchanged (for recycled material stiffness, see stiffness of CE3), while the impact and odor properties are significantly better than expected based on simple estimates of the properties of the recycled material. This enables the reuse of recycled materials in automotive applications to replace potentially expensive virgin HECO, while also helping to minimize plastic waste through recycling.
Claims
1. A composition obtainable by blending the following: (A) 18.0 to 60.0 wt. % of the multiphase composition HECO, based on the total composition; (B) 7.0 to 55.0 wt. % of recycled polypropylene-polyethylene blend B, based on the total composition; (C) 0.0 to 12.0 wt. % of high density polyethylene HDPE, based on the total composition; (D) 5.0 to 15.0 wt% of polyethylene, based on the total composition, which is the sum of the high-density polyethylene HDPE and the polyethylene contained in the recycled polypropylene-polyethylene blend B; (E) 2.0 to 12.0 wt. % of plastomer P, based on the total composition; and (F) 7.0 to 25.0 wt % of talc T, based on the total composition; wherein the multiphase composition HECO, the polypropylene-polyethylene blend B, the high-density polyethylene HDPE, the plastomer P and the talc T together constitute at least 90% by weight of the total composition; Among them further - The multiphase composition HECO comprises (a) a propylene homopolymer as a matrix, and (b) an ethylene-propylene rubber dispersed in the matrix, wherein the multiphase composition HECO has (i) a melting temperature Tm measured by DSC according to ISO 11357-3 at a heating and cooling rate of 10°C / min in the range of 150 to 159°C; (ii) a melt flow rate MFR2 measured according to ISO 1133 at a temperature of 230° C. under a load of 2.16 kg in the range of 20.0 to 120 g / 10 min; (iii) a crystalline fraction CF determined according to the CRYSTEX QC method ISO 6427, annex B, present in an amount ranging from 79.0 to 91.0% by weight relative to the total weight of the heterophasic composition HECO; (iv) a soluble fraction SF determined according to the CRYSTEX QC method ISO 6427, annex B, present in an amount ranging from 9.0 to 21.0% by weight relative to the total weight of the heterogeneous composition HECO; and (v) a total ethylene content measured by Fourier transform infrared spectroscopy FITR during CRYSTEX analysis in the range of 1.5 to 6.5 mol %, wherein ethylene is the only comonomer in the heterophasic composition HECO; - The recycled polypropylene-polyethylene blend B comprises: B-1) at least 85.0 wt. % of polypropylene relative to the total weight of said recycled polypropylene-polyethylene blend B, B-2) up to 15.0 wt. % of polyethylene, relative to the total weight of said recycled polypropylene-polyethylene blend B, Wherein the recycled polypropylene-polyethylene blend B has: i) a melt flow rate MFR2 measured according to ISO 1133 at a temperature of 230°C under a load of 2.16 kg in the range of 5.0 to 75 g / 10 min; and ii) a residual ash content in the range of 0.1 to 3.0 wt. % as measured by thermogravimetric analysis according to ISO 11358-1; and one or more of the following: iii) 0.1 ppm to 100 ppm of limonene content determined by solid phase microextraction using HS-SPME-GC-MS in headspace mode; iv) a content of one or more fatty acids in the range of 0.1 to 100 ppm as determined by solid phase microextraction using HS-SPME-GC-MS in headspace mode; v) a content of one or more polyamides of at most 1.5% by weight and above the detection limit, determined by NMR; vi) a content of one or more polystyrenes determined by NMR of 0.05 to 3.0% by weight; - The plastic body has a density of 850 to 900 kg / m 3 Ethylene 1-octene copolymers or ethylene 1-butene copolymers having a density measured according to ISO 1183-1 within a range of 1:1 to 5:
1.
2. The composition according to claim 1, wherein the multiphase composition HECO has a through 13 2,1 regio defects determined by C-NMR, and / or the melting temperature Tm measured by DSC according to ISO 11357-3 at a heating and cooling rate of 10°C / min in the range of 153 to 158°C.
3. The composition according to claim 1 or claim 2, wherein the ethylene content of the soluble fraction of the multiphase composition HECO measured by infrared spectroscopy during CRYSTEX analysis is in the range of 22.0 to 39.0 mol%.
4. The composition according to claim 1 or claim 2, wherein the ethylene content of the crystalline fraction of the multiphase composition HECO measured by infrared spectroscopy during CRYSTEX analysis is in the range of 0.0 to 0.7 mol%.
5. The composition according to claim 1 or claim 2, wherein the multiphase composition HECO has (i) an intrinsic viscosity of the soluble fraction in the range of 1.80 to 3.20 dl / g; (ii) an intrinsic viscosity of the crystalline fraction in the range of 0.80 to 1.80 dl / g; and (iii) a ratio of the intrinsic viscosity of the soluble fraction SF to the intrinsic viscosity of the crystalline fraction CF in the range of 1.50 to 2.
80.
6. The composition of claim 1 or claim 2, wherein at least 90 wt. % of the amount of the recycled polypropylene-polyethylene blend B originates from post-consumer waste.
7. The composition according to claim 1 or claim 2, wherein the weight ratio between the heterophasic composition HECO and the recycled polypropylene-polyethylene blend B is in the range of 0.2 to 8.
0.
8. The composition according to claim 1 or claim 2, wherein the plastomer is an ethylene 1-octene copolymer having a melt flow rate MFR2 measured according to ISO 1133 at a temperature of 190°C under a load of 2.16 kg in the range of 2.0 to 10.0 g / 10 min, and having a melt flow rate MFR2 in the range of 860 to 890 kg / m 2 Density measured according to ISO 1183-1 within the range.
9. according to the composition described in claim 1 or claim 2, wherein said high density polyethylene HDPE has 940 to 970kg / m 3 The density measured according to ISO 1183-1 is in the range of 400 Å and the melt flow rate MFR2 measured according to ISO 1133 at a temperature of 190° C. under a load of 2.16 kg is in the range of 2.0 to 20.0 g / 10 min.
10. The composition of claim 1 or claim 2, wherein the composition comprises 2 to 12 wt% of the high density polyethylene HDPE based on the total composition.
11. The composition according to claim 1 or claim 2, consisting of the following (A) 18.0 to 60.0 wt. % of the multiphase composition HECO, based on the total composition; (B) 7.0 to 55.0 wt. % of said recycled polypropylene-polyethylene blend B, based on the total composition; (C) 2.0 to 12.0 wt% of said high density polyethylene HDPE based on the total composition; (D) 2.0 to 12.0 wt. % of said plastomer P based on the total composition; (E) 7.0 to 25.0 wt% of said talc T based on the total composition; and (F) 1.0 to 10.0 wt % of Additive A based on the total composition.
12. A composition according to claim 1 or claim 2, wherein the talc T has a median particle size d measured according to ISO 13317-3 in the range of 0.5 to 2.0 μm. 50 and a top cut particle size d measured according to ISO 13317-3 in the range of 1.0 to 8.0 μm 95 .
13. A composition according to claim 1 or claim 2 having a melt flow rate MFR2 measured according to ISO 1133 at a temperature of 230°C under a load of 2.16 kg in the range of 10.0 to 30.0 g / 10 min.
14. A composition according to claim 1 or claim 2 having a VOC of less than 100 μg / gram of composition measured directly on material obtained from extrusion according to the procedure described in VDA 278.
15. An automotive article comprising at least 95% by weight of the composition according to any one of claims 1 to 14.
Citation Information
Patent Citations
Elastic substantially linear olefin polymers
US5272236A
Multi-stage process for producing polyethylene
WO1992012182A1
A process for forming a carrier material
WO1994014856A1
Supported olefin polymerization catalyst, its preparation and use
WO1995012622A1
Process for preparing polypropylene
WO1999024478A1