A magnesium-zirconium bimetallic modified resin, its preparation method and use for defluorination

By precipitating magnesium-zirconium metal oxide nanoparticles in macroporous strong alkaline resin to form magnesium-zirconium bimetallic modified resin, the problems of insufficient adsorption capacity of single-metal modified resin and narrow pH range of bimetallic-modified resin are solved. It has high-efficiency fluoride removal effect and anti-interference ability in a wide pH range, and is suitable for the treatment of fluorine pollution in neutral water bodies.

CN116272910BActive Publication Date: 2024-10-18SOUTHEAST UNIV
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202310503172.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-10-18
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

Existing monometallic modified resins have limited adsorption capacity and insufficient anti-interference ability in removing fluoride. Most bimetallic modified resins have a narrow pH applicable range and cannot effectively treat fluorine pollution in neutral water bodies.

Method used

Magnesium-zirconium bimetallic modified resin is used to precipitate magnesium and zirconium metal oxide nanoparticles in a macroporous strong alkaline anion exchange resin, and adjust the quaternary ammonium group to Cl type to form a magnesium-zirconium bimetallic modified resin, which is used to treat materials containing Fluorine wastewater, achieving high adsorption capacity and interference resistance in a wide pH range.

Benefits of technology

In water bodies with a pH range of 2 to 8, the adsorption capacity of fluoride ions is significantly improved, and the anti-interference ability is improved. The material is easy to operate, has low production cost, and has good regeneration performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272910B_ABST
    Figure CN116272910B_ABST
Patent Text Reader

Abstract

The present invention relates to a magnesium-zirconium bimetallic modified resin, a preparation method thereof and a defluorination application thereof. The material is made of resin as a raw material, magnesium chloride hexahydrate and zirconium oxychloride octahydrate as modification reagents, and metal Mg and Zr are precipitated in the resin pores in the form of Mg / Zr metal oxide nanoparticles. The precursor concentration of the metal ions is 0.5-1.5 mol / L, and Mg:Zr=1:3-3:1. The obtained magnesium-zirconium bimetallic modified resin can be used to remove fluorine from water. Compared with unmodified resin and single metal modified resin, the magnesium-zirconium bimetallic modified resin exhibits higher adsorption capacity and anti-interference in the pH range of 2-8, fast adsorption rate, good reproducibility, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a magnesium-zirconium bimetallic modified resin defluorination material and a preparation method and application thereof, belonging to the technical field of adsorption materials. Background Art

[0002] Fluorine (F) is one of the main elements that constitute organisms in the earth system and participate in the metabolic process. At the same time, F, like typical pollutants such as P and As, is also a major anionic pollutant in water. In recent years, with the large-scale application of fluorine-containing products, such as polytetrafluoroethylene plastics and fluorine-containing pesticides, surface water and groundwater have been seriously polluted. At present, high-fluorine groundwater is distributed in 27 provinces, municipalities, and autonomous regions across the country, especially in the arid and semi-arid areas of North China and Northwest China. Studies have shown that excessive fluoride intake has a certain degree of toxicity to human DNA, proteins, etc., which can cause poor tooth quality and osteoporosis, and even cause oral cancer, brain damage, Alzheimer's disease, etc. my country's "Sanitary Standard for Drinking Water" (GB5049-2006) stipulates that the fluoride concentration of centralized water supply is below 1 mg / L; my country's "Groundwater Quality Standard" (GB / T14848-2017) clearly stipulates that the fluoride concentration of Class I to III water is below 1 mg / L. For many years, the control of water pollution caused by fluoride has been a common concern of the world.

[0003] At present, the methods for removing fluoride from water bodies mainly include precipitation, electrochemical method, membrane separation method and adsorption method. Among them, adsorption method has great potential for fluoride removal due to its advantages of high cost-effectiveness, convenient operation, strong removal capacity and recyclable adsorbent. At present, various types of adsorbents have been developed to adsorb and remove fluoride ions from water, including natural mineral and industrial waste adsorbents, biomass adsorbents, metal (hydr)oxide adsorbents, carbon-based adsorbents, ion exchange resins, etc. Among them, ion exchange resins have broad application prospects due to their low price and good recyclability. However, using ion exchange resins alone to remove fluoride from water bodies will result in disadvantages such as small adsorption capacity, poor selectivity and low anti-interference ability. Therefore, it is usually necessary to physically or chemically modify the resin to improve its fluoride removal capacity. At present, metal loading modification of resin is one of the most effective chemical modification methods. Usually, metal ions or metal (hydr)oxides that can interact with fluoride ions are introduced into the resin, so that the resin composite material has a strong binding ability of metal ions, metal (hydr)oxides and fluoride ions while ensuring the original performance advantages.

[0004] To date, most metal-modified resin materials are single-metal modified materials, including aluminum-modified resins (Millar GJ, Couperthwaite SJ, Wellner DB, et al. Removal of fluoride ionsfrom solutionby chelating resin with imino-diacetate functionality[J]. Journal of waterprocess engineering, 2017, 20: 113-122.), zirconium-modified resins (Shin E, Dreisinger DB, Burns A D. Removal of fluoride from sodium sulfate brinebyzirconium pre-loaded chelating resins with amino-methyl phosphonic acidfunctionality[J]. Desalination, 2021, 505: 114985.), and lanthanum-modified resins (Robshaw T, Tukra S, Hammond DB, et al. Highly efficient fluoride extraction from simulant leachate of spent potlining via La-loadedchelating resin. Anequilibrium study[J]. Journal of hazardous materials, 2019,361: 200-209.) etc.However, single metal modified resins generally have disadvantages such as small adsorption capacity and narrow pH application range. Bimetallic modified resins can effectively overcome the defects of single metal modified resins, such as titanium zirconium bimetallic modified resin (Chen JK, Nie GZ, Liu Z Y, et al. Performance of polymer-based titanium and zirconiumoxides composite adsorbent for simultaneous removal of phosphorus and fluorine from water[J]. Huanjing Kexue, 2017, 38(5): 1947-1956.), lanthanum zirconium bimetallic modified resin (Du Y, Wang X, Nie G, et al. Enhanced phosphate removal by using La-Zr binarymetaloxide nanoparticles confined in millimeter-sized anion exchanger[J]. Journal of Colloid and Interface Science, 2020, 580: 234-244.) These bimetallic modified resins can not only maintain the performance advantages of the original resins, but also give play to the synergistic effect of bimetals to further improve the defluorination performance of the materials. However, most bimetallic modified resins only have an improvement in adsorption capacity, and the defluorination effect in neutral water is not good. At present, there are relatively few studies on the defluorination performance of bimetallic modified resins in neutral water.

[0005] Literature search shows that, so far, there are no reports on magnesium-zirconium bimetallic modified resin defluorination adsorbent materials. Generally speaking, magnesium-modified adsorbents alone have better defluoridation effects at pH 5-8, but their adsorption capacity is relatively low (He Zhili, He Zhixia, Chen Ruiqin. Adsorption performance of modified activated carbon for fluoride ions in aqueous solution [J]. Journal of Wuhan Institute of Technology, 2012, 34 (1): 43-47.). Zirconium-modified adsorbents alone have better defluoridation effects at pH 3, but it is difficult to fully play a role in defluoridation in water bodies with a neutral pH (Pan B, Xu J, Wu B, et al. Enhanced removal of fluoride by polystyrene anion exchanger supported hydrous zirconium oxide nanoparticles [J]. Environmental science & technology, 2013, 47 (16): 9347-9354.). In addition, single metal modified resins or unmodified resins often have limited anti-interference effects, and show a trend of significantly reduced adsorption in the presence of coexisting anions and high coexisting organic matter content. Moreover, most bimetallic modified resins have a narrow pH range of application. Summary of the invention

[0006] Technical problem: The current large-scale application of fluorine-containing products has led to serious pollution of surface water and groundwater in various regions across the country, and even affected the safety of human life and property. The monometallic modified resin has limited adsorption capacity in fluorine removal, the anti-interference ability needs to be improved, and most bimetallic modified resins have a narrow pH application range. The present invention provides a magnesium-zirconium bimetallic modified resin, its preparation method and defluorination use. The magnesium-zirconium bimetallic modified resin is prepared using resin as a raw material and magnesium chloride hexahydrate and zirconium oxychloride octahydrate as modification reagents. The material preparation method is simple, the operation is easy, and the production cost is low. The magnesium-zirconium bimetallic modified resin synthesized by the method of the present invention is used for the treatment of fluorine-containing wastewater, which not only achieves higher adsorption capacity and anti-interference in a wider pH range, but also has a fast adsorption rate and good reproducibility, and has broad application prospects.

[0007] Technical solution:

[0008] A magnesium-zirconium bimetallic modified resin defluorination material, magnesium ions and zirconium ions are precipitated in the macroporous strong alkaline anion exchange resin in the form of Mg / Zr metal oxide nanoparticles or Mg / Zr metal hydroxide nanoparticles, and the quaternary ammonium group in the resin is Cl type. The adsorption amount of fluoride ions in a solution with a fluoride ion concentration of 20 mg / L and pH=7 can reach 12.7 mg / L.

[0009] The magnesium-zirconium bimetallic modified resin defluorination material is used for defluorination in neutral water.

[0010] A method for preparing a magnesium-zirconium bimetallic modified resin defluorination material comprises the following steps:

[0011] 1) Resin pretreatment: Take the resin, wash it with hydrochloric acid, and then rinse it repeatedly with distilled water until the eluent is neutral; after washing and filtering, place it in a Soxhlet extractor and extract it with anhydrous ethanol to remove excess impurities; then dry it in an oven at 323 K for 12 h; the dried resin is stored in a dry container for later use.

[0012] The resin is a macroporous strongly basic anion exchange resin, including D213, D201, D202 and the like.

[0013] ) Prepare Mg and Zr precursor solutions: dissolve ZrOCl2·8H2O (zirconium oxychloride octahydrate) and MgCl2·6H2O (magnesium chloride hexahydrate) in a mixture of hydrochloric acid solution and anhydrous ethanol to obtain a precursor solution of metal ions. Precursor concentration = 0.5-1.5 mol / L, Mg:Zr = 1:3-3:1.

[0014] Here, the precursor concentration is the sum of the concentrations of Mg and Zr ions;

[0015] The molar ratio of Mg to Zr is a different ratio obtained by adjusting within the above-mentioned range of total ion concentration.

[0016] ) Adsorption of metal ions: slowly add the pretreated resin obtained in step 1) into the mixed salt solution of step 2), put it into a constant temperature oscillator for oscillation, so that the metal Mg and Zr enter the resin pores, and obtain a resin carrying two metal ions, which is filtered for use. The constant temperature oscillation time is 12~24h, the rotation speed is 180 r / min, and the temperature is 303~323K.

[0017] 4) Precipitation of metal ions: Add the resin carrying two metal ions obtained in step 3) into the NaOH solution, place it in a constant temperature oscillator and stir it for 24 hours, so that the metal Mg and Zr are precipitated in the resin pores in the form of Mg / Zr metal (hydr) oxide nanoparticles, and then rinse it repeatedly with distilled water until the eluent is neutral. The constant temperature oscillation time is 12~24 hours, the rotation speed is 180 r / min, and the temperature is 303~323K.

[0018] ) Group conversion: Take the resin with precipitated Mg / Zr metal oxide obtained in step 4), put it into NaCl solution and oscillate it at constant temperature for 4-8 hours to transform the quaternary ammonium group in the resin into Cl type, rinse it with distilled water until the eluent is neutral, and dry it in an oven at constant temperature to obtain a magnesium-zirconium bimetallic modified resin composite adsorbent.

[0019] ) Regeneration: After the adsorption reaction, the magnesium-zirconium bimetallic modified resin composite adsorbent is regenerated with a binary salt-alkali mixture of NaOH and NaCl (both 5%) and recycled to reduce the processing cost.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0021] 1. The present invention provides a magnesium-zirconium bimetallic modified resin defluorination material, which can give play to the synergistic effect of two metals and has a high fluorine adsorption capacity in a wide pH range, thus overcoming the shortcomings of low adsorption capacity of magnesium-modified resin alone and narrow pH application range of zirconium-modified resin alone.

[0022] 2. Compared with magnesium or zirconium modified resin alone, the adsorption capacity of the magnesium-zirconium bimetallic modified resin adsorption material of the present invention is increased by 40-200%, and the application range is expanded to pH=2-8. The adsorption amount of fluoride ions in a solution with a fluoride ion concentration of 20 mg / L and pH=7 can reach 12.7 mg / L, which effectively improves its adsorption and defluorination performance and application range. It is also simple to operate, the raw materials are easily available, and the production cost is low.

[0023] 3. Compared with the unmodified resin, the magnesium-zirconium bimetallic modified resin overcomes its limited anti-interference effect and exhibits a higher fluorine adsorption capacity in the presence of coexisting anions and high levels of coexisting organic matter. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the defluorination mechanism of the magnesium-zirconium bimetallic modified resin defluorination material of the present invention in water. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the embodiments. It should be noted that the specific embodiments described herein are only used to explain the present invention and do not limit the scope and application of the present invention.

[0026] Embodiment 1:

[0027] A method for preparing a magnesium-zirconium bimetallic modified resin defluorination material comprises the following steps:

[0028] (1) Prepare a mixed solution of Zr and Mg salts:

[0029] Take 150mL of hydrochloric acid solution and 50mL of anhydrous ethanol, place them in a 500mL conical flask and mix them thoroughly.

[0030] 13.56 g of magnesium chloride hexahydrate and 42.97 g of zirconium oxychloride octahydrate were weighed as metal precursors (precursor concentration = 1 mol / L, Mg:Zr = 1:2), placed in the above solution, and stirred evenly to obtain a hydrochloric acid ethanol solution of Zr and Mg salts.

[0031] (2) Adsorption of metal ions: Weigh 10 g of pretreated D213 resin and add it to the solution obtained in step (1). Place it in a constant temperature oscillator and keep stirring at 323K for 24 h to obtain a resin carrying two metal ions. Filter it for later use.

[0032] (3) Precipitation of metal ions: Add the resin obtained in step (2) to 200 mL of NaOH solution, continue to place it in a constant temperature oscillator and keep it at 323K and continue stirring for 24 hours to allow the metal precursor to precipitate as Mg / Zr metal oxide nanoparticles in the resin pores. Filter out the resin in the above solution and then rinse it repeatedly with distilled water until the eluent is neutral.

[0033] (4) The resin on which the Mg / Zr metal oxide nanoparticles were precipitated obtained in step (3) was placed in 200 mL of NaCl solution and oscillated at a constant temperature for 4 h to transform into the Cl type. The resin in the above solution was filtered out and rinsed with distilled water until the eluent was neutral. The washed resin was placed in an oven at 323K and dried at a constant temperature for 12 h to obtain a magnesium-zirconium bimetallic modified resin composite adsorbent.

[0034] Embodiment 2:

[0035] The difference from Example 1 is that in step (1), 30.51 g of magnesium chloride hexahydrate and 16.11 g of zirconium oxychloride octahydrate are weighed as metal precursors, and the precursor concentration is 1 mol / L; Mg:Zr=3:1.

[0036] Embodiment 3:

[0037] The difference from Example 1 is that in step (1), 10.17 g of magnesium chloride hexahydrate and 48.33 g of zirconium oxychloride octahydrate are weighed as metal precursors, the precursor concentration is 1 mol / L, and Mg:Zr=1:3.

[0038] Embodiment 4:

[0039] The difference from Example 1 is that in step (1), 6.78 g of magnesium chloride hexahydrate and 21.49 g of zirconium oxychloride octahydrate are weighed as metal precursors, the precursor concentration is 0.5 mol / L, and Mg:Zr=1:2.

[0040] Embodiment 5:

[0041] The difference from Example 1 is that in step (1), 20.34 g of magnesium chloride hexahydrate and 64.47 g of zirconium oxychloride octahydrate are weighed as metal precursors, the precursor concentration is 1.5 mol / L, and Mg:Zr=1:2.

[0042] Comparative Example 1:

[0043] A method for preparing a magnesium-modified resin defluorination material, which is different from Example 1 in that in step (1), magnesium chloride hexahydrate is used as a metal precursor, and 40.68 g of magnesium chloride hexahydrate (precursor concentration = 1 mol / L) is weighed to obtain a magnesium-modified resin adsorbent.

[0044] Comparative Example 2:

[0045] A method for preparing a zirconium-modified resin defluorination material, which is different from Example 1 in that in step (1), zirconium oxychloride octahydrate is used as a metal precursor, and 64.46 g of zirconium oxychloride octahydrate (precursor concentration = 1 mol / L) is weighed to obtain a zirconium-modified resin adsorbent.

[0046] Comparative Example 3:

[0047] 0.025 g unmodified resin D213.

[0048] Embodiment 6:

[0049] Investigation of adsorption capacity of modified resin

[0050] (1) Effect of metal precursor concentration and metal ratio: Weigh 0.025 g of the magnesium-zirconium bimetallic modified resin obtained in Examples 1-5, the magnesium-modified resin obtained in Comparative Examples 1 and 2, and the zirconium-modified resin, respectively, and place them in 50 mL of a NaF solution with a pH of 7 and a fluoride ion concentration of 20 mg / L. Shake and adsorb them in a conical flask at 25°C for 24 hours, and measure the fluorine adsorption amount. The adsorption capacity of the modified resin for fluoride ions is shown in Table 1:

[0051] Table 1

[0052]

[0053] In Examples 1-5, the concentration of the metal precursor solution and the molar ratio of Mg and Zr ions were changed to obtain metal-modified resins carrying different metal contents. It can be seen that different carrying amounts have a great influence on the adsorption capacity of the modified resin for fluoride ions. The adsorption capacity reaches the highest when the precursor concentration is 1 mol / L and Mg:Zr=1:2. Above or below this condition, the adsorption capacity decreases.

[0054] (2) Investigation of adsorption behavior of modified resin in solutions with different pH values: Weigh 0.025 g of magnesium-zirconium bimetallic modified resin obtained in Example 1, and place them in 50 mL of NaF solution with a fluoride ion concentration of 20 mg / L at pH=2, 3, 4, 5, 6, 7, 8, 9, and 10, respectively. Shake and adsorb at 25°C in a conical flask for 24 hours, and measure the fluorine adsorption capacity of magnesium-zirconium bimetallic modified resin. The adsorption capacity of magnesium-zirconium bimetallic modified resin for fluoride ions obtained by testing is 17.4, 22.5, 15.2, 14.4, 13.9, 12.7, 12.1, 9.5, and 5.3 mg / L, respectively. It can be seen that the application range of magnesium-zirconium bimetallic modified resin adsorption material of the present invention is broadened to pH=2~8, and the adsorption capacity of fluoride ions in a solution with a fluoride ion concentration of 20 mg / L and pH=7 can reach 12.7 mg / L.

[0055] (3) Investigation of adsorption behavior of modified resin for different solutes: 0.025 g of magnesium-zirconium bimetallic modified resin obtained in Example 1 (unmodified resin was used in the comparative example) was weighed and placed in 50 mL of NaF solution with a pH of 7 and a fluoride ion concentration of 20 mg / L. The solution was shaken and adsorbed at 25°C in a conical flask for 24 h, and the fluorine adsorption amount of magnesium-zirconium bimetallic modified resin was measured. Different solutes were doped in the NaF solution, and the groups were set as follows. The results are shown in Table 2.

[0056] Group 1: F - =20 mg / L;

[0057] Group 2: F - =20 mg / L, HCO3 - =100 mg / L;

[0058] Group 3: F - =20 mg / L, humic acid=500 mg / ;

[0059] Comparative Example 1: Using unmodified resin, F - =20 mg / L, HCO3 - =100 mg / L;

[0060] Comparative Example 2: Using unmodified resin, F - =20 mg / L, humic acid = 500 mg / L.

[0061] Table 2

[0062]

[0063] (4) Resin regeneration: Collect the resin used in the adsorption performance test of Example 1, place it in a binary salt-alkali mixture of NaOH and NaCl (both 5%) for regeneration, and continue to place it in a constant temperature oscillator to maintain 323K stirring for 24 hours. Filter out the resin in the above solution and rinse it with distilled water until the eluent is neutral. Place the washed resin in a 323K oven and dry it at a constant temperature for 12 hours to obtain a regenerated magnesium-zirconium bimetallic modified resin composite adsorbent. Place it in 50 mL of NaF solution with a pH of 7 and a fluoride ion concentration of 20 mg / L, and oscillate and adsorb it at 25°C in a conical flask for 24 hours to measure the fluorine adsorption capacity of the magnesium-zirconium bimetallic modified resin.

[0064] After repeating the above steps for 5 cycles of adsorption and regeneration, the adsorption capacity of the magnesium-zirconium bimetallic modified resin for fluoride ions was 11.7 mg / L. Therefore, the magnesium-zirconium bimetallic modified resin defluorination material has good regeneration performance and can be reused after regeneration.

[0065] The technical solutions disclosed and proposed by the present invention have been described through examples, but the protection scope of this patent is not limited thereto. It should be pointed out that it is obvious for ordinary technicians in this technical field to make several improvements and modifications based on the technical solutions and patent concepts of this patent without departing from the content of this patent, and these improvements and modifications are regarded as the protection scope of this patent.

Claims

1. A magnesium-zirconium bimetallic modified resin, characterized in that: The magnesium ions and zirconium ions are precipitated in the form of Mg / Zr metal oxide nanoparticles in a macroporous strongly basic anion exchange resin, and the quaternary ammonium groups in the resin are of Cl type.

2. The magnesium-zirconium bimetallic modified resin according to claim 1 is used to remove fluorine from water, characterized in that: The application range is pH=2~8; In a solution with a fluoride ion concentration of 20 mg / L and pH=7, the adsorption amount of fluoride ions can reach 12.7 mg / L; The magnesium-zirconium bimetallic modified resin composite adsorbent that has undergone the defluorination process is regenerated with a binary salt-alkali mixture of 5% NaOH and 5% NaCl after the adsorption reaction.

3. The method for preparing a magnesium-zirconium bimetallic modified resin according to claim 1, characterized in that: The following steps are involved: 1) Pretreatment of resin: take the resin, wash it with hydrochloric acid, and then rinse it repeatedly with distilled water until the eluent is neutral; after washing and filtering, place it in a Soxhlet extractor and extract it with anhydrous ethanol to remove excess impurities; then dry it at a constant temperature; store the dried resin in a dry container for later use; the resin is a macroporous strong alkaline anion exchange resin selected from D213, D201 or D202; 2) Preparation of Mg and Zr precursor solutions: dissolving ZrOCl2·8H2O and MgCl2·6H2O in a mixture of hydrochloric acid solution and anhydrous ethanol to obtain a precursor solution of metal ions; The precursor concentration is 0.5~1.5mol / L, Mg:Zr=1:3~3:1; 3) Adsorption of metal ions: slowly add the pretreated resin obtained in step 1) into the precursor solution of step 2), put it into a constant temperature oscillator for oscillation, so that the metals Mg and Zr enter the resin pores, and obtain a resin carrying two metal ions, which is filtered for later use; the constant temperature oscillation time is 12~24h, the rotation speed is 180 r / min, and the temperature is 303~323K; 4) Precipitation of metal ions: Add the resin carrying two metal ions obtained in step 3) into a NaOH solution, place it in a constant temperature oscillator and stir it for 24 hours to precipitate metal Mg and Zr in the form of Mg / Zr metal oxide nanoparticles in the resin pores, and then take it out and rinse it repeatedly with distilled water until the eluent is neutral; 5) Group transformation: Take the resin with precipitated Mg / Zr metal oxide nanoparticles obtained in step 4), put it into a NaCl solution and oscillate it at a constant temperature for 4-8 hours to transform the quaternary ammonium group in the resin into Cl type, rinse it with distilled water until the eluent is neutral, and dry it in an oven at a constant temperature to obtain a magnesium-zirconium bimetallic modified resin composite adsorbent.

Citation Information

Patent Citations

  • Internally-coated porous WEBS with controlled positioning of modifiers therein

    CA2221168A1

  • Nonpolar adsorption resin for adsorbing organic compounds and regeneration method for nonpolar adsorption resin

    CN102861557A

  • Composite adsorbing material for removing fluorine ions in water and preparation method thereof

    CN102872812A

  • Resin base phosphorus removal absorbent and preparation method thereof

    CN102921386A

  • Method for preparing super absorbent resin

    CN106574006A