A sodium-embedded cobalt-manganese composite oxide and a sodium-embedded lithium-ion battery positive electrode material
Through wet sodium embedding technology, atomic-level embedding of sodium is achieved, which solves the problem of uneven sodium ion embedding in existing lithium-ion battery cathode materials, improves battery capacity and charge and discharge efficiency, and improves the overall performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202310304109.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-27
AI Technical Summary
The mixing method of sodium ions in existing lithium-ion battery cathode materials only reaches the granular level, resulting in low battery capacity and low charge and discharge efficiency, and it is difficult for sodium ions to be embedded in the transition metal layer in large quantities, affecting battery performance.
The wet sodium embedding scheme is used to chemically react between the cobalt-manganese metal compound precursor and the sodium source in the reactor. The reaction conditions are controlled to achieve atomic-level embedding of sodium, forming a sodium-embedded cobalt-manganese composite oxide and improving the uniformity of sodium. and the intercalation amount, increasing the layer spacing of the cathode material to facilitate the deintercalation of lithium ions.
Through atomic-level sodium embedding technology, the capacity and first charge and discharge efficiency of lithium-ion batteries are significantly improved, and the performance of energy storage batteries is improved.
Smart Images

Figure CN116282200B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium ion battery precursor preparation technology, in particular to a sodium-embedded cobalt-manganese composite oxide and a sodium-embedded lithium ion battery positive electrode material. Background Art
[0002] Lithium-ion batteries are currently the main energy storage devices, widely used in mobile phones, laptops, power tools, automobiles, aerospace and other fields. In order to make up for the shortcomings of lithium-ion batteries, doping lithium-ion batteries is currently a hot research topic.
[0003] Among them, multi-metal doping of lithium-ion batteries has made great progress. For example, CN114447309A discloses a sodium ion doped lithium ion battery positive electrode material, the chemical formula of the positive electrode material is Lix-yNayNizM1-zO2, wherein M is one or more of Mn, Mg, Ti, Al, and Co. The preparation method is as follows: S1, preparing a NaxNizM1-zO2 precursor: uniformly mixing a metal M source, a Ni source, and a sodium source, sintering, and cooling to obtain a precursor material NaxNizM1-zO2; S2, mixing the obtained NaxNizM1-zO2 precursor with a lithium source, and then performing molten salt ion exchange to obtain a bulk material; S3, washing the obtained bulk material, performing solid-liquid separation and drying to obtain a powder material; S4, heat-treating the obtained powder material to obtain a positive electrode material.
[0004] This method uses a metal M source, a Ni source and a sodium source to evenly mix and then sinter. This mechanical and physical mixing only achieves a mixing effect at the particle level, the elements are unevenly dispersed, and it is difficult for sodium ions to be embedded in the transition metal layer in large quantities. Therefore, the battery capacity and charge and discharge efficiency are low. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem of low gram capacity of existing lithium-ion batteries, and to provide a sodium-embedded cobalt-manganese composite oxide. A cobalt-manganese metal compound precursor is used to react with a sodium source in a reactor, so that sodium can be embedded in a hydroxide lattice through a chemical reaction, and the sodium is more uniform inside the material, reaching the atomic level; while the mixing of sodium in conventional sodium-embedded lithium battery positive electrode materials adopts mechanical and physical mixing, and the mixing effect only reaches the particle level; through the wet sodium embedding scheme, the sodium reactor is carried out in a wet reaction, the energy consumption is lower, and the sodium element in the product is more uniform.
[0006] Since the ionic radius of sodium ions is much larger than that of lithium ions, it is difficult for sodium ions to be embedded in the transition metal layer in large quantities during dry mechanical fusion. The use of wet method for atomic-level sodium embedding can increase the embedded sodium content. The embedding of sodium ions is beneficial to the expansion of the interlayer spacing of the positive electrode material and the deintercalation of lithium ions, thereby increasing the battery's gram capacity.
[0007] Furthermore, since the ionic radius of sodium ions is much larger than that of lithium ions, it is difficult for sodium ions to be embedded in the transition metal layer in large quantities during dry mechanical fusion. The use of wet method for atomic-level sodium embedding can increase the embedded sodium content. The embedding of sodium ions is beneficial to the expansion of the interlayer spacing of the positive electrode material and the deintercalation of lithium ions, thereby improving the initial charge and discharge efficiency of the material.
[0008] The specific plan is as follows:
[0009] A method for preparing a sodium-cobalt-manganese composite oxide comprises the following steps:
[0010] S1, obtaining a cobalt-manganese metal compound precursor;
[0011] S2, adding the precursor, sodium metal compound, water, additive and oxidant described in S1 into a reactor for reaction; controlling the reaction conditions of the reactor, including: the concentration of sodium ions in the reactor is 1 to 12 mol / L, the reaction temperature is 50 to 90° C., and the reaction time is 3 to 60 hours;
[0012] S3, adding a strong oxidant to the reaction material obtained in S2, wherein the oxidizing ability of the strong oxidant is higher than that of the oxidant in S2, and controlling the reaction conditions, including: the sodium ion concentration in the system is 3 to 6 mol / L, and the reaction temperature is 20 to 90° C., so that the sodium ions are embedded in the structure of the cobalt-manganese metal compound to form a composite metal oxide;
[0013] S4, performing solid-liquid separation on the reaction material obtained in S3, collecting the solid phase for heat treatment to obtain a sodium-cobalt-manganese intercalated composite oxide, wherein the sodium-cobalt-manganese intercalated composite oxide is a solid solution, and sodium ions replace the sites of cobalt and / or manganese.
[0014] Furthermore, the cobalt-manganese metal compound precursor in S1 includes at least one of cobalt hydroxide, manganese hydroxide, cobalt carbonate and manganese oxide. Preferably, the cobalt-manganese metal compound precursor is prepared by a coprecipitation crystallization method, specifically comprising: adding water, a complexing agent, a precipitant, optional additives and a mixed metal solution, conducting a coprecipitation crystallization reaction, and obtaining the cobalt-manganese metal compound precursor by solid-liquid separation.
[0015] Furthermore, the additive in S2 is selected from at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium, and molybdenum metal compounds. The role of the additive is to use high-valent or low-valent elements to generate electrons or holes, improve conductivity, stabilize the lattice structure, and improve the cycle stability of the material.
[0016] Preferably, the sodium metal compound in S2 is at least one of sodium hydroxide, sodium acetate, sodium nitrate, sodium sulfate, sodium bicarbonate, and sodium oxalate, preferably at least one of sodium hydroxide, sodium sulfate, and sodium carbonate, and more preferably sodium hydroxide.
[0017] Preferably, the oxidant in S2 is selected from at least one of oxygen, air and hydrogen peroxide, preferably hydrogen peroxide.
[0018] Furthermore, the reaction conditions in S2 include that the concentration of sodium ions in the reactor is 1 to 12 mol / L, preferably 3 to 10 mol / L, and more preferably 3 to 6 mol / L. A sodium ion concentration lower than 1 mol / L will make it difficult for the sodium element to form a solid phase.
[0019] Furthermore, the reaction conditions in S2 include a reaction temperature of 50-80° C., preferably 60-80° C. This is because the enthalpy of the reaction system is positive below 50° C., making it difficult to carry out the intended reaction, or the reaction speed is too slow to obtain an effective reaction result.
[0020] Based on the principle similar to the temperature condition, the reaction conditions also include a reaction pressure of 0.1 to 50 MPa, preferably 1 to 10 MPa, more preferably 1 to 5 MPa;
[0021] Preferably, the stirring intensity is 0.1 to 1.6 kw / m 2 h, preferably 0.5-1kw / m 2 h, more preferably 0.7 to 0.9 kw / m 2 ·h;
[0022] Preferably, the reaction time is 3 to 60 hours, preferably 5 to 40 hours, and more preferably 15 to 35 hours.
[0023] Furthermore, the strong oxidant in S3 is selected from at least one of oxygen, sodium chlorate, hydrogen peroxide, potassium permanganate and nitric acid. The oxidizing property of the strong oxidant in this step should be higher than that in step S2, so as to promote the sodium element to further enter the crystal structure.
[0024] Based on the principle similar to the aforementioned strong oxidant, the reaction conditions in S3 include: the sodium ion concentration is 3.5-5.5 mol / L, preferably 3.5-5 mol / L, and more preferably 3.5-4.5 mol / L.
[0025] Preferably, the reaction conditions in S3 also include a reaction pressure of 0.1 to 50 MPa, preferably 1 to 10 MPa, more preferably 1 to 5 MPa;
[0026] Preferably, the reaction conditions in S3 also include a reaction temperature of 40-90°C, preferably 50-80°C, more preferably 60-75°C;
[0027] Preferably, the reaction conditions in S3 also include a stirring intensity of 0.1 to 1.6 kw / m 2h, preferably 0.5-1kw / m 2 h, more preferably 0.7-0.9 kw / m 2 ·h.
[0028] Furthermore, the temperature of the heat treatment in S4 is 400-1000° C., preferably 500-900° C., and more preferably 650-800° C. Under such heat treatment conditions, the embedded sodium element can be stably retained in the material lattice.
[0029] Preferably, the heat treatment time is 3 to 36 hours, preferably 5 to 25 hours, and more preferably 10 to 20 hours.
[0030] The present invention also protects the sodium-cobalt-manganese composite oxide prepared by the preparation method of the sodium-cobalt-manganese composite oxide, wherein the chemical formula of the sodium-cobalt-manganese composite oxide is Na x Mn a Co b Me c O2, wherein 0≤x≤0.2, 0≤a≤1, 0≤b≤1, 0≤c≤0.2, wherein a+b+c=1, and Me is at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium, and molybdenum.
[0031] The present invention also protects a sodium-embedded lithium-ion battery positive electrode material, which is prepared by mixing and calcining the sodium-embedded cobalt-manganese composite oxide and a lithium source. The chemical formula of the sodium-embedded lithium-ion battery positive electrode material is Li x Na y Mn a Co b Me c O2, wherein 0.5≤x≤1.3, 0≤y≤0.2, 0≤a≤1, 0≤b≤1, 0≤c≤0.2, wherein a+b+c=1, and Me is at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium, and molybdenum metals.
[0032] Preferably, the lithium source is one or more of lithium carbonate, lithium hydroxide, and lithium acetate. The conditions for the mixed calcination include a temperature of 400-1000°C, preferably 600-1000°C, and more preferably 700-1000°C; a calcination time of 5-40h, preferably 5-25h, and more preferably 10-20h; and a calcination atmosphere of air or oxygen.
[0033] The present invention also protects a lithium ion battery, comprising the lithium ion battery positive electrode material.
[0034] Beneficial effects:
[0035] In the present invention, the concentration of sodium ions in the reactor is controlled to be 1-12 mol / L, the reaction temperature is controlled to be 20-90°C, and the reaction time is controlled to be 3-60 hours, so that the sodium ions can enter the hydroxide sites of cobalt and / or manganese to form a solid solution structure prototype, and under the action of a strong oxidant, the metal ion concentration in the system is controlled to be 3-6 mol / L, and the reaction temperature is controlled to be 20-90°C, the sodium further enters the hydroxide sites, thereby obtaining a composite metal oxide solid solution, and the structure is stable after heat treatment, a single diffraction peak is shown in the XRD spectrum, and the composite metal oxide is cobalt-manganese, and the embedded sodium element is not reflected in the XRD spectrum.
[0036] In the present invention, the sodium-embedded cobalt-manganese composite oxide prepared by a wet method is a sodium-embedded solid solution, which realizes atomic-level sodium element dispersion. It is mixed with a lithium source as a precursor and calcined to obtain a lithium-ion battery material with significant improvements in gram capacity and initial charge and discharge efficiency, which is conducive to the preparation of high-performance energy storage batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solution of the present invention, the accompanying drawings will be briefly introduced below. Obviously, the accompanying drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.
[0038] Figure 1 This is a scanning electron microscope image of the sodium-cobalt-manganese composite hydroxide provided in Example 1 of the present invention;
[0039] Figure 2 This is a scanning electron microscope image of a positive electrode material provided in Example 1 of the present invention;
[0040] Figure 3 This is a battery charge and discharge test result diagram provided by the present invention. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the examples, those without specifying specific techniques or conditions are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those without specifying the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially. In the following examples, if not clearly stated, "%" refers to weight percentage.
[0042] The test methods used below include: Battery charge and discharge test, the main conditions are as follows:
[0043] The positive electrode material, conductive carbon black and polyvinylidene fluoride (PVDF) were dissolved in NMP solvent at a mass ratio of 80:10:10 under vacuum to prepare a positive electrode slurry with a solid content of 70% by weight. The positive electrode slurry was coated on the current collector aluminum foil, dried at 120°C in vacuum for 12 hours, and punched to obtain a positive electrode disc with a diameter of 19 mm. Graphite, CMC and SBR were dissolved in deionized water at a mass ratio of 90:5:5 under vacuum to prepare a negative electrode slurry with a solid content of 40% by weight. The negative electrode slurry was coated on the current collector copper foil, dried at 100°C in vacuum for 12 hours, and punched to obtain a negative electrode disc with a diameter of 19 mm, and the negative electrode capacity: positive electrode capacity = 1.1:1. The battery assembly was carried out in a glove box filled with argon. The assembly order was positive electrode shell-positive electrode sheet-diaphragm-negative electrode sheet-stainless steel sheet-spring sheet-negative electrode shell. The electrolyte was 1 mol / L LiPF6 / EC:DMC (volume ratio of 1:1) with the addition of 10% (volume fraction) fluoroethylene carbonate (FEC), and the diaphragm was a polypropylene microporous membrane.
[0044] Calculation method of charge and discharge efficiency: Charge and discharge efficiency = first discharge capacity / first charge capacity.
[0045] Example 1
[0046] S1. Add salt-free water into the reactor, control the ammonia concentration to 5.5g / L, pH to 11.80, and the stirring intensity to 1.0kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali (sodium hydroxide), and a metal solution with a molar ratio of cobalt: manganese = 1:1 are added to the reactor in sequence for coprecipitation crystallization reaction for 70 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the morphology of the precursor is spherical.
[0047] S2. The precursor obtained in S1 is added into the reactor with sodium hydroxide, hydrogen peroxide (concentration of 10wt%), high-purity water and aluminum hydroxide in a molar ratio of 10:3:6:15:0.1 for sodium insertion reaction, and the sodium ion concentration is controlled to be 3.0-3.5mol / L, the reaction temperature is controlled to be 65°C, the reaction pressure is 3.0MPa, and the stirring intensity is 0.8kw / m 2 ·h, the reaction time is 20h, and a composite metal oxide is formed.
[0048] S3, hydrogen peroxide (concentration of 20wt%) and sodium hydroxide were added to the reaction slurry obtained in S2 again, and the sodium ion concentration was controlled to be 3.5mol / L, the reaction temperature was controlled at 60-65°C, the reaction pressure was 3.0MPa, and the stirring intensity was input power 0.8kw / m 2 ·h, the reaction time is 10h.
[0049] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese composite hydroxide. The scanning electron microscope photo of the sodium-cobalt-manganese composite hydroxide is shown in FIG. Figure 1 As shown, from Figure 1 It can be seen that the material is a single crystal product.
[0050] The prepared sodium cobalt manganese composite hydroxide was heat treated at 760 degrees Celsius for 12 hours, and then lithium carbonate was further added according to the formula design needs, and then calcined at 930 degrees Celsius for 15 hours in an air atmosphere to obtain Li 0.90 Na 0.15 Mn 0.49 5Co 0.495 Al 0.01 O2 positive electrode material, denoted as QN1.
[0051] The scanning electron microscope photo of the positive electrode material QN1 is as follows Figure 2 As shown, it can be seen that it is a single crystal product.
[0052] Example 2
[0053] S1. Add salt-free water into the reactor, control the ammonia concentration to 7g / L, pH to 11.50, and the stirring intensity to 0.9kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali, and a metal solution with a molar ratio of cobalt: manganese = 0.49:0.5 are added to the reactor in sequence for coprecipitation crystallization reaction for 100 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the precursor has a spherical morphology.
[0054] S2. The precursor obtained in S1 is added into the reactor with sodium acetate, hydrogen peroxide, high-purity water and zirconium oxide in a molar ratio of 10:2:15:0.1 for sodium insertion reaction. The reaction temperature is controlled at 75°C, the reaction pressure is 3.8MPa, and the stirring intensity is 0.9kw / m 2 ·h, the reaction time is 35h, and a composite metal oxide is formed.
[0055] S3. Add a strong oxidant (sodium chlorate and potassium permanganate mixed in a molar ratio of 1:1) and sodium hydroxide to the reaction slurry obtained in S2, control the alkali ion concentration to 4.5 mol / L, the reaction temperature to 70°C, the reaction pressure to 3.8 MPa, and the stirring intensity to an input power of 0.7 kw / m 2 ·h, the reaction time is 10h.
[0056] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese composite hydroxide, and the obtained sodium-cobalt-manganese composite hydroxide is heat-treated at 700 degrees Celsius for 12 hours, and lithium hydroxide, a lithium source, is further added according to the formula design needs, and then the obtained product is calcined at 880 degrees Celsius for 13 hours in an air atmosphere to obtain Li0.83 Na 0.17 Co 0.49 Mn 0.5 Zr 0.01 O2 positive electrode material, denoted as QN2. Scanning electron microscopy of QN2 shows that it is a single crystal product.
[0057] Example 3
[0058] S1. Add salt-free water into the reactor, control the ammonia concentration to 5.5g / L, pH to 11.80, and the stirring intensity to 1.0kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali, and a metal solution with a molar ratio of cobalt: manganese = 1:2 are added into the reactor in sequence for coprecipitation crystallization reaction for 70 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the precursor has a spherical morphology.
[0059] S2. The precursor obtained in S1 is added into the reactor with sodium hydroxide, hydrogen peroxide (concentration of 10wt%), high-purity water and magnesium hydroxide in a molar ratio of 10:2:5:13:0.2 for sodium insertion reaction. The reaction temperature is controlled at 75°C, the reaction pressure is 5.0MPa, and the stirring intensity is 0.7kw / m 2 ·h, the reaction time is 25h, and a composite metal oxide is formed.
[0060] S3, hydrogen peroxide (concentration of 20wt%) and sodium hydroxide were added to the reaction slurry obtained in S2 again, the sodium ion concentration was controlled to be 5mol / L, the reaction temperature was controlled to be 65-70°C, the reaction pressure was 5.0MPa, and the stirring intensity was input power 0.7kw / m 2 ·h, the reaction time is 10h.
[0061] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese intercalated composite hydroxide. The scanning electron microscope of the sodium-cobalt-manganese intercalated composite hydroxide shows that it is a single crystal product.
[0062] The prepared sodium cobalt manganese composite hydroxide was heat treated at 800 degrees Celsius for 10 hours, and then lithium carbonate was further added according to the formula design needs, and then calcined at 900 degrees Celsius for 15 hours in an air atmosphere to obtain Li 0.90 Na 0.13 Mn 0.65 Co 0.33 Mg 0.02 O2 positive electrode material, denoted as QN3. The scanning electron microscope photo of the positive electrode material QN3 shows that it is a single crystal product.
[0063] Example 4
[0064] S1. Add salt-free water into the reactor, control the ammonia concentration to 5.5g / L, pH to 11.80, and the stirring intensity to 1.0kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali, and a metal solution with a molar ratio of cobalt: manganese = 2:1 are added to the reactor in sequence for coprecipitation crystallization reaction for 70 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the precursor has a spherical morphology.
[0065] S2. The precursor obtained in S1 is added into the reactor with sodium hydroxide, hydrogen peroxide (concentration of 10wt%), high-purity water and titanium oxide in a molar ratio of 12:3:4:10:0.1 for sodium insertion reaction. The reaction temperature is controlled at 80°C, the reaction pressure is 2.0MPa, and the stirring intensity is 1.0kw / m 2 ·h, the reaction time is 15h, and a composite metal oxide is formed.
[0066] S3, hydrogen peroxide (concentration of 20wt%) and sodium hydroxide were added to the reaction slurry obtained in S2 again, the sodium ion concentration was controlled to be 5mol / L, the reaction temperature was controlled to be 50-55°C, the reaction pressure was 5.0MPa, and the stirring intensity was input power 1.5kw / m 2 ·h, the reaction time is 15h.
[0067] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese-embedded composite hydroxide. The scanning electron microscope photo of the sodium-cobalt-manganese-embedded composite hydroxide shows a single crystal product of the material.
[0068] The prepared sodium cobalt manganese composite hydroxide was heat treated at 800 degrees Celsius for 15 hours, and then lithium carbonate was further added according to the formula design needs, and then calcined at 800 degrees Celsius for 15 hours in an air atmosphere to obtain Li 0.90 Na 0.15 Mn 0.33 1Co 0.661 Ti 0.008 O2 positive electrode material, denoted as QN4. Scanning electron microscopy of positive electrode material QN4 shows that it is a single crystal product.
[0069] Example 5
[0070] S1. Add salt-free water into the reactor, control the ammonia concentration to 7g / L, pH to 11.50, and the stirring intensity to 0.9kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali, and a metal solution with a molar ratio of cobalt: manganese = 0.3:0.5 are added to the reactor in sequence for coprecipitation crystallization reaction for 100 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the precursor has a spherical morphology.
[0071] S2. The precursor obtained in S1 is added into the reactor with sodium acetate, hydrogen peroxide, high-purity water and yttrium oxide in a molar ratio of 10:2.5:16:0.1 for sodium insertion reaction. The reaction temperature is controlled at 70°C, the reaction pressure is 2.5MPa, and the stirring intensity is 0.9kw / m 2 ·h, the reaction time is 35h, and a composite metal oxide is formed.
[0072] S3. Add a strong oxidant (sodium chlorate and potassium permanganate mixed in a molar ratio of 1:1) and sodium hydroxide to the reaction slurry obtained in S2, control the sodium ion concentration to 5 mol / L, the reaction temperature to 60°C, the reaction pressure to 2.5 MPa, and the stirring intensity to an input power of 0.7 kw / m 2 ·h, the reaction time is 10h.
[0073] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese composite hydroxide, and the obtained sodium-cobalt-manganese composite hydroxide is heat-treated at 800 degrees Celsius for 12 hours, and lithium hydroxide, a lithium source, is further added according to the formula design needs, and then the obtained product is calcined at 850 degrees Celsius for 13 hours in an air atmosphere to obtain Li 0.83 Na 0.17 Co 0.37 Mn 0.62 Y 0.01 O2 positive electrode material, denoted as QN5. Scanning electron microscopy of QN5 shows that it is a single crystal product.
[0074] Example 6
[0075] S1. Add salt-free water into the reactor, control the ammonia concentration to 7g / L, pH to 11.50, and the stirring intensity to 0.9kw / m 2 h, the temperature is 50°C, ammonia water, liquid alkali, and a metal solution with a molar ratio of cobalt: manganese = 0.3:0.7 are added to the reactor in sequence for coprecipitation crystallization reaction for 100 hours, and a precursor containing cobalt and manganese is obtained after solid-liquid separation, and the precursor has a spherical morphology.
[0076] S2. The precursor obtained in S1 is added into the reactor with sodium acetate, hydrogen peroxide, high-purity water and molybdenum oxide in a molar ratio of 10:3:14:0.1 for sodium insertion reaction. The reaction temperature is controlled at 80°C, the reaction pressure is 4.5MPa, and the stirring intensity is 1.0kw / m 2 ·h, the reaction time is 35h, and a composite metal oxide is formed.
[0077] S3. Add a strong oxidant (sodium chlorate and potassium permanganate mixed in a molar ratio of 1:1) and sodium hydroxide to the reaction slurry obtained in S2, control the alkali ion concentration to 6 mol / L, the reaction temperature to 75°C, the reaction pressure to 3.5 MPa, and the stirring intensity to an input power of 0.7 kw / m 2 ·h, the reaction time is 10h.
[0078] S4. After the reaction is completed, solid-liquid separation is performed to obtain a sodium-cobalt-manganese composite hydroxide, and the obtained sodium-cobalt-manganese composite hydroxide is heat-treated at 700 degrees Celsius for 12 hours, and lithium hydroxide, a lithium source, is further added according to the formula design needs, and then the obtained product is calcined at 880 degrees Celsius for 13 hours in an air atmosphere to obtain Li 0.83 Na 0.17 Co 0.297 Mn 0.693 Mo 0.01 O2 positive electrode material, denoted as QN6. Scanning electron microscopy of QN6 shows that it is a single crystal product.
[0079] Comparative Example 1
[0080] This comparative example refers to Example 1, except that the reaction temperature in S2 is controlled at 45°C. It is found that the composite metal oxide obtained after the reaction in S3 is a mixture, and the scanning electron microscope shows that the morphology of the materials is quite different. Further lithium carbonate is added as a lithium source, and then calcined at 930°C for 15h in an air atmosphere, and the obtained material is recorded as DN1.
[0081] Comparative Example 2
[0082] This comparative example refers to Example 1, except that in S2, sodium hydroxide, hydrogen peroxide, high-purity water and aluminum hydroxide are added to the reactor in a molar ratio of 10:3:6:15:0.1 for sodium insertion reaction, and the concentration of sodium ions is 0.5 mol / L. It is found that the composite metal oxide obtained after the reaction of S3 is a mixture, and the scanning electron microscope shows that the morphology of the materials is quite different. Further lithium carbonate is added as a lithium source, and then calcined at 930°C for 15 hours in an air atmosphere, and the obtained material is recorded as DN2.
[0083] Comparative Example 3
[0084] This comparative example refers to Example 1, except that in S3, the concentration of the oxidant hydrogen peroxide is the same as that in S2. It is found that the composite metal oxide obtained after the reaction of S3 is a mixture, and the scanning electron microscope shows that the morphology of the materials is quite different. Further lithium carbonate is added as a lithium source, and then calcined at 930°C for 15h in an air atmosphere, and the obtained material is recorded as DN3.
[0085] Comparative Example 4
[0086] This comparative example refers to Example 1, except that the reaction temperature in S2 is controlled at 45°C, and in S3, the sodium ion concentration is 2.0 mol / L, and the reaction temperature is controlled at 45°C. It is found that the composite metal oxide obtained after the reaction of S3 is a mixture, and the scanning electron microscope shows that the morphology of the materials is quite different. Further lithium carbonate is added as a lithium source, and then calcined at 930°C for 15h in an air atmosphere, and the obtained material is recorded as DN4.
[0087] Performance Testing
[0088] Perform charge and discharge tests on the battery, such as Figure 3 As shown, according to the voltage-specific capacity curve, the positive electrode material prepared in Example 1 has a charge capacity of 171.1 mAh / g and a discharge capacity of 166.3 mAh / g in the charge-discharge range of 3.0-4.4 V at a rate of 0.1 C, and an initial efficiency of up to 97.1%.
[0089] The battery charge and discharge test results of other samples are shown in Table 1.
[0090] Table 1 Battery charge and discharge test results
[0091]
[0092] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0093] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0094] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a sodium-cobalt-manganese composite oxide, characterized in that: The following steps are involved: S1, obtaining a cobalt-manganese metal compound precursor, wherein the cobalt-manganese metal compound precursor includes at least one of cobalt hydroxide, manganese hydroxide, cobalt carbonate, and manganese oxide, and the cobalt-manganese metal compound precursor is prepared by a coprecipitation crystallization method, specifically comprising: adding water, a complexing agent, a precipitant, an additive, and a mixed metal solution to perform a coprecipitation crystallization reaction, wherein the mixed metal solution contains cobalt and manganese elements, and obtaining the cobalt-manganese metal compound precursor by solid-liquid separation; S2, adding the precursor, sodium metal compound, water, additive and oxidant described in S1 into a reactor for reaction; controlling the reaction conditions of the reactor, including: the concentration of sodium ions in the reactor is 1-12 mol / L, the reaction temperature is 50-90°C, the reaction pressure is 0.1-50 MPa, the reaction time is 3-60 h, and the stirring intensity is 0.1-1.6 kw / m 2 h; the additive is selected from at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium and molybdenum metal compounds; S3, adding a strong oxidant to the reaction material obtained in S2, wherein the oxidizing ability of the strong oxidant is higher than that of the oxidant in S2, and controlling the reaction conditions, including: the sodium ion concentration in the system is 3-6 mol / L, the reaction temperature is 20-90°C, the reaction pressure is 0.1-50 MPa, and the stirring intensity is 0.1-1.6 kw / m 2 h, thereby embedding sodium ions into the structure of cobalt-manganese metal compounds to form composite metal oxides; S4, performing solid-liquid separation on the reaction material obtained in S3, collecting the solid phase for heat treatment to obtain a sodium-cobalt-manganese intercalated composite oxide, wherein the sodium-cobalt-manganese intercalated composite oxide is a solid solution, and sodium ions replace the sites of cobalt and / or manganese.
2. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 1, characterized in that: The sodium metal compound in S2 is at least one of sodium hydroxide, sodium acetate, sodium nitrate, sodium sulfate, sodium bicarbonate, and sodium oxalate.
3. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 2, characterized in that: The sodium metal compound in S2 is at least one of sodium hydroxide, sodium sulfate and sodium carbonate.
4. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 3, characterized in that: The sodium metal compound in S2 is sodium hydroxide.
5. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to any one of claims 2 to 4, characterized in that: The oxidant in S2 is selected from at least one of oxygen, air and hydrogen peroxide.
6. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 5, characterized in that: The oxidant in S2 is hydrogen peroxide.
7. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to any one of claims 2 to 4, characterized in that: The concentration of sodium ions in the reactor in S2 is 1~10 mol / L.
8. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 7, characterized in that: The concentration of sodium ions in the reactor in S2 is 3-10 mol / L.
9. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 8, characterized in that: The concentration of sodium ions in the reactor in S2 is 3-6 mol / L.
10. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 7, characterized in that: The reaction temperature in S2 is 50-80°C.
11. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 10, characterized in that: The reaction temperature in S2 is 60-80°C.
12. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 10, characterized in that: The reaction pressure in S2 is 1-10 MPa.
13. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 12, characterized in that: The reaction pressure in S2 is 1-5 MPa.
14. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 10, characterized in that: The stirring intensity in S2 is 0.5-1kw / m 2 ·h.
15. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 14, characterized in that: The stirring intensity in S2 is 0.7~0.9kw / m 2 ·h.
16. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 1, characterized in that: The reaction time in S2 is 5-40h.
17. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 16, characterized in that: The reaction time in S2 is 15-35h.
18. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 1, characterized in that: The strong oxidant in S3 is selected from at least one of oxygen, sodium chlorate, hydrogen peroxide, potassium permanganate and nitric acid.
19. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 18, characterized in that: The sodium ion concentration described in S3 is 3.5~5.5mol / L.
20. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 19, characterized in that: The sodium ion concentration in S3 is 3.5-5 mol / L.
21. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 20, characterized in that: The sodium ion concentration in S3 is 3.5-4.5 mol / L.
22. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 18, characterized in that: The reaction pressure in S3 is 1-10 MPa.
23. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 22, characterized in that: The reaction pressure in S3 is 1-5 MPa.
24. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 18, characterized in that: The reaction temperature in S3 is 40-90°C.
25. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 24, characterized in that: The reaction temperature in S3 is 50-80°C.
26. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 25, characterized in that: The reaction temperature in S3 is 60-75°C.
27. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 18, characterized in that: The stirring intensity in S3 is 0.5-1kw / m 2 ·h.
28. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 27, characterized in that: The stirring intensity in S3 is 0.7-0.9kw / m 2 ·h.
29. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 18, characterized in that: The temperature of the heat treatment in S4 is 400-1000°C.
30. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 29, characterized in that: The temperature of the heat treatment in S4 is 500-900°C.
31. The method for preparing the sodium-cobalt-manganese composite oxide according to claim 30, characterized in that: The temperature of the heat treatment in S4 is 650-800°C.
32. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 29, characterized in that: The heat treatment time in S4 is 3 to 36 hours.
33. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 32, characterized in that: The heat treatment time in S4 is 5-25h.
34. The method for preparing the sodium-embedded cobalt-manganese composite oxide according to claim 33, characterized in that: The heat treatment time in S4 is 10-20 hours.
35. The sodium-intercalated cobalt-manganese composite oxide prepared by the method for preparing the sodium-intercalated cobalt-manganese composite oxide according to any one of claims 1 to 34, characterized in that: The chemical formula of the sodium-cobalt-manganese composite oxide is Na x Mn a Co b Me c O2, wherein 0≤x≤0.2, 0≤a≤1, 0≤b≤1, 0≤c≤0.2, wherein a+b+c=1, and Me is at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium, and molybdenum.
36. A sodium-embedded lithium-ion battery positive electrode material, prepared by mixing and calcining the sodium-embedded cobalt-manganese composite oxide of claim 35 and a lithium source, wherein the chemical formula of the sodium-embedded lithium-ion battery positive electrode material is Li x Na y Mn a Co b Me c O2, wherein 0.5≤x≤1.3, 0≤y≤0.2, 0≤a≤1, 0≤b≤1, 0≤c≤0.2, wherein a+b+c=1, and Me is at least one of titanium, aluminum, magnesium, zirconium, tungsten, yttrium, strontium, niobium, and molybdenum metals.
37. The sodium-embedded lithium-ion battery positive electrode material according to claim 36, characterized in that: The lithium source is one or more of lithium carbonate, lithium hydroxide, and lithium acetate. The mixed calcination conditions include a temperature of 400-1000° C., a calcination time of 5-40 hours, and a calcination atmosphere of air or oxygen.
38. The sodium-embedded lithium-ion battery positive electrode material according to claim 37, characterized in that: The mixed calcination conditions include a temperature of 600-1000°C.
39. The sodium-embedded lithium-ion battery positive electrode material according to claim 38, characterized in that: The mixed calcination conditions include a temperature of 700-1000°C.
40. The sodium-embedded lithium-ion battery positive electrode material according to claim 37, characterized in that: The mixed calcination conditions include a calcination time of 5-25 hours.
41. The sodium-embedded lithium-ion battery positive electrode material according to claim 40, characterized in that: The mixed calcination conditions include a calcination time of 10-20 hours.
42. A lithium ion battery comprising the lithium ion battery positive electrode material according to any one of claims 36 to 41.
Citation Information
Patent Citations
Method for synthesizing lithium, nickel, manganese and cobalt composite oxide powder material
CN103762355A
Sodium-ion-containing lithium-rich manganese-based positive electrode material, precursor and preparation method thereof
CN111554920A