A visual card and a method for manufacturing the same
By hollowing out an opaque substrate and covering it with a transparent film for high-temperature lamination, the problems of poor color printing and insufficient abrasion resistance for video cards are solved, achieving high-quality transparent layer window flatness and a cost-effective manufacturing process.
Patent Information
- Application Number
- CN202111422338.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-11-26
AI Technical Summary
When existing video cards are made of transparent materials, the printing color is poor and the wear resistance is insufficient, and the hollow part is easily deformed during the high-temperature lamination process, causing the display window to be uneven and affecting product quality.
Use an opaque base material for hollow processing and cover its surface with a transparent film. Through high-temperature lamination, the card base with a low softening point fills the hollow window to ensure the flatness of the transparent layer window. At the same time, transparent glue is used to bond the laminated card base. , electronic components and middle layer card base to form a high-quality video card.
It improves the wear resistance of the video card and the flatness of the transparent layer window, improves product quality, and reduces costs through hot pressing, which has better manufacturing effects than cold pressing.
Smart Images

Figure CN116176053B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of card production, and in particular to a visual card and a manufacturing method thereof. Background Art
[0002] In the prior art, the visual card has a display area, and the display area requires transparency and visibility, so the surface is printed with transparent materials. Since it is a transparent material, a part of the color inside the product can be revealed, so the product cannot achieve the required printing color well. In addition, although the transparent varnish printed on the surface of the transparent material can increase the wear resistance of the product, the effect is not ideal. After that, a technical solution for producing the visual card using an opaque material was invented, but in the process of using the opaque material for production, new problems will occur, that is, the visual card has a display area, and the display area requires transparency and visibility, so it is necessary to hollow out the display window on the opaque printing layer, and the hollowed-out card base needs to be laminated with a transparent film on the surface at high temperature, but the temperature is high during the high temperature lamination process, resulting in the transparent layer of the hollowed-out part being wrinkled and deformed, and finally resulting in the display window being uneven, and the transparency is not good, which affects the quality of the visual card. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a visual card and a manufacturing method thereof.
[0004] In a first aspect, an embodiment of the present invention provides a method for manufacturing a visual card, comprising:
[0005] Step S1: hollowing out a window at a preset position of an opaque substrate to obtain a first pressure-bearing card base;
[0006] Step S2: a transparent film is coated on the front surface of the first pressure-bearing card base, a card base with a low Vicat softening point is padded on the back surface of the first pressure-bearing card base, and then high-temperature lamination is started. During the high-temperature lamination process, the card base with a low Vicat softening point is softened and filled into the hollowed-out window on the first pressure-bearing card base to obtain a first laminated card base, and the first laminated card base is used as the front card base after lamination; the first pressure-bearing card base and the transparent film coated on the front surface are not fused with the card base with a low Vicat softening point padded on the back surface;
[0007] Step S3: using another opaque substrate as a second pressure-bearing card base, laminating the front surface of the second pressure-bearing card base, and performing high-temperature lamination to obtain a laminated back surface card base;
[0008] Step S4: align the laminated front card base, the electronic components, the middle layer card base with the hollow area and the laminated back card base up and down, and glue them together with transparent glue to obtain a visual card.
[0009] In a second aspect, an embodiment of the present invention provides a visual card, which comprises from top to bottom: a laminated front card base, an intermediate layer card base and a laminated back card base, the intermediate layer card base is provided with a hollow area, and an electronic component is provided in the hollow area on the intermediate layer card base, the laminated front card base comprises an opaque substrate with a hollow window and a transparent film covering the front surface of the opaque substrate, the laminated back card base comprises an opaque substrate and a film covering the front surface of the opaque substrate, the laminated front card base, the intermediate layer card base, the electronic component and the laminated back card base are placed in sequence up and down and bonded together by transparent glue.
[0010] Compared with the prior art, the present invention has the following advantages:
[0011] The technical solution of the present invention adopts an opaque material and hollows out a window at a preset position to obtain a first pressure-bearing card base, and a transparent film is coated on the front surface of the first pressure-bearing card base, thereby increasing the wear resistance of the product; the card base with a low Vicat softening point, the first pressure-bearing card base and the transparent film coated on the front surface are subjected to high-temperature lamination, and during the high-temperature and high-pressure lamination process, the card base with a low Vicat softening point is melted first, and the hollowed-out window on the first pressure-bearing card base is filled, thereby ensuring the flatness of the transparent layer window and improving the quality of the visual card. The present invention adopts a hot pressing method, which is more effective and less costly in manufacturing visual cards than a cold pressing method. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 A flow chart of a method for manufacturing a visual card provided in Embodiment 1 of the present invention;
[0013] Figure 2 A flow chart of a method for manufacturing a visual card provided in Embodiment 2 of the present invention;
[0014] Figure 3 This is a schematic structural diagram of the first pressure-bearing card base in Example 2;
[0015] Figure 4 It is a schematic diagram of a part of the structure of the first pressure-bearing card base in the second embodiment for manufacturing a single visual card;
[0016] Figure 5 It is a cross-sectional schematic diagram of a first pressure-bearing card base for making a single visual card in the second embodiment;
[0017] Figure 6 It is a cross-sectional schematic diagram of aligning the adhesive film, the first pressure-bearing card base, and the PE film in the upper and lower parts for making a single visual card in step 102-1 in the second embodiment;
[0018] Figure 7 is a cross-sectional schematic diagram of a card base after the first lamination for making a single visual card in step 102-2 in the second embodiment;
[0019] Figure 8 It is a cross-sectional schematic diagram of the front card base after lamination for making a single visual card in step 102-3 in the second embodiment;
[0020] Fig. 9 It is a cross-sectional schematic diagram of a laminated front card base with a protective layer for making a single visual card in step 102-4 in the second embodiment;
[0021] Fig.10 It is a cross-sectional schematic diagram of aligning the adhesive film and the second pressure-bearing card base in the upper and lower parts for making a single visual card in step 103-2 in the second embodiment;
[0022] Fig.11 It is a cross-sectional schematic diagram of the back side card base after lamination for making a single visual card in step 103-3 in the second embodiment;
[0023] Fig.12 It is a cross-sectional schematic diagram of the laminated reverse card base with a protective layer for making a single visual card in step 103-4 in Example 2;
[0024] Fig.13 This is a schematic structural diagram of the intermediate layer card base without electronic components placed in step 104-2 in the second embodiment;
[0025] Fig.14 This is a schematic structural diagram of the intermediate layer card base on which the electronic components are placed in step 104-2 in the second embodiment;
[0026] Fig.15 It is a structural schematic diagram of an intermediate layer card base without electronic components placed thereon for making a single visual card in step 104-2 in the second embodiment;
[0027] Fig.16 It is a schematic structural diagram of an intermediate layer card base with electronic components placed thereon for making a single visual card in step 104-2 in the second embodiment;
[0028] Fig.17 It is a cross-sectional schematic diagram of aligning the laminated front card base with a protective layer, the electronic component, the middle layer card base and the laminated back card base with a protective layer up and down for making a single visual card in step 105 of the second embodiment;
[0029] Fig.18 is a cross-sectional schematic diagram of the finished visual card obtained in step 106 in Example 2;
[0030] Fig.19 is a cross-sectional schematic diagram of another finished visual card obtained in step 106 in embodiment 2;
[0031] Fig. 20 A cross-sectional schematic diagram of a visual card provided in Embodiment 3 of the present invention;
[0032] Fig.21 A cross-sectional schematic diagram of another visual card having a card base with a low Vicat softening point provided in Example 3 of the present invention;
[0033] Fig. 22 A cross-sectional schematic diagram of a visual card in which the screen of a display screen and a hollow window are aligned in another electronic assembly provided in Embodiment 3 of the present invention;
[0034] Fig.23 Another cross-sectional schematic diagram of a visual card provided in Example 3 of the present invention having a card base with a low Vicat softening point, in which the screen of the display screen in the electronic component is aligned with the hollow window, and the transparent film in the front card base after lamination and the film in the back card base after lamination are both provided with adhesive films. DETAILED DESCRIPTION
[0035] The present application proposes a visual card and a method for manufacturing the same. The specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be interpreted as limiting the present application.
[0036] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with those in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as here.
[0037] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention are further described in detail below with reference to the accompanying drawings.
[0038] Embodiment 1
[0039] Embodiment 1 of the present invention provides a method for manufacturing a visual card, such as Figure 1 As shown, including:
[0040] Step S1: hollowing out a window at a preset position of an opaque substrate to obtain a first pressure-bearing card base;
[0041] Optionally, before the window is hollowed out, the process further includes: printing a coating on the front surface of the opaque substrate; the process used for printing the coating can be: offset printing, silk screen printing, digital printing, etc., and the pattern can be customized;
[0042] Further, the ink is printed on the front surface of the opaque substrate to form a printed coating.
[0043] Step S2: a transparent film is coated on the front surface of the first pressure-bearing card base, and a card base with a low Vicat softening point is padded on the back surface, and then high-temperature lamination is started. During the high-temperature lamination process, the card base with a low Vicat softening point is softened and then filled into the hollowed-out window on the first pressure-bearing card base to obtain a first laminated card base, and the first laminated card base is used as the front card base after lamination;
[0044] Specifically, in this embodiment, the first pressure-bearing card base and the transparent film covering the front surface are not fused with the card base with a low Vicat softening point of the back pad;
[0045] Optionally, in this embodiment, the first laminated card base is used as the laminated front card base, comprising: tearing off the card base with a low Vicat softening point on the reverse side of the first laminated card base to obtain an integrated laminated front card base; the card base with a low Vicat softening point can preferably use a PE film;
[0046] Optionally, if there is a coating in the first laminated card base, the softening point of the coating is higher than the softening point of the card base of the reverse pad of the first pressure-bearing card base;
[0047] In this embodiment, the softening point refers to the softening point of the material. temperature ; Mainly refers to Amorphous The temperature at which a polymer begins to soften. The Vicat softening point is the temperature at which a 1 mm2 needle is pressed into the sample by 1 mm in a specific liquid heat transfer medium under a certain load and a certain constant temperature increase; this temperature reflects the expected softening point when a material is used in a heating device.
[0048] Specifically, in this embodiment, the side of the first pressure-bearing card base exposed outward is the front side, and the side facing inward is the back side;
[0049] Preferably, the material of the card base with a low Vicat softening point in this embodiment is a material that does not adhere to the first pressure-bearing card base during high-temperature lamination, preferably a PE film (i.e., PE protective layer, the full name in English is: Polyethylene, which is a high molecular organic compound with the simplest structure, and the PE protective layer uses a special polyethylene (PE) plastic film as a base material);
[0050] In this embodiment, the material of the transparent film coated on the front surface of the first pressure-bearing card base in this step can be PVC, PET, PETG, PE, PC, etc. The transparent film can be a film with adhesive or without adhesive film, that is, the front surface of the first pressure-bearing card base is coated with an adhesive film or without adhesive film; in this embodiment, an adhesive film is preferably used; the thickness of the transparent film is ≤0.05 mm, and preferably a transparent film with a thickness of 0.04-0.05 mm is used;
[0051] Optionally, in this embodiment, a protective layer is covered on the front surface of the front card base after lamination, specifically: the protective layer is arranged on the front surface of the front card base after lamination, and the protective layer and the front card base after lamination are integrated into one body by heat pressing or bonding, and the protective layer is used to protect the front surface of the front card base after lamination (i.e., the front surface of the product) from scratches and contamination during the production process;
[0052] Step S3: using another opaque substrate as a second pressure-bearing card base, laminating the front surface of the second pressure-bearing card base, and performing high-temperature lamination to obtain a laminated back surface card base;
[0053] Optionally, in step S3, using another opaque substrate as the second pressure-bearing card base includes: printing a coating on the front surface of another opaque substrate as the second pressure-bearing card base; the process used for printing the coating can be: offset printing, silk screen printing, digital printing, etc., and the pattern can be customized;
[0054] Furthermore, ink is printed on the front surface of another opaque substrate to generate a printed coating, and the opaque substrate with the printed coating is used as a second pressure-bearing card base.
[0055] Optionally, in this embodiment, a protective layer is covered on the front surface of the back card base after lamination, specifically: the protective layer is arranged on the front surface of the back card base after lamination, and the protective layer and the back card base after lamination are integrated into one body by heat pressing or bonding; the protective layer is used to protect the front surface of the back card base after lamination (i.e., the back of the product) from scratches and contamination during the production process;
[0056] In this embodiment, the front surface of the second pressure-bearing card base is coated with a film, specifically: the front surface of the second pressure-bearing card base is coated with a transparent film or an opaque film;
[0057] Furthermore, the front surface of the second pressure-bearing card base is coated with an adhesive film or without an adhesive film, preferably with an adhesive film;
[0058] Optionally, in this embodiment, there is no order in the manufacturing process of the front card base after lamination and the back card base after lamination, that is, the order of step S1, step S2 and step S3 can be swapped;
[0059] Step S4: Align the laminated front card base, the electronic components, the middle layer card base with the hollow area, and the laminated back card base up and down, and glue them together with transparent glue to obtain a visual card;
[0060] In this embodiment, if the obtained visual card has a protective layer on the front and / or back, then after step S4, the method further includes: tearing off the protective layer;
[0061] Optionally, in this embodiment, using transparent glue to bond together to obtain a visual card includes: using transparent glue to bond together to obtain a whole block of material, and cutting the whole block of material to obtain multiple visual cards;
[0062] Optionally, in this embodiment, the whole block of material is cut into a plurality of visual cards by engraving or punching.
[0063] The thickness of the visual card produced by the method of this embodiment is no more than 0.84 mm, preferably 0.68-0.84 mm.
[0064] If the front surface and / or the back surface of the whole block of material is covered with a protective layer in this embodiment, the protective layer needs to be torn off before or after cutting the whole block of material.
[0065] Optionally, before step S4 in this embodiment, the method further includes: hollowing out an area on the intermediate card base for placing electronic components. The electronic components include: a display screen or a solar cell panel.
[0066] The technical solution of the present invention adopts an opaque material and hollows out a window at a preset position to obtain a first pressure-bearing card base, and a transparent film is coated on the front surface of the first pressure-bearing card base, thereby increasing the wear resistance of the product; the card base with a low Vicat softening point, the first pressure-bearing card base and the transparent film coated on the front surface are subjected to high-temperature lamination, and during the high-temperature and high-pressure lamination process, the card base with a low Vicat softening point is melted first, and the hollowed-out window on the first pressure-bearing card base is filled, thereby ensuring the flatness of the transparent layer window and improving the quality of the visual card. The present invention adopts a hot pressing method, which is more effective and less costly in manufacturing visual cards than a cold pressing method.
[0067] Embodiment 2
[0068] Embodiment 2 of the present invention provides a method for manufacturing a visual card, such as Figure 2 As shown, including:
[0069] Step 101: Printing ink on the front surface of an opaque substrate to generate a printed coating, and hollowing out windows at preset positions of the opaque substrate to obtain a first pressure-bearing card base;
[0070] like Figure 3 , which is a schematic diagram of the structure of the first pressure-bearing card base in this embodiment, Figure 4 This is a schematic diagram of a portion of the structure of the first pressure-bearing card base used for making a single visual card in this embodiment;
[0071] Specifically, step 101 includes:
[0072] Step 101-1, selecting a corresponding opaque substrate according to product requirements;
[0073] In this embodiment, the material of the opaque substrate can be: PVC, PET, PETG, PE, PC, etc., preferably PVC and PET, and the color of the opaque substrate can be selected from various colors, preferably white;
[0074] Step 101 - 2 , printing ink on the front surface of the opaque substrate to generate a printed coating, and hollowing out windows at preset positions to obtain a first pressure-bearing card base.
[0075] Optionally, in this embodiment, the hollowed-out window can be punched, cut, engraved, or lasered; one or more windows can be hollowed out at a preset position to obtain the first pressure-bearing card base; the shape of the window can be square, rectangular, elliptical, circular, etc.; the size and position of the window can be customized; Figure 5 FIG. 1 is a cross-sectional schematic diagram of a first pressure-bearing card base for making a single visual card in this embodiment;
[0076] Step 102: The front surface of the first pressure-bearing card base is covered with a tape film, and the back surface is padded with a PE film, and then high-temperature lamination is started. During high-temperature lamination, the PE film will soften. After the PE film softens, the window is filled to obtain a first laminated card base, and the PE film on the back side of the first laminated card base is torn off to obtain an integrated laminated front card base, and a protective layer is covered on the front surface of the laminated front card base, and then low-temperature hot pressing is performed;
[0077] In this embodiment, the front surface of the front card base is covered with a protective layer after lamination and then subjected to low-temperature hot pressing at a temperature lower than the temperature of high-temperature lamination;
[0078] The thickness of the adhesive film used in this embodiment does not exceed 0.05 mm, preferably 0.04-0.05 mm; the thicker the PE film, the better;
[0079] Specifically, in this embodiment, step 102 includes:
[0080] Step 102-1, the adhesive film is arranged on the front side of the first pressure-bearing card base, and the PE film is arranged on the back side of the first pressure-bearing card base, and the adhesive film, the first pressure-bearing card base and the PE film are aligned and placed up and down;
[0081] In this embodiment, the cross-sectional schematic diagram of aligning the adhesive film, the first pressure-bearing card base, and the PE film in the upper and lower parts for making a single visual card is shown as follows: Figure 6 As shown;
[0082] Step 102-2, start high-temperature lamination of the aligned adhesive film, the first pressure-bearing card base, and the PE film; during high-temperature lamination, the PE film will soften, and after the PE film softens, it fills the window on the first pressure-bearing card base to obtain an integrated first laminated card base,
[0083] In this embodiment, after high-temperature lamination, the adhesive film covering the front surface of the first pressure-bearing card base is flat and wrinkle-free; Figure 7 , which is a cross-sectional schematic diagram of a card base after first lamination for making a single visual card in this embodiment;
[0084] Step 102-3, tearing off the PE film on the back side of the card base after the first lamination to obtain an integrated front side card base after lamination;
[0085] like Figure 8 , which is a cross-sectional schematic diagram of a laminated front card base for making a single visual card in this embodiment;
[0086] Step 102-4, providing a protective layer on the front surface of the front card base after lamination;
[0087] In this embodiment, the protective layer is used to prevent the front surface of the card base from being scratched, stained, or contaminated during the production process; Fig. 9 , which is a cross-sectional schematic diagram of a laminated front card base with a protective layer for making a single visual card in this embodiment;
[0088] Step 103: printing ink on the front surface of another opaque substrate to generate a printed coating to obtain a second pressure-bearing card base, coating the front surface of the second pressure-bearing card base with a tape film, laminating at high temperature to obtain a laminated back card base, and covering the front surface of the laminated back card base with a protective layer;
[0089] Specifically, in this embodiment, step 103 includes:
[0090] Step 103-1, according to product requirements, select a corresponding opaque substrate, print ink on the front surface of the opaque substrate to generate a printed coating to obtain a second pressure-bearing card base;
[0091] In this embodiment, the material of the opaque substrate can be: PVC, PET, PETG, PE, PC, etc., preferably PVC and PET, and the color of the opaque substrate can be selected from various colors, preferably white;
[0092] Step 103-2, applying an adhesive film to the front surface of the second pressure-bearing card base, and aligning the adhesive film and the second pressure-bearing card base up and down;
[0093] In this embodiment, the cross-sectional schematic diagram of aligning the adhesive film and the second pressure-bearing card base up and down for making a single visual card is shown as follows: Fig.10 As shown;
[0094] Step 103-3, laminating the aligned adhesive film and the second pressure-bearing card base at high temperature to obtain an integrated laminated back card base;
[0095] like Fig.11 , which is a cross-sectional schematic diagram of the back card base after lamination for making a single visual card in this embodiment;
[0096] Step 103-4, after lamination, the front surface of the back card base is covered with a protective layer;
[0097] In this embodiment, the protective layer is used to protect the front surface of the back card base after lamination from being scratched, stained, or contaminated during the production process; Fig.12 , which is a cross-sectional schematic diagram of a laminated reverse card base with a protective layer for making a single visual card in this embodiment;
[0098] Step 104: hollowing out the middle layer card base to place electronic components;
[0099] Step 104-1, according to product requirements, select a corresponding substrate as the intermediate layer card base;
[0100] In this embodiment, the material of the substrate selected in this step can be: PVC, PET, PETG, PE, PC, etc., and the color is not limited, and both transparent and opaque are acceptable. Preferably, a white PVC card base is used as the middle layer card base;
[0101] Step 104-2, hollowing out an area for placing electronic components on the middle layer card base;
[0102] Optionally, in this embodiment, the processes that can be used to hollow out the area for placing the electronic components on the card base include: punching, dull cutting, engraving, laser, etc.; the shape, size, and size of the hollowed-out area can be adjusted according to the structure of the electronic component, and the electronic component needs to be completely placed in the card base; after step 104-2, the structures of the intermediate layer card base without the electronic component and with the electronic component placed are respectively Fig.13 and Fig.14 As shown, the structures of the intermediate layer card base without electronic components and with electronic components placed thereon for making a single visual card are respectively Fig.15 and Fig.16 As shown;
[0103] Step 105: Align the laminated front card base with a protective layer, the electronic components, the middle layer card base, and the laminated back card base with a protective layer up and down, and glue them together with transparent glue to obtain a whole large piece;
[0104] In this embodiment, a cross-sectional schematic diagram of the laminated front card base with a protective layer, the electronic components, the middle layer card base and the laminated back card base with a protective layer aligned vertically for making a single visual card is shown in FIG. Fig.17 As shown;
[0105] Step 106: cutting the bonded whole piece of material and tearing off the protective layers on the two outer surfaces to obtain a plurality of visual cards;
[0106] Optionally, the operation of tearing off the protective layer on the front surface in this step can also be performed before cutting the entire large piece of material;
[0107] In this embodiment, the cutting of the bonded whole block can be performed by carving or punching. The visual card size can be a standard card size or a customized special-shaped card size. The thickness of the visual card is 0.76±0.08 mm. Fig.18 FIG. 1 is a schematic cross-sectional view of the visual card manufactured in this embodiment.
[0108] Optionally, in this embodiment, the PE film on the back of the card base after the first lamination in step 102 may not be torn off, and the visual card cross-section obtained after step 106 is as follows: Fig.19 shown.
[0109] Optionally, the electronic assembly in this embodiment may also include a solar cell panel. Fig.18 and Fig.19 The solar panels that collect solar energy can also be placed in the screen position of the electronic components.
[0110] The technical solution of the present invention adopts an opaque material for printing, which has good hiding power and will not show the color inside the product, so as to better meet the requirements of printing color; in addition, the front surface is covered with a transparent adhesive film to increase the wear resistance of the product; the PE film with a Vicat softening point lower than the printed coating card base, the printed coating on the first pressure-bearing card base and the adhesive film are laminated at high temperature. During the high temperature and high pressure lamination process, the PE film melts first to fill the window position on the printed coating card base, thereby ensuring the flatness of the transparent layer window and improving the quality of the visual card. In this embodiment, a hot pressing method is adopted, which is more effective and less costly in manufacturing visual cards than a cold pressing method. The method of this embodiment discloses a process of making a whole block of large material, and then finally cutting the whole block of large material to obtain multiple visual cards, so as to achieve batch production and improve the efficiency of manufacturing visual cards.
[0111] Embodiment 3
[0112] Embodiment 3 of the present invention provides a visual card obtained by using the manufacturing method provided in the above embodiment, such as Fig. 20 As shown, the visual card comprises from top to bottom: a laminated front card base, an intermediate card base and a laminated back card base, the intermediate card base is provided with a hollow area, and an electronic component is provided in the hollow area on the intermediate card base, the laminated front card base comprises an opaque substrate with a hollow window and a transparent film covered on the front surface of the opaque substrate, the laminated back card base comprises an opaque substrate and a film covered on the front surface of the opaque substrate, and the laminated front card base, the intermediate card base, the electronic component and the laminated back card base are bonded together by transparent glue.
[0113] Optionally, the laminated front card base of the visual card of this embodiment may also include a card base with a low Vicat softening point, such as Fig.21 As shown, the card base with low Vicat softening point is arranged between the opaque substrate with hollow windows and the middle layer card base, and the card base with low Vicat softening point fills the hollow windows; preferably, the card base with low Vicat softening point is a PE film. The opaque substrate and the transparent film on the front surface in this embodiment are not fused with the card base with low Vicat softening point on the back surface;
[0114] In this embodiment, the two outer surfaces of the visual card are referred to as the front surfaces of the opaque substrate (i.e., the side exposed to the outside);
[0115] Optionally, the laminated front card base of the visual card in this embodiment further includes a printed coating, which is disposed between the opaque substrate with the hollow window and the transparent film covering the front surface of the opaque substrate;
[0116] And / or, after lamination, the reverse card base further comprises a printed coating layer, which is disposed between the opaque substrate and the film covering the front surface of the opaque substrate.
[0117] Optionally, the transparent film in this embodiment may be a film with adhesive or without adhesive. If it is a transparent film, the thickness is ≤ 0.05 mm, preferably, the thickness of the transparent film is 0.04-0.05 mm;
[0118] Optionally, the electronic component in this embodiment includes a display screen or a solar panel;
[0119] Furthermore, the hollow window is aligned with the screen of the display screen or the solar panel in the electronic component, such as Fig. 22 As shown, the screen of the display screen is taken as an example.
[0120] Optionally, the film on the front surface of the opaque substrate in the reverse card base after lamination is a transparent film or an opaque film;
[0121] Furthermore, after lamination, the transparent film on the front surface of the opaque substrate in the back card base is with or without an adhesive film.
[0122] For example, the front card base of the visual card in this embodiment includes a card base with a low Vicat softening point after lamination, and the screen of the display screen in the electronic component is aligned with the hollow window position, and the transparent film in the front card base after lamination and the film in the back card base after lamination are both adhesive films, then the cross-sectional view of the visual card is as follows: Fig.23 shown.
[0123] Compared with the visual card in the prior art, the visual card provided by this embodiment is more wear-resistant, has a smoother transparent layer window, and is of higher quality.
[0124] Although the present application is described herein in conjunction with various embodiments, in the process of implementing the claimed application, those skilled in the art may understand and implement other variations of the disclosed embodiments by viewing the drawings, the disclosure, and the appended claims. In the claims, the word "comprising" does not exclude other components or steps, and "one" or "an" does not exclude multiple situations. A single processor or other unit may implement several functions listed in a claim. Certain measures are recorded in different dependent claims, but this does not mean that these measures cannot be combined to produce good results.
[0125] Although the present application has been described in conjunction with specific features and embodiments thereof, it is obvious that various modifications and combinations may be made thereto without departing from the spirit and scope of the present application. Accordingly, this specification and the drawings are merely exemplary illustrations of the present application as defined by the appended claims, and are deemed to have covered any and all modifications, variations, combinations or equivalents within the scope of the present application. Obviously, those skilled in the art may make various modifications and variations to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.
Claims
1. A method for manufacturing a visual card, characterized in that: include: Step S1: hollowing out a window at a preset position of an opaque substrate to obtain a first pressure-bearing card base; Step S2: a transparent film is coated on the front surface of the first pressure-bearing card base, a card base with a low Vicat softening point is padded on the back surface of the first pressure-bearing card base, and then high-temperature lamination is started. During the high-temperature lamination process, the card base with a low Vicat softening point is softened and filled into the hollowed-out window on the first pressure-bearing card base to obtain a first laminated card base, and the first laminated card base is used as the front card base after lamination; the first pressure-bearing card base and the transparent film coated on the front surface are not fused with the card base with a low Vicat softening point padded on the back surface; Step S3: using another opaque substrate as a second pressure-bearing card base, laminating the front surface of the second pressure-bearing card base, and performing high-temperature lamination to obtain a laminated back surface card base; Step S4: aligning the laminated front card base, the electronic components, the middle layer card base with the hollow area and the laminated back card base up and down, and gluing them together with transparent glue to obtain a visual card; Before step S3, the method further includes: hollowing out an area on the intermediate layer card base for placing electronic components.
2. The method according to claim 1, characterized in that Before hollowing out a window at a preset position of an opaque substrate, the method further includes: printing a coating on the front surface of the opaque substrate, wherein the softening point of the printed coating is higher than the softening point of the card base of the reverse pad of the first pressure-bearing card base.
3. The method according to claim 2, characterized in that The step of printing a coating on the front surface of the opaque substrate specifically comprises: printing ink on the front surface of the opaque substrate to generate a printed coating.
4. The method according to claim 1, characterized in that The transparent film is coated on the front surface of the first pressure-bearing card base, specifically: the front surface of the first pressure-bearing card base is coated with an adhesive film or without an adhesive film.
5. The method according to claim 1, characterized in that The step S2 further comprises: covering the front surface of the front card base with a protective layer after the lamination.
6. The method according to claim 5, characterized in that The protective layer is covered on the front surface of the laminated front card base, specifically: the protective layer is arranged on the front side of the laminated front card base, and the protective layer and the laminated front card base are integrated into one by heat pressing or bonding.
7. The method according to claim 1, characterized in that In the step S3, using another opaque substrate as the second pressure-bearing card base includes: printing a coating on the front surface of another opaque substrate as the second pressure-bearing card base.
8. The method according to claim 7, characterized in that The coating printed on the front surface of another opaque substrate is used as the second pressure-bearing base, specifically: ink is printed on the front surface of another opaque substrate to generate a printed coating, and the opaque substrate with the printed coating is used as the second pressure-bearing base.
9. The method according to claim 1, characterized in that The step S3 further comprises: covering the front surface of the back card base with a protective layer after the lamination.
10. The method according to claim 9, characterized in that The protective layer is covered on the front surface of the laminated back card base, comprising: arranging the protective layer on the front surface of the laminated back card base, and integrating the protective layer and the laminated back card base into one by heat pressing or bonding.
11. The method according to claim 1, characterized in that The coating on the front surface of the second pressure-bearing card base specifically includes: coating the front surface of the second pressure-bearing card base with a transparent film or an opaque film.
12. The method according to claim 11, characterized in that The transparent film is coated on the front surface of the second pressure-bearing card base, specifically: the front surface of the second pressure-bearing card base is coated with an adhesive film or without an adhesive film.
13. The method according to claim 1, characterized in that The method of using transparent glue to bond together to obtain a visual card comprises: using transparent glue to bond together to obtain a whole block of material, and cutting the whole block of material to obtain a plurality of visual cards.
14. The method according to claim 5 or 9, characterized in that After obtaining the visual card, the method further comprises: tearing off the protective layer.
15. The method according to claim 13, characterized in that The step of cutting the whole block of material to obtain a plurality of visual cards comprises: cutting the whole block of material obtained by bonding by carving or punching to obtain a plurality of finished visual cards.
16. The method according to claim 1, wherein: The thickness of the transparent film is ≤0.05 mm.
17. The method according to claim 1, wherein: The step S2 of using the first laminated card base as a laminated front card base includes: tearing off the card base with a low Vicat softening point on the reverse side of the first laminated card base to obtain an integrated laminated front card base.
18. The method of claim 1, wherein: The electronic components include display screens or solar panels.
19. The method according to claim 1, wherein: The card base with low Vicat softening point is a PE film.
20. A visual card manufactured according to the method of claim 1, characterized in that: The visual card comprises from top to bottom: a laminated front card base, an intermediate layer card base and a laminated back card base, the intermediate layer card base is provided with a hollow area, and an electronic component is provided in the hollow area on the intermediate layer card base, the laminated front card base comprises an opaque substrate with a hollow window and a transparent film covered on the front surface of the opaque substrate, the laminated back card base comprises an opaque substrate and a film covered on the front surface of the opaque substrate, and the laminated front card base, the intermediate layer card base, the electronic component and the laminated back card base are bonded together by transparent glue.
21. The visual card of claim 20, wherein: After lamination, the front card base also includes a card base with a low Vicat softening point, which is arranged between the opaque substrate with a hollow window and the middle layer card base, and the card base with a low Vicat softening point fills the hollow window; the opaque substrate and the transparent film covered on the front surface are not fused with the card base with a low Vicat softening point on the back pad.
22. A visual card as claimed in claim 20 or 21, characterized in that The laminated front card base further comprises a printed coating, which is arranged between the opaque substrate with the hollow window and the transparent film covering the front surface of the opaque substrate; And / or, the laminated back-side card base further comprises a printed coating layer disposed between the opaque substrate and the film covering the front surface of the opaque substrate.
23. A visual card as claimed in claim 20 or 21, characterized in that The transparent film is a film with adhesive or a film without adhesive.
24. A visual card as claimed in claim 20 or 21, characterized in that The electronic components include display screens or solar panels.
25. The visual card of claim 24, wherein: The hollow window is aligned with the screen of the display screen or the solar cell panel in the electronic component.
26. The visual card of claim 20 or 21, wherein: The thickness of the transparent film is ≤0.05 mm.
27. The visual card according to claim 20 or 21, wherein the film on the front surface of the opaque substrate in the reverse card base after lamination is a transparent film or an opaque film.
28. The visual card of claim 27, wherein the transparent film on the front surface of the opaque substrate in the back card base after lamination is an adhesive film or a non-adhesive film.
29. The visual card of claim 21, wherein: The card base with low Vicat softening point is a PE film.