Optical film, polarizing plate and liquid crystal display device

By locally increasing the laser absorption rate in the surface area of ​​the optical film and setting an appropriate light absorption ratio, the problems of insufficient laser shearability and transparency damage of the cycloolefin resin film in the existing technology are solved, and efficient laser shearing and prevention are achieved. Light leak effect.

CN116157255BActive Publication Date: 2024-10-18KONICA MINOLTA INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202180059593.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-27
Publication Date
2024-10-18
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

In the prior art, polarizer protective films containing cyclic olefin resins have low laser absorption rates during laser shearing, resulting in insufficient shearability, and adding a large amount of laser absorbers in order to improve laser shearability will damage the optical film. Transparency, prone to light leakage problems.

Method used

By locally increasing the laser absorption rate in the surface area of ​​the optical film, and setting the light absorption ratio between the surface area and the inner area between 1.1 and 20, it is ensured that the laser shearability is improved without damaging the transparency, and light leakage in the display device is suppressed. .

Benefits of technology

It is possible to improve the laser shearability without damaging the transparency of the optical film, reduce the stress difference during the laser shearing process, and avoid light leakage in the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116157255B_ABST
    Figure CN116157255B_ABST
Patent Text Reader

Abstract

The optical film of the present invention contains a cycloolefin resin. When the area from one side of the optical film to a depth of 30% of the thickness is defined as a surface area Sa, the area from the other side of the optical film to a depth of 30% of the thickness is defined as a surface area Sb, and the area between the surface area Sa and the surface area Sb is defined as an inner area C, at least the ratio As / Ac of the absorption coefficient As of the light with a wavelength of 9.6 μm in the surface area Sa to the absorption coefficient Ac of the light with a wavelength of 9.6 μm in the inner area C is 1.1 to 20, and the absorption coefficient of the light with a wavelength of 9.6 μm of the optical film is 1.5×10 ‑5 / μm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical film, a polarizing plate and a liquid crystal display device. Background Art

[0002] Display devices such as liquid crystal display devices include polarizing plates. The polarizing plate includes a polarizer and a polarizer protective film. As the polarizer protective film, a cycloolefin resin film is sometimes used from the viewpoint of having excellent transparency and high moisture resistance.

[0003] Such a polarizer is usually used after the polarizer and the polarizer protective film are bonded together with an adhesive, etc., and then sheared into a given size. The polarizer is sheared, for example, by a mechanical shearing method using a knife, a laser shearing method using a laser, etc. In the mechanical shearing method, fine damage is easily generated, and the residual stress is also easily uneven, so in recent years, the laser shearing method has been adopted more.

[0004] Cycloolefin resin films are generally difficult to cut with lasers due to their low laser absorption rate.

[0005] On the other hand, in order to enable cutting by the laser shearing method, there is known a polarizing plate using a polarizer protective film including a substrate containing a laser absorbent (for example, see Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: International Publication No. 2018 / 139638 Summary of the invention

[0009] Technical problem solved by the invention

[0010] However, the laser shearing property of the polarizer protective film containing cycloolefin resin in Patent Document 1 is still insufficient. Therefore, in order to shear the polarizer protective film with laser, laser irradiation under high illumination is required. As a result, the polarizer with high laser absorptivity is prone to burn and produce soot, causing the polarizer to be contaminated. On the other hand, if a large amount of laser absorbent (light absorbing material) is added to improve the laser shearing property, the transparency of the optical film is easily damaged.

[0011] In this regard, the inventors have found that by partially increasing the laser absorptivity of the surface region of the polarizer protective film (optical film), the laser shearing property can be improved without damaging the transparency of the optical film. On the other hand, if the laser absorptivity of the surface region is too high, there is a new problem that light leakage is easily generated in the display device.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an optical film, a polarizing plate, and a liquid crystal display device capable of improving laser shearing properties without causing light leakage in a display device.

[0013] Technical means of solving problems

[0014] The present invention relates to the following optical films, polarizing plates, and liquid crystal display devices.

[0015] The optical film of the present invention is an optical film containing a cycloolefin resin, wherein a region from a surface of one side of the optical film to a depth of 30% of the thickness of the optical film is defined as a surface region Sa, a region from a surface of the other side of the optical film to a depth of 30% of the thickness of the optical film is defined as a surface region Sb, and a region between the surface region Sa and the surface region Sb is defined as an inner region C, at least a ratio As / Ac of an absorption coefficient As of light of a wavelength of 9.6 μm measured by an ATR method in the surface region Sa to an absorption coefficient Ac of light of a wavelength of 9.6 μm measured by an ATR method in the inner region C is 1.1 to 20, and an absorption coefficient of light of a wavelength of 9.6 μm in the optical film is 1.5×10 -5 / μm or more.

[0016] The polarizing plate of the present invention comprises a polarizer and the optical film of the present invention disposed on at least one surface of the polarizer.

[0017] The liquid crystal display device of the present invention comprises a liquid crystal cell, and a first polarizing plate and a second polarizing plate sandwiching the liquid crystal cell, and at least one of the first polarizing plate and the second polarizing plate is the polarizing plate of the present invention.

[0018] Effects of the Invention

[0019] According to the present invention, it is possible to provide an optical film, a polarizing plate, and a liquid crystal display device capable of improving laser shearing properties without causing light leakage in a display device. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] [ Figure 1 ] Figure 1 It is a schematic cross-sectional view showing the surface layer region and the inner layer region of the optical film.

[0021] [Figure 2] Figure 2A is a cross-sectional view showing the structure of the optical film of this embodiment, Figure 2B It is a cross-sectional view showing the structure of an optical film according to a modification.

[0022] [ Figure 3 ] Figure 3 It is a cross-sectional view showing the structure of the polarizing plate according to this embodiment.

[0023] [Figure 4] Figure 4A and B means Figure 3 A cross-sectional view of a method for manufacturing a polarizing plate. DETAILED DESCRIPTION

[0024] As described above, by locally increasing the laser absorptivity of the surface region of the optical film, the laser shearing property can be improved without impairing the transparency of the optical film. However, light leakage is likely to occur when the optical film is manufactured into a display device.

[0025] The reason is not clear, but it is presumed as follows: If the laser absorptivity of the surface region of the optical film is locally too high, the heat generated by laser absorption in the surface region becomes much greater than that in the inner region, and stress difference is likely to occur.

[0026] In contrast, in the present invention, the laser absorptivity of the surface region of the optical film is appropriately increased. That is, the absorption coefficient of the light with a wavelength of 9.6 μm of the entire optical film is set to a given value or above, and the ratio As / Ac of the absorption coefficient As of the light with a wavelength of 9.6 μm of the surface region Sa and the absorption coefficient Ac of the light with a wavelength of 9.6 μm of the inner region C is set to 1.1 to 20, preferably 3 to 15. In this way, the laser shearing property can be improved, and the stress difference caused by the heat caused by laser absorption between the surface region Sa and the inner region C can be reduced, so that light leakage in the display device can be suppressed. The following is an explanation of the structure of the present invention.

[0027] 1. Optical film

[0028] The optical film of the present invention contains a cycloolefin resin and has a laser absorptivity that is locally high (higher than that of an inner layer region) in at least one surface layer region of the optical film.

[0029] Figure 1 1 is a schematic cross-sectional view showing the surface layer regions Sa and Sb and the inner layer region C of the optical film 10 .

[0030] When the regions from the surface 10a on one side and the surface 10b on the other side of the optical film 10 to a depth of 30% of the thickness of the optical film 10 are respectively defined as the surface regions Sa and Sb, and the region therebetween is defined as the inner region C, the laser absorptivity of at least one surface region Sa is higher than the laser absorptivity of the inner region C. Specifically, it is preferred that the ratio As / Ac of the absorption coefficient As of the light with a wavelength of 9.6 μm of at least one surface region Sa to the absorption coefficient Ac of the light with a wavelength of 9.6 μm of the inner region C is 1.1 to 20.

[0031] If As / Ac is 1.1 or more, the laser absorptivity of the surface region Sa can be relatively increased, so it is easy to improve the laser shearing property. If As / Ac is 20 or less, the heat generated by the laser absorption in the surface region Sa will not be excessively greater than the heat generated by the laser absorption in the inner region C, so the stress difference caused by this can be reduced. Thus, light leakage in the display device can be suppressed. From the same point of view, As / Ac is more preferably 3 to 15.

[0032] As / Ac can be measured by the following method.

[0033] 1) First, using a micro-FTIR (UMA600 and FTS3000 manufactured by Agilent), the ATR method was used with an incident light diameter of 100 μm, a Ge prism (incident angle 45°), a detector of MCT-A, and a resolution of 4.0 cm -1 , cumulative: 64 times, the infrared absorption spectrum was measured. Based on the infrared absorption spectrum obtained, the portion corresponding to a wavelength of 9.6 μm (frequency 1041 cm -1 ) is measured, and the absorbance A of the entire optical film 10 is measured.

[0034] 2) Next, 30% of the thickness is cut from one surface 10a of the optical film 10. Then, the absorbance A1 of the cut surface is measured in the same manner as in 1) above.

[0035] 3) Furthermore, 30% of the thickness is cut from the other surface 10b of the optical film 10. Then, the absorbance A2 of the cut surface is measured in the same manner as in 1) above.

[0036] 4) The absorbances A, A1 and A2 obtained in 1) to 3) above are applied to the following formula to calculate the absorption coefficient As of the surface region Sa and the absorption coefficient Ac of the inner region C, respectively.

[0037] Absorption coefficient of surface area Sa As=(A-A1)×loge10÷(0.3T)

[0038] Absorption coefficient of inner region C Ac = A2×loge10÷(0.4T) (T: thickness of optical film 10

[0039] A: Absorbance of the optical film 10

[0040] A1: Absorbance measured by cutting 30% of the thickness T of the optical film 10 from one surface 10a of the optical film 10

[0041] A2: absorbance measured by cutting 30% of the thickness T of the optical film 10 from the other surface 10 b of the optical film 10 )

[0042] The laser absorption coefficient of the surface region Sb on the other side of the optical film 10 may be higher than or equal to the laser absorption coefficient of the inner region C. That is, the ratio As / Ac of the absorption coefficient As of the light with a wavelength of 9.6 μm in the surface region Sb of the optical film 10 to the absorption coefficient Ac of the light with a wavelength of 9.6 μm in the inner region C may be 1 to 20 or 1.1 to 20.

[0043] Furthermore, the absorption coefficient of the light with a wavelength of 9.6 μm of the optical film 10 is preferably 1.5×10 -5 / μm or more, more preferably 2.0×10 -5 ~50×10 -5 / μm.

[0044] As / Ac and the absorption coefficient A of the optical film 10 can be adjusted according to the distribution, type, content, etc. of the material (light absorbing material) that absorbs laser light. That is, in order to increase As / Ac to a given value or above, it is preferred that the surface region Sa and the inner region C of the optical film 10 each contain a light absorbing material; and that the content Ms of the light absorbing material in the surface region Sa is greater than the content Mc of the light absorbing material in the inner region C (specifically, Ms / Mc is 2.5 to 20, preferably 3.5 to 15). The light absorbing material will be described in detail below.

[0045] Such an optical film 10 may be a laminated film having a base layer and a surface layer, or may be a single-layer film.

[0046] In the following embodiments, an example in which the optical film is a laminated film having a base layer and a surface layer will be described.

[0047] Figure 2A It is a cross-sectional view showing the structure of the optical film 10 according to the present embodiment.

[0048] like Figure 2A As shown, the optical film 10 of the present embodiment includes a base layer 11 and two surface layers 12 and 13 sandwiching the base layer 11 .

[0049] The base material layer 11 contains a cycloolefin resin and a light absorbing material.

[0050] 1-1. Base material layer

[0051] 1-1-1. Cycloolefin resin

[0052] The cycloolefin resin is a polymer including a structural unit derived from a norbornene-based monomer.

[0053] The norbornene-based monomer is represented by the following formula (1).

[0054] [Chemical formula 1]

[0055] Formula (1)

[0056]

[0057] R in formula (1) 1 ~R 4 They respectively represent a hydrogen atom, a halogen atom, a hydrocarbon group or a polar group.

[0058] Examples of the halogen atom include a fluorine atom, a chlorine atom and the like.

[0059] The hydrocarbon group is a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and more preferably 1 or 2 carbon atoms. Examples of the hydrocarbon group include alkyl groups such as methyl, ethyl, propyl and butyl groups. The hydrocarbon group may further have a divalent linking group containing an oxygen atom, a nitrogen atom, a sulfur atom or a silicon atom (e.g., a carbonyl group, an imino group, an ether bond, a silyl ether bond, a thioether bond, etc.).

[0060] Examples of polar groups include carboxyl, hydroxyl, alkoxy, alkoxycarbonyl, allyloxycarbonyl, amino, amide, and methylene groups (-(CH2) n -, n is an integer greater than or equal to 1). Among them, an alkoxycarbonyl group and an aryloxycarbonyl group are preferred, and an alkoxycarbonyl group is more preferred.

[0061] Among them, R 1 ~R 4 At least one of them is preferably a polar group. This is because, when a cycloolefin resin containing a structural unit derived from a norbornene-based monomer having a polar group is formed by a solution casting method, it is easy to dissolve in a solvent, and the glass transition temperature of the obtained film is also easy to increase. On the other hand, in the melt film forming method, the cycloolefin resin may not contain a structural unit derived from a norbornene-based monomer having a polar group.

[0062] In addition, in R 1 ~R 4 In, R 1 and R 2 Both (or R 3 and R 4 Both of these) can be hydrogen atoms.

[0063] p in formula (1) represents an integer of 0 to 2. From the viewpoint of improving the heat resistance of the optical film, p is preferably 1 to 2.

[0064] Specific examples of the norbornene-based monomer represented by formula (1) are shown below. Examples of the norbornene-based monomer having a polar group include the following.

[0065] [Chemical formula 2]

[0066]

[0067] Examples of the norbornene-based monomer having no polar group include the following.

[0068] [Chemical formula 3]

[0069]

[0070] The content of the structural unit derived from the norbornene-based monomer may be 50 to 100 mol % based on the total structural units constituting the cycloolefin resin.

[0071] The cycloolefin resin may further include structural units derived from other monomers copolymerizable with the structural units derived from the norbornene monomers. Examples of other copolymerizable monomers include: (when the norbornene monomers have polar groups) norbornene monomers without polar groups, cycloolefin monomers without norbornene skeletons such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene.

[0072] As the cycloolefin resin, a commercially available product may be used. Examples of the commercially available product include ARTON (registered trademark) G, ARTON F, ARTON R, and ARTON RX manufactured by JSR Corporation.

[0073] The weight average molecular weight Mw of the cycloolefin resin is not particularly limited, but is preferably 20,000 to 300,000, more preferably 30,000 to 250,000, and further preferably 40,000 to 200,000. When the weight average molecular weight Mw of the cycloolefin resin is within the above range, the mechanical properties of the optical film can be improved without impairing the molding processability.

[0074] The weight average molecular weight Mw of the cycloolefin resin can be measured by gel permeation chromatography (GPC).

[0075] Specifically, a gel permeation chromatograph (HLC8220GPC manufactured by TOSOH Corporation) was used as a measuring apparatus, and a series of TSK-GEL G6000HXL-G5000HXL-G5000HXL-G4000HXL-G3000HXL manufactured by TOSOH Corporation was used as a column.

[0076] Then, 20±0.5 mg of the sample was dissolved in 10 ml of tetrahydrofuran and filtered through a 0.45 mm filter. 100 ml of the solution was injected into the column (temperature 40° C.), and measured at 40° C. using detector RI, and converted to polystyrene to determine the weight average molecular weight.

[0077] The glass transition temperature Tg of the cycloolefin resin is usually preferably 110° C. or higher, more preferably 110 to 350° C., and more preferably 120 to 250° C. When the Tg of the cycloolefin resin is 110° C. or higher, deformation is unlikely to occur even under high temperature conditions. When the Tg is 350° C. or lower, molding processability is unlikely to be impaired, and thermal degradation of the cycloolefin resin during molding can be further suppressed.

[0078] The glass transition temperature can be measured by a method based on JIS K 7121-2012 using DSC (Differential Scanning Colorimetry).

[0079] The content of the cycloolefin resin is not particularly limited, but is preferably 50% by mass or more, more preferably 70 to 99% by mass, based on the optical film.

[0080] 1-1-2. Light absorbing materials

[0081] The light absorbing material may have an absorption coefficient of 4.0×10- 3 Such a light absorbing material is usually a compound having a carbonyl group, preferably an ester compound or (meth)acrylic polymer particles.

[0082] <Ester Compound>

[0083] The ester compound may be any of a sugar ester compound, a polycondensation ester compound, and a polyol ester compound.

[0084] (Sugar ester compound)

[0085] The sugar ester compound is a compound obtained by esterifying all or part of the OH groups of a monosaccharide, a disaccharide or a trisaccharide. Such a sugar ester compound is preferably a compound represented by the following formula (FA).

[0086] [Chemical formula 4]

[0087] Formula (FA)

[0088]

[0089] R1 to R8 in formula (FA) represent a substituted or unsubstituted alkylcarbonyl group or a substituted or unsubstituted arylcarbonyl group. R1 to R8 may be the same as or different from each other.

[0090] The substituted or unsubstituted alkylcarbonyl group is preferably a substituted or unsubstituted alkylcarbonyl group having 2 or more carbon atoms. Examples of the substituted or unsubstituted alkylcarbonyl group include methylcarbonyl (acetyl), ethylcarbonyl, etc. Examples of the substituent that the alkyl group has include aryl groups such as phenyl.

[0091] The substituted or unsubstituted arylcarbonyl group is preferably a substituted or unsubstituted arylcarbonyl group having 7 or more carbon atoms. Examples of the arylcarbonyl group include a phenylcarbonyl group. Examples of the substituent that the aryl group has include an alkyl group such as a methyl group.

[0092] Examples of R1 to R8 in formula (FA) include the following.

[0093] [Chemical formula 5]

[0094]

[0095] The average degree of substitution of the sugar ester compound is preferably 3 to 6. The average degree of substitution of the sugar ester compound indicates the average proportion of esterified OH groups in the total number of OH groups of the sugar as a raw material.

[0096] (Polyol ester compound)

[0097] The polyol ester is an esterification product of an aliphatic polyol having a valence of 2 or more (preferably an aliphatic polyol having a valence of 2 to 20) and a monocarboxylic acid.

[0098] Examples of the polyol include adonitol, arabitol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, dibutylene glycol, 1,2,4-butylene triol, 1,5-pentanediol, 1,6-hexanediol, hexanetriol, galactitol, mannitol, 3-methylpentane-1,3,5-triol, pina alcohol, sorbitol, trimethylolpropane, trimethylolethane, xylitol, and the like, preferably triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, sorbitol, trimethylolpropane, and xylitol.

[0099] The monocarboxylic acid is not particularly limited, and may be any of aliphatic monocarboxylic acids such as acetic acid and propionic acid, alicyclic monocarboxylic acids such as cyclopentanecarboxylic acid and cyclohexanecarboxylic acid, and aromatic monocarboxylic acids such as benzoic acid and toluic acid.

[0100] The carboxylic acid used in the polyol ester compound may be one kind or a mixture of two or more kinds. In addition, all the OH groups in the polyol may be esterified or a part of them may remain as OH groups.

[0101] The molecular weight of the sugar ester compound and the polyol ester compound also depends on the production method of the optical film, but is preferably moderately low from the viewpoint of easily obtaining good compatibility with the cycloolefin resin. Specifically, the molecular weight of the sugar ester compound or the ester compound may be, for example, 300 to 1500, preferably 600 to 1200.

[0102] (polycondensation ester compound)

[0103] The polycondensation ester compound is a polycondensate (polymer) including a structural unit obtained by reacting a dicarboxylic acid with a diol.

[0104] The dicarboxylic acid may be any one of an aromatic dicarboxylic acid, an aliphatic dicarboxylic acid, and an alicyclic dicarboxylic acid, preferably an aromatic dicarboxylic acid. The dicarboxylic acid may be one or a mixture of two or more. Preferably, an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid are mixed.

[0105] The diol may be any of an aromatic diol, an aliphatic diol, and an alicyclic diol, and is preferably an aliphatic diol, and more preferably a diol having 1 to 4 carbon atoms. The diol may be one kind or a mixture of two or more kinds.

[0106] That is, the polycondensation ester compound preferably comprises a structural unit obtained by reacting a dicarboxylic acid including an aromatic dicarboxylic acid with a diol having 1 to 8 carbon atoms, and more preferably comprises a structural unit obtained by reacting a dicarboxylic acid including an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid with a diol having 1 to 8 carbon atoms. Both ends of the polycondensation ester molecule may be capped or uncapped.

[0107] Among these ester compounds, sugar ester compounds are particularly preferred because they have a moderately low molecular weight and excellent compatibility with cycloolefin resins.

[0108] <(Meth)acrylic polymer particles>

[0109] The (meth)acrylic polymer particles are particles of a polymer containing a structural unit derived from (meth)acrylic acid esters, and are preferably particles of a polymer containing a structural unit derived from methyl methacrylate.

[0110] The polymer containing a structural unit derived from methyl methacrylate may further contain a structural unit derived from other comonomers. Examples of other comonomers include: (meth)acrylic acid alkyl esters having 1 to 18 carbon atoms other than methyl methacrylate; α,β-unsaturated acids such as (meth)acrylic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; styrenes such as styrene and α-methylstyrene; polyfunctional (meth)acrylates having two or more (meth)acryloyl groups such as (poly)ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; polyfunctional monomers such as (meth)acrylate allyl alkyl esters such as (meth)acrylate and allyl alkyl (meth)acrylate, etc.

[0111] Among them, the polymer is preferably a cross-linked polymer, that is, preferably a copolymer comprising structural units derived from methyl methacrylate and structural units derived from multifunctional monomers; more preferably, it is a copolymer comprising structural units derived from methyl methacrylate, structural units derived from styrene, and structural units derived from multifunctional monomers.

[0112] From the viewpoint of improving the laser absorption rate of the substrate layer 11, the content of the structural unit derived from the (meth)acrylate containing a carbonyl group is preferably given or more. From such a viewpoint, the total amount of the structural unit derived from methyl methacrylate is preferably 30 mol% or more, more preferably 50 to 80 mol% relative to the total structural units constituting the polymer.

[0113] The content of the structural unit derived from the polyfunctional monomer is preferably 3 to 50 mol %, more preferably 10 to 35 mol %, based on the total of all structural units constituting the polymer.

[0114] The (meth)acrylic polymer particles are preferably polymers whose refractive index difference with the cycloolefin resin is 0.01 or less. Such (meth)acrylic polymer particles are unlikely to reduce the transparency of the obtained optical film.

[0115] The refractive index of the cycloolefin resin and the (meth)acrylic polymer particles are the refractive index of light at a wavelength of 550 nm. The refractive index of light at a wavelength of 550 nm can be obtained, for example, by preparing a sample film containing each component alone and measuring the refractive index of light at a wavelength of 550 nm of the sample film using a UVSEL spectroscopic ellipsometer manufactured by Horiba.

[0116] The Tg of the (meth)acrylic polymer particles is preferably 80° C. or higher. The Tg of the (meth)acrylic polymer particles can be measured in accordance with JIS K 7121-2012 or ASTM D 3418-82 in the same manner as described above.

[0117] The average particle size of the (meth)acrylic polymer particles is not particularly limited, and is preferably 50 to 500 nm, for example. If the average particle size is within the above range, the laser absorptivity can be increased, and unevenness of a suitable size can be formed on the surface of the film, thereby imparting slip properties. From this viewpoint, the average particle size of the (meth)acrylic polymer particles is more preferably 0.07 to 0.28 μm.

[0118] The average particle size of the (meth)acrylic polymer particles can be measured by the following procedure.

[0119] The average particle size of the (meth) acrylic polymer particles in the optical film can be measured by the following method. First, the optical film is sheared and the obtained sheared surface is observed by TEM. Then, the particle size is measured for any 100 particles. The particle size is the same as above, and is measured as the circle equivalent diameter of 100 particles obtained by TEM photography. Then, the average value of the obtained particle size is set as the "average particle size". It should be noted that in the TEM image, the portion with a brightness of more than 150% of the average brightness of the field of view is judged as a particle.

[0120] The content of the light absorbing material in the base layer 11 can be set so that Ms / Mc and further As / Ac of the optical film 10 satisfy the above ranges and the absorption coefficient A of the entire optical film 10 satisfies the above ranges.

[0121] That is, the content Mc' of the light absorbing material in the substrate layer 11 is preferably less than the content Ms' of the light absorbing material in the surface layer 12 (or 13). Specifically, the content Mc' of the light absorbing material in the substrate layer 11 is preferably 0.1 to 4.5% by mass, and more preferably 0.3 to 3.5% by mass relative to the substrate layer 11. If the content Mc' of the light absorbing material in the substrate layer 11 is within the above range, it is easy to adjust Ms / Mc (or Ms' / Mc') and further As / Ac to the above range, and at the same time, the absorption coefficient A of the entire optical film 10 is within the above range. As a result, the laser shearing property of the optical film 10 can be improved, and the difference in the amount of heat generated by the laser between the substrate layer 11 and the surface layer 12 (or 13) can be reduced, so that light leakage in the display device can be easily suppressed.

[0122] 1-1-3. Other ingredients

[0123] The base layer 11 may further contain other components such as inorganic fine particles as necessary.

[0124] Inorganic particles have the function of improving the slip properties of the optical film. Examples of inorganic materials constituting the inorganic particles include oxides such as silicon dioxide (SiO2), titanium dioxide, aluminum oxide, and zirconium oxide. Among them, silicon dioxide is preferred from the viewpoint of being able to reduce the increase in the haze of the film.

[0125] Examples of commercially available silica particles include AEROSIL R812 and R972 (manufactured by Nippon Aerosil Co., Ltd.), and NanoTek SiO2 (manufactured by CI Chemical Co., Ltd.).

[0126] The average primary particle size of the inorganic fine particles is preferably 5 to 50 nm. If the average primary particle size of the inorganic fine particles is 5 nm or more, the surface of the film can be roughened, so it is easy to impart slipperiness. If it is 50 nm or less, it is easy to suppress the increase of haze. The average primary particle size of the inorganic fine particles is more preferably 5 to 30 nm. The average primary particle size of the inorganic fine particles in the optical film 10 can be measured by the same method as described above.

[0127] The content of the inorganic fine particles is not particularly limited, but may be 0 to 5% by mass, preferably 0 to 2% by mass, based on the mass of the optical film.

[0128] 1-1-4. Physical properties

[0129] The thickness of the base material layer 11 is not particularly limited and may be set so that As / Ac and the absorption coefficient of the entire optical film are within the above ranges. For example, the thickness is preferably 30 to 60 μm, and more preferably 35 to 55 μm.

[0130] 1-2. Surface layers 12 and 13

[0131] The surface layer 12 is included in the surface region Sa from the surface 10a on one side of the optical film 10 to 30% of the thickness; the surface layer 13 is included in the surface region Sb from the surface 10b on the other side of the optical film 10 to 30% of the thickness (refer to Figure 1 and 2A The surface layers 12 and 13 may be respectively composed of a thermoplastic resin composition containing a thermoplastic resin and a light absorbing material (mode 1), or may be composed of a cured product of a curable composition containing a curable compound having light absorption (curable compound as a light absorbing material) and a curing agent (mode 2).

[0132] <For Method 1>

[0133] The surface layers 12 and 13 may be respectively composed of a resin composition containing a thermoplastic resin and a light absorbing material. It should be noted that the thermoplastic resin may also serve as the light absorbing material.

[0134] (Thermoplastic resin)

[0135] The thermoplastic resin contained in the thermoplastic resin composition is not particularly limited as long as it has light transparency, and may be a cycloolefin resin, a (meth)acrylic resin, or the like.

[0136] The cycloolefin resin contained in the surface layer 12 (or 13 ) may be the same as the cycloolefin resin contained in the base layer 11 .

[0137] The (meth)acrylic resin contained in the surface layer 12 (or 13) can function not only as a thermoplastic resin but also as a light absorbing material.

[0138] The (meth)acrylic resin is preferably a polymer containing a structural unit derived from methyl methacrylate. The polymer may also contain a structural unit derived from a monomer copolymerizable with methyl methacrylate. Examples of other monomers copolymerizable with methyl methacrylate include: (meth)acrylic acid alkyl esters having 1 to 18 carbon atoms other than methyl methacrylate such as 2-ethylhexyl methacrylate; α,β-unsaturated acids such as (meth)acrylic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; styrenes such as styrene and α-methylstyrene; maleic anhydride; maleimides such as maleimide and N-phenylmaleimide; glutaric anhydride, etc.

[0139] The content of the structural unit derived from methyl methacrylate is preferably 50% by mass or more, more preferably 70% by mass or more, based on all structural units constituting the copolymer. The weight average molecular weight of the (meth)acrylic resin is more preferably 40,000 to 500,000.

[0140] Among them, the thermoplastic resin contained in the surface layer 12 (or 13) is preferably a cycloolefin resin from the viewpoint of good interlayer adhesion with the base layer 11 and less likely to impair transparency.

[0141] The composition of the cycloolefin resin contained in the surface layer 12 (or 13) may be the same as or different from the composition of the cycloolefin resin contained in the base layer 11. In terms of improving interlayer adhesion and production efficiency, it is preferred that the composition of the cycloolefin resin contained in the surface layer 12 (or 13) is the same as the composition of the cycloolefin resin contained in the base layer 11.

[0142] (Light absorbing material)

[0143] As the light absorbing material contained in the surface layer 12 (or 13 ), the same material as the light absorbing material contained in the base material layer 11 can be used.

[0144] The type of light absorbing material contained in the surface layer 12 (or 13) may be the same as or different from the type of light absorbing material contained in the base layer 11. From the viewpoint of improving manufacturing efficiency, the type of light absorbing material contained in the surface layer 12 (or 13) is preferably the same as the type of light absorbing material contained in the base layer 11.

[0145] The content of the light absorbing material in the surface layer 12 (or 13) is preferably set so that Ms / Mc and further As / Ac of the optical film 10 satisfy the above ranges and the absorption coefficient A of the entire optical film 10 satisfies the above ranges.

[0146] That is, the content Ms' of the light absorbing material in the surface layer 12 (or 13) is preferably greater than the content Mc' of the light absorbing material in the base layer 11. Specifically, although it also depends on the content Ms' of the light absorbing material in the surface layer 12 (or 13), Ms' / Mc' is preferably 2.5 to 50, and more preferably 7 to 15. For example, the content Ms' of the light absorbing material in the surface layer 12 (or 13) is preferably 1 to 30% by mass, and more preferably 3 to 10% by mass relative to the surface layer 12 (or 13). If the content Ms' of the light absorbing material in the surface layer 12 (or 13) is within the above range, it is easy to adjust Ms / Mc (Ms' / Mc') and further As / Ac to the above range, and at the same time, the absorption coefficient A of the entire optical film 10 is within the above range. As a result, the laser shearing property of the optical film 10 can be improved, and the difference in the amount of heat generated by the laser between the base layer 11 and the surface layer 12 (or 13) can be reduced, so that light leakage in the display device can be easily suppressed. That is, from the viewpoint of suppressing light leakage in the display device, it is preferable that Ms' / Mc' is not too large and Ms' is not too large.

[0147] (Other ingredients)

[0148] The surface layer 12 (or 13 ), like the base layer 11 , may further contain other components such as inorganic fine particles.

[0149] <For Method 2>

[0150] The surface layer 12 (or 13) may be composed of a cured product of a curable composition containing a curable compound having light absorption and a curing agent.

[0151] The light-absorbing curable compound contained in the curable composition is preferably a urethane compound having a group reactive with a curing agent.

[0152] (Carbamate compound)

[0153] The carbamate compound having a functional group that reacts with a curing agent is obtained by reacting a polyol with a polyisocyanate. The carbamate compound may be a monomer or a prepolymer. Such a carbamate compound, for example, has a functional group (hydroxyl, acrylate, carboxyl, acrylamide, etc.) that remains unreacted after the reaction of the polyol with the polyisocyanate as a group that reacts with a curing agent.

[0154] Examples of polyols include polyester polyols obtained by reacting a polyol compound (e.g., ethylene glycol, propylene glycol, 1,4-butanediol, neopentyl glycol, glycerol, trimethylolpropane, etc.) with a polyacid (e.g., dicarboxylic acids including polycarboxylic acids such as adipic acid, succinic acid, sebacic acid, glutaric acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, polycarboxylic acids such as tricarboxylic acids such as trimellitic acid, or anhydrides thereof); polyether polyols (e.g., poly(oxypropylene ether) polyols, poly(oxyethylene-propylene ether) polyols); polycarbonate polyols, etc. Among them, polycarbonate polyurethane is preferred.

[0155] The curing agent is a compound having two or more functional groups in the molecule that react with the (unreacted) functional groups contained in the carbamate compound. For example, examples of curing agents for carbamate compounds containing a hydroxyl group (as a group that reacts with the curing agent) include epoxy compounds, isocyanate compounds, tertiary amine compounds, and carbodiimide compounds; examples of curing agents for carbamate compounds having an acrylamide group (as a group that reacts with the curing agent) include active hydrogen compounds such as dicarboxylic acids.

[0156] It should be noted that the urethane compound (urethane acrylate) having an acrylate group (as a group reactive with a curing agent) is a compound obtained by reacting a polyol having an acrylate group with a polyisocyanate, or a compound obtained by reacting a polyol with a polyisocyanate and then esterifying the unreacted isocyanate group of the obtained urethane compound with (meth)acrylic acid.

[0157] Urethane acrylate may be used in combination with other (meth)acrylate compounds. Examples of other (meth)acrylate compounds include isocyanuric acid acrylates such as isocyanuric acid diacrylates and isocyanuric acid triacrylates.

[0158] The curing agent for the urethane acrylate may be a free radical curing agent. Examples of the free radical curing agent include intramolecular cleavage type initiators such as α-hydroxyalkylphenone.

[0159] (Other ingredients)

[0160] The curable composition may further contain other components such as a curing accelerator, a curing aid, and fine particles as necessary.

[0161] For example, when an epoxy compound is used as a curing agent, a tertiary amine compound or a boron trifluoride complex may be used as a curing accelerator. Examples of the fine particles include inorganic fine particles such as silica particles.

[0162] <Common matters between Method 1 and 2>

[0163] As described above, the surface layer 12 (or 13) may be composed of a thermoplastic resin composition containing a thermoplastic resin and a light absorbing material (mode 1), or may be composed of a cured product of a curable composition containing a light absorbing curable compound and a curing agent (mode 2). Among them, from the viewpoint of good interlayer adhesion with the base layer 11 and difficulty in peeling, the surface layer 12 (or 13) is preferably composed of mode 1, i.e., a thermoplastic resin composition containing a thermoplastic resin and a light absorbing material; (similar to the base layer 11), it is more preferably composed of a thermoplastic resin composition containing a cycloolefin resin and a light absorbing material.

[0164] 1-1-4. Physical properties

[0165] The thickness of the surface layer 12 (or 13) can be set in such a way that the As / Ac and the absorption coefficient A of the entire optical film are within the above ranges, and is not particularly limited. It is preferably 0.3 to 30% relative to the total thickness of the substrate layer 11 and the surface layer 12 (or 13), and more preferably 2 to 10%. Specifically, the total thickness of the substrate layer 11 and the surface layer 12 (or surface layer 13) is preferably 20 to 100 μm, and more preferably 35 to 60 μm. In addition, the thickness of the substrate layer 11 is preferably 15 to 60 μm, and more preferably 30 to 50 μm.

[0166] 1-3. Physical properties of optical films

[0167] (Total light transmittance)

[0168] The total light transmittance of the optical film is not particularly limited as long as it has sufficient light transmittance, but is preferably 80% or more, more preferably 85% or more, and further preferably 88% or more. The total light transmittance of the optical film can be measured in accordance with JIS K7361-1:1997.

[0169] The total light transmittance of the optical film can be adjusted, for example, by the content of the light absorbing material, etc. In order to increase the total light transmittance of the optical film, for example, the content of the light absorbing material is preferably set to a predetermined value or less.

[0170] (Absorption coefficient)

[0171] As for the absorption coefficient A of the optical film, as described above, the absorption coefficient A of light with a wavelength of 9.6 μm is preferably 1.5×10 -5 / μm or more. The absorption coefficient A of the optical film is 1.5×10 -5 When the optical film has a diameter of 2.0×10 / μm or more, it can absorb laser light appropriately, thereby improving the laser shearing property. The optical film has an absorption coefficient A of 2.0×10 / μm or more, which is more preferable from the viewpoint of not easily damaging the transparency and not easily causing light leakage in the display device. -5 ~50×10 -5 / μm, more preferably 5.0×10-5 ~20×10 -5 The absorption coefficient A of the optical film can be calculated by measuring the absorbance under the above conditions by the ATR method as described above.

[0172] The extinction coefficient A of the optical film can be adjusted by the type and content of the light absorbing material, etc. From the viewpoint of increasing the extinction coefficient A of the optical film, it is preferable to increase the content of the light absorbing material.

[0173] (Phase difference Ro and Rt)

[0174] The optical film may have phase difference values ​​Ro and Rt corresponding to its use. For example, when the optical film is used as a zero phase difference film of a polarizing plate, the phase difference Ro in the in-plane direction measured under a measurement wavelength of 590 nm and an environment of 23° C. and 55% RH preferably satisfies 0 nm ≤ Ro ≤ 5 nm, and the phase difference Rt in the thickness direction preferably satisfies -5 nm ≤ Rt ≤ 5 nm.

[0175] Ro and Rt of the optical film are respectively defined by the following formulae.

[0176] Formula (2a): Ro = (nx - ny) × d

[0177] Formula (2b): Rt = ((nx + ny) / 2-nz) × d (where,

[0178] nx represents the refractive index in the slow axis direction (the direction with the highest refractive index) of the optical film in the plane.

[0179] ny represents the refractive index in the direction perpendicular to the slow axis in the optical film plane.

[0180] nz represents the refractive index in the thickness direction of the optical film

[0181] d represents the thickness of the optical film (nm).

[0182] The in-plane slow axis of an optical film refers to an axis having the highest refractive index in the film surface. The in-plane slow axis of an optical film can be confirmed by an automatic birefringence meter Axo Scan (AxoScan Mueller Matrix Polarimeter: manufactured by AXOME TRICS).

[0183] The Ro and Rt of the optical film can be measured by the following method.

[0184] 1) The optical film was humidified in an environment of 23° C. and 55% RH for 24 hours. The average refractive index of the optical film was measured using an Abbe refractometer, and the thickness d was measured using a commercially available micrometer.

[0185] 2) The retardation Ro and Rt of the optical film after humidity control at a measurement wavelength of 590 nm were measured under an environment of 23° C. and 55% RH using an automatic birefringence meter Axo Scan (Axo Scan Mueller Matrix Polarimeter: manufactured by AXOMETRICS).

[0186] The phase differences Ro and Rt of the optical film can be adjusted mainly by the stretching ratio. In order to increase the phase differences Ro and Rt of the optical film, it is preferable to increase the stretching ratio.

[0187] (thickness)

[0188] The thickness of the optical film is not particularly limited, but is preferably 20 to 100 μm, and more preferably 35 to 70 μm.

[0189] 1-4. Manufacturing method

[0190] The optical film of the present invention can be manufactured by any method. For example, the optical film 10 having the surface layer 12 (or 13) can be obtained by co-casting the substrate layer 11 and the surface layer 12 (or 13) (co-casting method), or can be obtained by coating and curing the surface layer 12 (or 13) after manufacturing the substrate layer 11 (coating method).

[0191] <Co-casting method>

[0192] The optical film 10 of the embodiment 1 is preferably produced by a co-casting method. The co-casting method may be a solution co-casting method or a melt co-casting method.

[0193] (Melt co-casting method)

[0194] In melt co-casting, a hot melt of a thermoplastic resin composition for a substrate layer and a hot melt of a thermoplastic resin composition for a surface layer are co-casted, cooled and solidified to obtain a co-cast film. Specifically, the optical film of the present invention can be obtained through the following steps: A1) a step of preparing a thermoplastic resin composition for a substrate layer and a thermoplastic resin composition for a surface layer; A2) a step of co-casting a hot melt of a thermoplastic resin composition for a substrate layer and a hot melt of a thermoplastic resin composition for a surface layer, cooling and solidifying; and A3) a step of stretching the obtained film-like product as required.

[0195] In the step A1), the components are dry-blended and then melt-kneaded using a biaxial extruder or the like to obtain pellets.

[0196] In step A2), the prepared pellets of the thermoplastic resin composition for the substrate layer and the thermoplastic resin composition for the surface layer are melt-kneaded by a twin-screw extruder or the like, and then co-cast from a co-casting die. When the glass transition temperature of the resin is Tg, the heat melting temperature in the melt co-casting can be (Tg+30) to (Tg+70)°C.

[0197] In the step A3), stretching can be performed according to the optical properties to be obtained, and the film is preferably stretched in one or more directions including the width direction (TD direction), the conveying direction (MD direction), and the oblique direction.

[0198] The stretching ratio is set according to the optical performance obtained, for example, from the viewpoint of functioning as a low phase difference film, it can be set to 1.01 to 1.3 times. The stretching ratio is defined as (stretching direction dimension of the film after stretching) / (stretching direction dimension of the film before stretching). The stretching temperature (drying temperature during stretching) is preferably (Tg-20) to (Tg+30)°C.

[0199] (Solution co-casting method)

[0200] In solution co-casting, a solution (dopant) in which components for the substrate layer are dissolved in a solvent and a solution (dopant) in which components for the surface layer are dissolved in a solvent are co-casted and then dried to obtain a co-cast film. Specifically, the optical film of the present invention can be manufactured by the following steps: B1) a step of preparing a dopant containing a cycloolefin resin, a light absorbing material and a solvent; B2) a step of casting the obtained dopant on a support, drying and peeling off to obtain a cast film; and B3) a step of stretching the obtained cast film as required.

[0201] In the step B1), a cycloolefin resin and a light absorbing material are dissolved or dispersed in a solvent to prepare a dopant.

[0202] The solvent used includes an organic solvent (good solvent) capable of dissolving at least the cycloolefin resin. Examples of the good solvent include: chlorine-based organic solvents such as dichloromethane; non-chlorine-based organic solvents such as methyl acetate, ethyl acetate, acetone, tetrahydrofuran, etc., preferably dichloromethane.

[0203] The solvent used may also include a poor solvent. Examples of the poor solvent include aliphatic alcohols having 1 to 4 carbon atoms such as methanol and ethanol, preferably ethanol. Since the dopant further including an aliphatic alcohol is easily gelled, it can be easily peeled off from the metal support.

[0204] In step B2), the obtained dopant is cast on a support by ejecting it from a casting die, etc. The solvent is evaporated until the dopant cast on the support can be peeled off from the support by a peeling roll.

[0205] The solvent is then evaporated and the resulting cast film is peeled off using a peeling roll. The amount of residual solvent in the cast film on the support during peeling depends on the drying conditions, the length of the support, etc., and may be, for example, 50 to 120% by mass. The residual solvent amount is defined by the following formula.

[0206] Residual solvent amount (mass %) = (mass of cast film before heating treatment - mass of cast film after heating treatment) / (mass of cast film after heating treatment) × 100

[0207] The heat treatment for measuring the residual solvent amount was performed at 115° C. for 1 hour.

[0208] In step B3), the cast film is stretched. The stretching ratio and stretching temperature may be the same as those in step A3).

[0209] The amount of residual solvent in the cast film at the start of stretching is preferably the same as the amount of residual solvent in the cast film at the time of peeling, and is, for example, preferably 20 to 30% by mass, more preferably 25 to 30% by mass.

[0210] <Coating method>

[0211] The optical film 10 of the second embodiment is preferably manufactured by a coating method. Specifically, the optical film 10 of the second embodiment can be obtained through the following steps: C1) a step of manufacturing a substrate layer 11; C2) a step of applying a curable composition containing a light-absorbing curable compound and a curing agent to the obtained substrate layer 11 and curing the curable composition to form a surface layer 12 (or 13).

[0212] In the step C1), the base layer 11 may be produced by the melt casting method or the solution casting method as described above.

[0213] In step C2), a curable composition containing a light-absorbing curable compound and a curing agent is applied to the surface of the base layer 11. The curable composition can be applied by any coating method, for example, by roll coating.

[0214] Then, the curable composition is cured to obtain the surface layer 12 (or 13). The curing of the curable composition may be thermal curing or photocuring, and photocuring is preferred.

[0215] 1-5. Modifications

[0216] It should be noted that in the above-described embodiment, the optical film 10 is shown as an example having two surface layers (see Figure 2A ), but is not limited thereto, and may also have a surface layer (refer to Figure 2B ).

[0217] Figure 2B 1 is a diagram showing a configuration of an optical film 10 according to a modified example. Figure 2B As shown, the optical film 10 may have only one skin layer 12. In particular, if the skin layer 12 (or 13) includes a crosslinked product of the curable composition (the embodiment 2), the optical film 10 preferably has only one skin layer.

[0218] 2. Polarizer

[0219] Figure 3 1 is a cross-sectional view showing the structure of the polarizing plate 100 of this embodiment. Figure 2A The optical film 10 of is taken as an example of the optical film 10 .

[0220] like Figure 3 As shown, the polarizing plate 100 of this embodiment includes: a polarizer 20, an optical film 10 of the present invention arranged on one side thereof, other optical films 30 arranged on the other side, and multiple adhesive layers 40 arranged between the polarizer 20 and the optical film 10 and between the polarizer 20 and the other optical films 30, respectively.

[0221] 2-1. Polarizer 20

[0222] The polarizer is an element that allows only light of a polarization plane in a given direction to pass through, and is a polyvinyl alcohol-based polarizing film. Among the polyvinyl alcohol-based polarizing films, there are films obtained by dyeing the polyvinyl alcohol-based film with iodine and films obtained by dyeing with a dichroic dye.

[0223] The polyvinyl alcohol polarizing film may be a film obtained by uniaxially stretching a polyvinyl alcohol film and then dyeing it with iodine or a dichroic dye (preferably a film further treated with a boron compound for durability); or a film obtained by dyeing a polyvinyl alcohol film with iodine or a dichroic dye and then uniaxially stretching it (preferably a film further treated with a boron compound for durability). The absorption axis of the polarizer is parallel to the maximum stretching direction.

[0224] The thickness of the polarizer is preferably 5 to 30 μm, and more preferably 5 to 20 μm from the viewpoint of reducing the thickness of the polarizing plate.

[0225] 2-2. Optical film 10

[0226] The optical film of the present invention is disposed on at least one surface of the polarizer (at least the surface facing the liquid crystal unit). Figure 3 In the figure, the surface layer 12 is arranged on the polarizer 20 side.

[0227] 2-3. Other optical films 30

[0228] Other Optical Films The optical film 10 of the present invention may be used, and other optical films such as polarizer protective films may be used. Examples of other optical films include polyester films and cellulose ester films (TAC films, etc.).

[0229] 2-4. Adhesive layer 40

[0230] The adhesive layer is disposed between the optical film 10 (or other optical film 30) and the polarizer 20 to bond them together. The adhesive constituting the adhesive layer is not particularly limited, and may be obtained by drying a completely saponified polyvinyl alcohol aqueous solution (water paste), or may be a cured product of an active energy ray-curable adhesive. The active energy ray-curable adhesive may be a photo-radical polymerizable composition utilizing photo-radical polymerization, a photo-cationic polymerizable composition utilizing photo-cationic polymerization, or a combination thereof.

[0231] The thickness of the adhesive layer may be, for example, about 0.01 to 10 μm, and preferably about 0.03 to 5 μm.

[0232] 2-5. Manufacturing method

[0233] Figure 4A and Figure 4B Yes means Figure 3 A cross-sectional view of a method for manufacturing a polarizing plate.

[0234] like Figure 4A As shown in FIG. 1 and B, the polarizing plate 100 of the present embodiment can be obtained by the following method: after obtaining a laminate 200 including a polarizer 20, an optical film 10 of the present invention disposed (laminated) on one side thereof, and another optical film 30 disposed (laminated) on the other side thereof (refer to FIG. Figure 4A ), irradiating the obtained laminate 200 with laser light L from the optical film 10 side, and cutting the laminate 200 into a given size (refer to Figure 4B ).

[0235] From the viewpoint of improving laser shearing properties, in laminating the polarizer 20 to the optical film 10 of the present invention, after laminating the surface layer 12 or 13 (the surface layer 12 in FIG. 2 ) of the optical film 10 of the present invention with a high light absorption coefficient to the polarizer 20 side, laser shearing is performed to a given size. Alternatively, laminating can be performed using an adhesive.

[0236] Laser cutting is performed from the optical film 10 side (at Figure 4A The laser is irradiated on the surface layer 13 side of the optical film 10 (in the middle). At this time, the optical film 10 can be sheared with less irradiation energy because the surface layers 12 and 13 of the optical film 10 have high laser absorption. Therefore, since the polarizer 20 is not excessively exposed to the laser, it is possible to prevent the polarizer 20 from being burned and sooting due to excessive absorption of the laser. Thus, contamination of the polarizer can be suppressed.

[0237] 3. Liquid crystal display device

[0238] The liquid crystal display device of the present invention includes a liquid crystal cell, a first polarizing plate arranged on one surface of the liquid crystal cell, and a second polarizing plate arranged on the other surface of the liquid crystal cell.

[0239] The display mode of the liquid crystal unit is not particularly limited, and may be, for example, STN (Super-Twisted Nematic), TN (Twisted Nematic), OCB (Optically Compensated Bend), HAN (Hybrid aligned Nematic), VA (Vertical Alignment, MVA (Multi-domain Vertical Vertical Alignment), PVA (Patterned Vertical Alignment)), IPS (In-Plane-Switching), etc. Among them, the IPS mode is preferred.

[0240] One or both of the first polarizing plate and the second polarizing plate are the polarizing plates of the present invention. The polarizing plate of the present invention is preferably arranged so that the optical film of the present invention is located on the liquid crystal cell side.

[0241] As described above, the polarizer 100 of the present invention has good laser shearing properties, which not only reduces the pollution of the polarizer, but also adjusts As / Ac to a suitable range. Therefore, since the heat generated by laser absorption in the surface layer 12 (or 13) of the optical film 10 is not too large relative to the heat generated by laser absorption in the substrate layer 11, it is not easy to generate stress differences caused by this. Thus, light leakage when used as a display device can be suppressed.

[0242] Example

[0243] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited thereto.

[0244] 1. Optical film materials

[0245] (1) Cycloolefin resin

[0246] As cycloolefin resins, the following COP1 to 6 were prepared.

[0247] [Table 1]

[0248]

[0249] In addition, the structural units A to D derived from the monomer are as follows, respectively.

[0250] [Chemical formula 6]

[0251]

[0252] The Tg and Mw of COP1 to 6 were measured by the following method.

[0253] [Glass transition temperature (Tg)]

[0254] The glass transition temperature of the resin is measured using DSC (Differential Scanning Colorimetry) in accordance with JIS K 7121-2012.

[0255] [Weight average molecular weight (Mw)]

[0256] The weight average molecular weight (Mw) of the resin was measured using gel permeation chromatography (HLC8220GPC manufactured by TOSOH) and a chromatographic column (TSK-GEL G6000HXL-G5000HXL-G5000HXL-G4000HXL-G3000HXL manufactured by TOSOH in series). 20±0.5 mg of the sample was dissolved in 10 ml of tetrahydrofuran and filtered with a 0.45 mm filter. 100 ml of the solution was injected into the column (temperature 40° C.), measured at detector RI and temperature 40° C., converted to styrene, and the weight average molecular weight was obtained.

[0257] (2) Light absorbing materials

[0258] <Light Absorbing Material A>

[0259] [Chemical formula 7]

[0260]

[0261] <Light absorbing material B>

[0262] Methyl methacrylate (MMA) / styrene (St) / ethylene glycol dimethacrylate (EGDMA) (70 / 10 / 20 molar ratio) copolymer particles (refractive index 1.51, average particle size 0.14 μm)

[0263] <Light Absorbing Material C>

[0264] Methyl methacrylate (MMA) / styrene (St) / ethylene glycol dimethacrylate (EGDMA) (70 / 10 / 20 molar ratio) copolymer particles (refractive index 1.51, average particle size 0.35 μm)

[0265] <Light absorbing material D>

[0266] Pentaerythritol tetrabenzoate (molecular weight 552)

[0267] <Light Absorbing Material E>

[0268] Methyl methacrylate (MMA) / styrene (St) / ethylene glycol dimethacrylate (EGDMA) (70 / 10 / 20 molar ratio) copolymer particles (refractive index 1.51, average particle size 0.3 μm)

[0269] <Light absorbing material F>

[0270] Water-based urethane resin (Super Flex 210 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)

[0271] <Light Absorbing Material G>

[0272] Urethane acrylate (UA-1100 manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0273] Isocyanuric acid EO modified diacrylate and triacrylate

[0274] <Light absorbing material H>

[0275] (Meth) acrylic resin (MMA / N-phenylmaleimide / 2-ethylhexyl methacrylate polymer, Mw 800000)

[0276] <Light Absorbing Material I>

[0277] Pentaerythritol tetrabenzoate (molecular weight 552)

[0278] When the absorption coefficient of light of wavelength 9.0 to 11.0 μm of light absorbing materials A to I was measured by ATR method, it was 4.0×10 -3 ~6.0×10 -3 / μm.

[0279] 2. Preparation of optical films

[0280] <Example 1>

[0281] (Preparation of substrate film)

[0282] The resins in Table 2 and 2% by mass of the additives based on the resins were melt-kneaded and mixed using a single-screw extruder ( The obtained film was melt-extruded from a coat-hanger T-die (width 150 mm) and stretched while being transported to prepare a substrate film (substrate layer) with a thickness of 50 μm.

[0283] (Surface formation)

[0284] First, SUPER FLEX 210 (aqueous urethane resin, light absorbing material F) manufactured by Daiichi Kogyo Seiyaku Co., Ltd., adipic acid as a curing agent, and epoxy resin were dissolved in pure water to obtain a curable composition having a SUPER FLEX 210 concentration of 10% by mass.

[0285] Next, the prepared curable composition was applied onto the surface of the obtained substrate film using an extrusion coater and dried at 80°C for 5 minutes to form a surface layer with a thickness of 0.2 μm. Thus, an optical film having a two-layer structure of substrate film (substrate layer) / surface layer was obtained.

[0286] <Example 2>

[0287] (Preparation of substrate film)

[0288] In the same manner as in Example 1, a substrate film (substrate layer) having a thickness of 50 μm was obtained.

[0289] (Surface formation)

[0290] First, the following materials were stirred and mixed, and then filtered through a polypropylene filter having a pore size of 0.4 μm to prepare a curable composition.

[0291] Urethane acrylate (UA-1100 manufactured by Shin-Nakamura Chemical Co., Ltd.): 12% by mass

[0292] Isocyanuric acid EO-modified diacrylate and triacrylate (M-315 manufactured by Toagosei Co., Ltd.): 8% by mass (the above is light absorbing material G)

[0293] Silica fine particle dispersion (V-8804 manufactured by JGC Catalysts & Chemicals Co., Ltd.): 60 parts by mass

[0294] IRGACURE 184 (manufactured by BASF Japan): 2.4% by mass

[0295] KF-351A (polyether-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd.) 0.4 mass%

[0296] Methanol 18 mass%

[0297] Propylene glycol monomethyl ether acetate (PGME): 12 mass%

[0298] Next, the prepared curable composition was applied to the surface of the substrate film using an extrusion coater, dried at 80° C., and then nitrogen was blown to form an atmosphere with an oxygen concentration of 1.0% by volume or less. At the same time, an ultraviolet lamp was used with an illumination of 100 mW / cm 2 , irradiation 0.2J / cm 2The film was cured by ultraviolet irradiation under the conditions of , and a surface layer with a thickness of 0.5 μm was formed. Thus, an optical film having a two-layer structure of base film / surface layer was obtained.

[0299] <Example 3>

[0300] (Preparation of particles for substrate layer)

[0301] COP1 and the light absorbing material A were mixed using a vacuum NAUTA mixer so that the content of the light absorbing material A was 0.5 mass %, dried, and then melted using a biaxial extruder to obtain pellets of a resin mixture.

[0302] (Preparation of Surface Layer Particles)

[0303] Pellets of the resin mixture were obtained in the same manner as above except that the light absorbing material H ((meth)acrylic resin) was used.

[0304] (Co-casting)

[0305] The obtained substrate layer particles and surface layer particles are respectively supplied to two twin-shaft extruders under a nitrogen atmosphere to be melted and co-cast. That is, a co-extrusion die is used to melt co-cast in a manner such that the substrate layer is the center and the surface layer is located on both sides thereof. The set temperature of the twin-shaft extruder is all set to 180°C, and the co-extrusion die is set to 190°C. The co-extrusion die is a hanger-type 3-layer laminated multi-manifold die. Then, the melt-extruded film is sandwiched and formed between a cooling roller and an elastic contact roller, and then cooled with a cooling roller, and then peeled off with a stripping roller to obtain an optical film with a 2-layer structure of a substrate layer / surface layer.

[0306] <Examples 4 to 17 and Comparative Example 1>

[0307] Except having changed the composition and thickness of the base layer and the surface layer as shown in Table 2, it carried out similarly to Example 3, and obtained the optical film which has the three-layer structure of surface layer / base layer / surface layer.

[0308] <Example 18>

[0309] (Preparation of light absorbing material additive solution)

[0310] 95 parts by mass of dichloromethane were placed in a sealed container, and 5 parts by mass of light absorbing material B ((meth)acrylic polymer particles) were added while stirring. Then, the mixture was stirred and mixed for 50 minutes using a dissolver. 2000 g of the obtained mixed solution was passed through a high-pressure dispersion device (trade name: ultra-high pressure homogenizer M110-E / H, manufactured by Microfluidics Corporation) and treated once at 175 MPa to prepare a light absorbing material dispersion. This was filtered using FINEMET NF manufactured by Nippon Seisen Co., Ltd. to prepare a light absorbing material additive solution.

[0311] (Preparation of dopant for surface layer)

[0312] The following dopant was prepared. First, dichloromethane and ethanol were added to a pressure dissolving tank. COP6 (cycloolefin resin) and the light absorbing material additive solution (light absorbing material) were added while stirring, heated, and completely dissolved while stirring. The mixture was filtered with Anzai filter paper No. 244 manufactured by Anzai Filter Paper Co., Ltd. to prepare a dopant.

[0313] Dichloromethane: 300 parts by mass

[0314] Ethanol: 19 parts by mass

[0315] COP6 (cycloolefin resin): 100 parts by mass

[0316] Light absorbing material additive solution (light absorbing material B): 75 parts by mass

[0317] (Preparation of dopant for substrate layer)

[0318] In the preparation of the dopant, the dopant is prepared in the same manner except that the light absorbing material additive liquid is not added.

[0319] (Film Making)

[0320] Then, the surface layer dopant and the substrate layer dopant were uniformly co-cast on a stainless steel belt support at a temperature of 33° C. and a width of 1500 mm using an endless belt casting device. The temperature of the stainless steel belt was controlled at 30° C. After the solvent was evaporated until the residual solvent content in the dopant co-cast on the stainless steel belt support was 30% by mass, it was peeled off from the stainless steel belt support at a peeling tension of 130 N / m.

[0321] The cast film obtained by peeling was stretched at 160°C (Tg of the resin - 10°C) at a stretching ratio of 50% in the width direction (TD direction). The residual solvent at the start of stretching was 10% by mass. Then, it was dried at 130°C while being conveyed in a drying area with multiple rollers. Then, it was wound up to obtain an optical film having a three-layer structure of surface layer / substrate layer / surface layer.

[0322] <Examples 19 to 21>

[0323] Except having changed the composition of a base material layer and a surface layer as shown in Table 2, it carried out similarly to Example 18, and obtained the optical film.

[0324] <Examples 22 to 26, Comparative Example 10>

[0325] Except that the types and thicknesses of the light absorbing materials of the substrate layer and the surface layer were changed as shown in Table 3, an optical film having a three-layer structure of surface layer / substrate layer / surface layer was obtained in the same manner as in Example 4.

[0326] <Comparative Examples 2 to 4>

[0327] An optical film was obtained in the same manner as in Production Examples 3, 4, and 7 of International Publication No. 2018 / 139638.

[0328] <Comparative Example 5>

[0329] An optical film was obtained in the same manner as in Example 4 of International Publication No. 2015 / 098956.

[0330] <Comparative Example 6>

[0331] An optical film (single-layer film) was obtained in the same manner as in Example 12 except that the content of the light absorbing material E in the base material layer was changed as shown in Table 3 and the surface layer was not formed.

[0332] <Comparative Example 7>

[0333] Except having changed the content of the light absorbing material B as shown in Table 3, it carried out similarly to the comparative example 6, and obtained the optical film (single layer film).

[0334] <Comparative Example 8>

[0335] The thermoplastic resin (J0) used in Manufacturing Example 1 of International Publication No. 2018 / 139638 was dried at 100°C for 5 hours. The dried thermoplastic resin (J0) was supplied to an extruder and melted in the extruder. The molten thermoplastic resin (J0) was extruded from a T-die in a sheet form onto a casting drum through a polymer tube and a polymer filter. The extruded thermoplastic resin (J0) was cooled to obtain a pre-stretched substrate having a thickness of 70 μm. The obtained substrate was stretched to 1.4 times to obtain an optical film having a thickness of 50 μm.

[0336] <Comparative Example 9>

[0337] On the optical film of Comparative Example 8, a curable composition similar to the curable composition of Example 2 was applied except that the light absorbing material was not included, followed by drying and curing to form a surface layer, thereby obtaining an optical film.

[0338] <Evaluation>

[0339] The absorption coefficient and the presence or absence of bleed-out of the obtained optical film were evaluated by the following method. The bleed-out was evaluated only for some Examples and Comparative Examples.

[0340] (1) Absorption coefficient ratio (As / Ac)

[0341] 1) First, using a micro-FTIR (UMA600 and FTS3000 manufactured by Agilent), the ATR method was used with an incident light diameter of 100 μm, a Ge prism (incident angle 45°), a detector of MCT-A, and a resolution of 4.0 cm -1 , cumulative: 64 times, the infrared absorption spectrum was measured. Based on the infrared absorption spectrum obtained, the portion corresponding to a wavelength of 9.6 μm (frequency 1041 cm -1 ) to obtain the absorbance A of the entire optical film.

[0342] 2) Next, 30% of the thickness is cut from one surface a of the optical film, and the absorbance A1 of the cut surface is measured in the same manner as in 1).

[0343] 3) Furthermore, 30% of the thickness is cut from the other surface b of the optical film, and the absorbance A2 of the cut surface is measured in the same manner as in 1).

[0344] 4) The absorbances A, A1 and A2 obtained in 1) to 3) above are applied to the following formula to calculate the absorption coefficient As of the surface layer region and the absorption coefficient Ac of the inner layer region, respectively.

[0345] Surface absorption coefficient As = (A-A1) × loge10 ÷ (0.3T)

[0346] Internal absorption coefficient Ac = A2 × loge10 ÷ (0.4T)

[0347] (T: thickness of optical film

[0348] A: Absorbance of optical film

[0349] A1: Absorbance measured by cutting 30% of the thickness T of the optical film from one surface 10a of the optical film

[0350] A2: absorbance measured by cutting 30% of the thickness T of the optical film from the other side surface 10b of the optical film)

[0351] (2) Exudation

[0352] The obtained film was placed in a high temperature thermo at 90°C and a wet heat thermo at 80°C and 90%RH for 3000 hours. The film was taken out at any time and observed for surface precipitates. The observation was carried out in a dark room under green light.

[0353] In addition, the time required for the precipitate to be observed is shown in Tables 2 and 3.

[0354] Furthermore, a polarizer and a display device were prepared using the obtained optical film. Then, the polarizing plate quality and light leakage were evaluated by the following methods.

[0355] (3) Polarizer evaluation (polarizer quality)

[0356] (Preparation of polarizer)

[0357] A PVA resin film having a degree of polymerization of 2400, a saponification degree of 99.7 mol % and a thickness of 75 μm was prepared. The film was stretched 3 times in the film conveying direction while being dyed in an iodine aqueous solution at 30°C, and then stretched in a 4 mass % boric acid, 5 mass % potassium iodide aqueous solution at 60°C so that the total stretching ratio was 6 times the original length. In addition, the stretched film was immersed in a 2 mass % potassium iodide aqueous solution at 30°C for several seconds to be washed. The obtained stretched film was dried at 90°C to obtain a polarizer.

[0358] (Preparation of polarizing plate)

[0359] A polarizer is bonded to the surface layer (or light absorbing layer) of the optical film with an adhesive, and a PET film is bonded to the back layer with an adhesive to produce a polarizing plate.

[0360] (Laser shearing properties)

[0361] The obtained polarizer was irradiated with a carbon dioxide gas laser with a wavelength of 9.6 μm on the optical film to shear the polarizer. The shearing conditions were a frequency of 20 kHz, an output of 59 W, and a speed of 60 m / min. The surface vicinity of the shearing length of 10 cm was confirmed by a microscope and evaluated.

[0362] S: Completely free of dirt and coal

[0363] A: Dirt and coal are only slightly observed in the shearing part

[0364] B: Dirt and coal are slightly observed around the shearing part

[0365] C: Dirt and soot are more obvious, but can be cleaned

[0366] ×: Severe dirt and soot, unusable

[0367] If it is C or higher, it is judged to be good.

[0368] (4) Evaluation of display device (light leakage)

[0369] First, the polarizer previously attached to the Hitachi liquid crystal display device Wooo W32L-H90 as an IPS type liquid crystal display device was carefully peeled off. Then, the polarizer cut by laser was attached so that the transmission axis of the polarizer originally attached was consistent with that of the liquid crystal display device to prepare the liquid crystal display device. The polarizer cut by laser was attached so that the optical film of the present invention was on the liquid crystal cell side.

[0370] Then, the obtained liquid crystal display device was observed with naked eyes in a dark room in a state of full black display, and light leakage at the edge was evaluated by 10 persons.

[0371] SS: 10 people can't see any light leakage at all

[0372] S: 1 in 10 people observed weak light leakage

[0373] A: 2-3 out of 10 people observed weak light leakage

[0374] B: 4 to 6 out of 10 people observed weak light leakage

[0375] C: 7 out of 10 people observed weak light leakage. No problem in practical use.

[0376] ×: 10 people observed strong light leakage

[0377] If it is C or higher, it is judged to be good.

[0378] Table 2 shows the compositions and evaluation results of the optical films of Examples 1 to 21, and Table 3 shows the compositions and evaluation results of the optical films of Examples 22 to 26 and Comparative Examples 1 to 10.

[0379]

[0380]

[0381] As shown in Tables 2 and 3, the optical films of Examples 1 to 26 with the absorption coefficient ratio As / Ac adjusted to 1.1 to 20 have good laser shear properties and excellent polarizing plate quality (less contamination). In addition, the obtained display device has no light leakage.

[0382] In contrast, the optical films of Comparative Examples 1 to 3 and 6 to 8, in which the absorption coefficient ratio As / Ac was less than 1.1, had poor laser shearing properties and poor polarizer quality. On the other hand, the optical films of Comparative Examples 4, 5, 9 and 10, in which As / Sc exceeded 20, were found to cause light leakage in display devices.

[0383] This application claims priority based on Japanese Patent Application No. 2020-128426 filed on July 29, 2020. The contents described in the specification and drawings of that application are incorporated herein by reference in their entirety.

[0384] Industrial Applicability

[0385] According to the present invention, an optical film, a polarizing plate, and a liquid crystal display device capable of improving laser shearing properties without causing light leakage in a display device can be provided.

[0386] Explanation of symbols

[0387] 10Optical film

[0388] 11 Base material layer

[0389] 12, 13 surface

[0390] 20 Polarizing filter

[0391] 30Other optical films

[0392] 40 bonding layers

[0393] 100 polarizers

[0394] 200 Layers

[0395] Sa, Sb surface area

[0396] C inner area

[0397] L Laser

Claims

1. An optical film comprising a cycloolefin resin, wherein: When the area from one side of the optical film to a depth of 30% of the thickness of the optical film is defined as a surface area Sa, the area from the other side of the optical film to a depth of 30% of the thickness of the optical film is defined as a surface area Sb, and the area between the surface area Sa and the surface area Sb is defined as an inner area C, The ratio As / Ac of the absorption coefficient As of the light with a wavelength of 9.6 μm measured by the ATR method in the surface layer region Sa to the absorption coefficient Ac of the light with a wavelength of 9.6 μm measured by the ATR method in the inner layer region C is 1.1 to 17.3, The absorption coefficient of the optical film for light with a wavelength of 9.6 μm is 1.5×10 -5 / μm or more 58×10 -5 / μm or less.

2. The optical film according to claim 1, wherein The ratio As / Ac is 3-15.

3. The optical film according to claim 1 or 2, wherein: The surface region Sa and the inner region C each contain a light absorption coefficient of 4.0×10 -3 / μm or more light absorbing material.

4. The optical film according to claim 3, wherein: The content Ms of the light absorbing material in the surface layer region Sa is greater than the content Mc of the light absorbing material in the inner layer region C.

5. The optical film according to claim 4, wherein: Ms / Mc is 2.5~20.

6. The optical film according to claim 3, comprising: a substrate layer comprising a cycloolefin resin and the light absorbing material; and a surface layer which is laminated on at least one surface of the base layer and contains a cycloolefin resin and the light absorbing material or contains a (meth) acrylic resin as the light absorbing material; The content of the light absorbing material Ms' in the surface layer is greater than the content Mc' of the light absorbing material in the base layer.

7. The optical film according to claim 6, wherein: Ms' / Mc' is 2.5~50.

8. The optical film according to claim 3, comprising: a substrate layer comprising the cycloolefin resin and the light absorbing material; and a surface layer which is laminated on at least one surface of the base layer and is composed of a cured product of a curable composition containing a curing agent and a curable compound as the light absorbing material; The curable compound is a urethane compound having a group reactive with a curing agent.

9. The optical film according to claim 8, wherein: The light absorbing material includes an ester compound or (meth)acrylic polymer particles.

10. The optical film according to claim 9, wherein: The light absorbing material is a sugar ester compound.

11. A polarizing plate, comprising: Polarizer, and The optical film according to any one of claims 1 to 10 disposed on at least one surface of the polarizer.

12. The polarizing plate according to claim 11, wherein The surface included in the surface layer region Sa of the optical film is bonded to the polarizer.

13. A liquid crystal display device comprising: Liquid crystal unit, and a first polarizing plate and a second polarizing plate sandwiching the liquid crystal cell, At least one of the first polarizing plate and the second polarizing plate is the polarizing plate according to claim 11 or 12.

Citation Information

Patent Citations

  • Multilayer film, polarization plate, and multilayer film production method

    WO2015098956A1

  • Display device

    WO2018139638A1

  • Adhesive film

    CN103597046A

  • Optical film, circularly polarizing plate, and image display device

    CN104136947A

  • Optical film

    CN106661247A