Metal oxide based capacitive ion diode and its preparation method and application

By using metal oxide materials with intercalation pseudocapacitive behavior and porous carbon-based counter electrodes in capacitive ion diodes, combined with a special electrolyte, the problems of low energy storage density and high cost in the existing technology are solved, and a more efficient High rectification ratio and energy storage density reduce costs.

CN116313559BActive Publication Date: 2024-10-22LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310217053.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-08
Publication Date
2024-10-22
Estimated Expiration
2043-03-08

AI Technical Summary

Technical Problem

The problems of existing capacitive ion diodes with low unidirectional energy storage density and high cost are mainly due to the strict requirements on the pore structure of porous carbon electrodes, which results in high manufacturing costs and limited energy storage density.

Method used

Metal oxide materials with intercalation pseudocapacitance behavior are used as electrode materials. By combining with porous carbon-based counter electrodes and special electrolytes, selective storage of anions and cations in the electrolyte is achieved, and the rectification ratio and energy storage density are improved.

Benefits of technology

The rectification ratio, mass specific capacitance, volume specific capacitance and unidirectional energy storage density of the capacitive ion diode have been improved, reducing costs and ensuring that the device works efficiently and stably for a long time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116313559B_ABST
    Figure CN116313559B_ABST
Patent Text Reader

Abstract

The present invention discloses a metal oxide-based capacitive ion diode and a preparation method and application thereof. The preparation method comprises preparing a metal oxide-based working electrode and a porous carbon-based counter electrode, wherein the metal oxide-based working electrode uses a metal oxide with intercalation pseudocapacitive behavior; preparing an electrolyte, wherein only one type of ions among the anions and cations in the electrolyte can be stored in the metal oxide; assembling the metal oxide-based working electrode and the porous carbon-based counter electrode, and placing them in the electrolyte for packaging to obtain a metal oxide-based capacitive ion diode. The present invention proposes for the first time to use a metal oxide material with intercalation pseudocapacitive behavior as an electrode material for a capacitive ion diode, and utilizes its selective storage behavior for anions and cations in the electrolyte to realize the unidirectional energy storage characteristics of the device, and the prepared metal oxide-based capacitive ion diode has the advantages of high rectification ratio, mass specific capacitance, volume specific capacitance, and unidirectional energy storage density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention discloses a metal oxide based capacitive ion diode and a preparation method and application thereof, specifically a metal oxide based capacitive ion diode, a preparation method and application thereof in an ion / electron coupling circuit, belonging to the field of electrochemical energy storage and the emerging field of ion / electron coupling circuits. Background Art

[0002] Capacitive ion diodes are a new type of electrochemical functional device based on supercapacitors. They have a device structure similar to that of supercapacitors and the unidirectional conduction characteristics of semiconductor diodes. They are considered to be the most promising basic components for building new ion circuits, and have broad application prospects in future technical fields such as in vivo diagnosis and treatment, human-computer interfaces, and neural network interactions. In 2019, Professor Stefan Kaskel of the Dresden University of Technology first proposed the concept of capacitive ion diodes, and constructed the first capacitive ion diode using the size screening effect of porous carbon electrodes on anions and cations. Thanks to the differential storage behavior of microporous carbon electrodes for anions and cations, the capacitive ion diode exhibits electrochemical behavior of unidirectional energy storage and unidirectional conduction volt-ampere characteristics similar to traditional semiconductor diodes. These special properties are expected to expand the use scenarios of traditional supercapacitors to new technical fields, enabling them to play an important role in power transmission, signal transmission, and logical operations, and therefore have attracted widespread attention.

[0003] However, the above-mentioned capacitive ion diode based on the ion screening effect has strict requirements on the pore structure of the porous carbon electrode. In order to make the device have a higher rectification ratio, the porous carbon electrode should have a relatively single pore size distribution, which will undoubtedly greatly increase the manufacturing cost of the porous carbon electrode, especially the pure microporous carbon electrode. At the same time, the limited mass specific capacitance and low stacking density of the carbon material greatly limit the unidirectional energy storage density of the constructed capacitive ion diode, which is not conducive to the long-term, efficient and stable operation of the capacitive ion diode. Summary of the invention

[0004] The purpose of the present application is to provide a metal oxide-based capacitive ion diode and a preparation method and application thereof, so as to solve the technical problems of low unidirectional energy storage density and high cost of existing capacitive ion diodes.

[0005] A first aspect of the present invention provides a method for preparing a metal oxide-based capacitive ion diode, comprising:

[0006] A metal oxide-based working electrode and a porous carbon-based counter electrode are prepared, wherein the metal oxide used in the metal oxide-based working electrode is a metal oxide having intercalation pseudocapacitive behavior;

[0007] Preparing an electrolyte, wherein only one type of ions among the anions and cations of the electrolyte can be stored in the metal oxide;

[0008] The metal oxide-based working electrode and the porous carbon-based counter electrode are assembled and placed in the electrolyte, and then packaged to obtain a metal oxide-based capacitive ion diode.

[0009] Preferably, the loading amount of the porous carbon-based counter electrode active substance is 1 to 2 times the loading amount of the metal oxide-based working electrode active substance.

[0010] Preferably, the preparation of the metal oxide-based working electrode specifically comprises:

[0011] The metal oxide material is mixed with a conductive agent and a binder, and then a dispersant is added to obtain a slurry;

[0012] The slurry is disposed on a current collector to obtain a metal oxide-based working electrode.

[0013] Preferably, the mass ratio of the metal oxide material, the conductive agent and the binder is 6 to 9:1 to 3:1.

[0014] Preferably, the metal oxide material is at least one of niobium pentoxide, molybdenum trioxide, tungsten trioxide and titanium dioxide.

[0015] Preferably, the porous carbon-based counter electrode is prepared, specifically comprising:

[0016] The porous carbon material is mixed with a conductive agent and a binder, and then a dispersant is added to obtain a slurry;

[0017] The slurry is disposed on a current collector to obtain a porous carbon-based counter electrode.

[0018] Preferably, the mass ratio of the porous carbon material, the conductive agent and the binder is 6 to 9:1 to 3:1.

[0019] Preferably, the electrolyte in the electrolyte is an inorganic salt or an organic salt;

[0020] The concentration of the electrolyte is 0.001-10 mol / L.

[0021] A second aspect of the present invention provides a metal oxide-based capacitive ion diode, which is prepared using the above-mentioned method for preparing the metal oxide-based capacitive ion diode.

[0022] A third aspect of the present invention provides an ion / electron coupling circuit, in which the above-mentioned metal oxide-based capacitive ion diode is used.

[0023] Compared with the prior art, the metal oxide-based capacitive ion diode and its preparation method and application of the present invention have the following beneficial effects:

[0024] The present invention proposes for the first time to use a metal oxide material with intercalation pseudocapacitive behavior as the electrode material of a capacitive ion diode, and utilizes its selective storage behavior of anions and cations in an electrolyte to realize the unidirectional energy storage characteristics of the device. The prepared metal oxide-based capacitive ion diode has the advantages of high rectification ratio, mass specific capacitance, volume specific capacitance, unidirectional energy storage density and low cost, achieving a leap-forward improvement in the comprehensive performance of the capacitive ion diode. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart of a method for preparing a metal oxide-based capacitive ion diode according to an embodiment of the present invention;

[0026] Figure 2 This is a low-magnification scanning electron microscope image of the niobium pentoxide material in Example 1 of the present invention;

[0027] Figure 3 This is a high-magnification scanning electron microscope image of the niobium pentoxide material in Example 1 of the present invention;

[0028] Figure 4 is the X-ray diffraction pattern of the niobium pentoxide material in Example 1 of the present invention;

[0029] Figure 5 The cyclic voltammetry curve of the niobium pentoxide electrode in Example 1 of the present invention, wherein (a) is the sweep rate of 0.5 mVs -1 , 0.8mV s -1 , 1.0mV s -1 Cyclic voltammetry curve of niobium pentoxide electrode at a scan rate of 2.0 mV s -1 , 5.0mVs -1 , 8.0mV s -1 Cyclic voltammetry curve of niobium pentoxide electrode at ;

[0030] Figure 6 The constant current charge-discharge curve of the niobium pentoxide electrode in Example 1 of the present invention, wherein (a) is the current density of 0.1Ag -1 , 0.2Ag -1 , 0.5Ag -1 , 0.8Ag -1 , 1Ag -1 (b) is the constant current charge-discharge curve of the niobium pentoxide electrode at a current density of 1Ag. -1 , 2Ag -1 , 3Ag -1 , 4Ag -1, 5Ag -1 Constant current charge-discharge curve of niobium pentoxide electrode at 2 ℃;

[0031] Figure 7 is the first type rectification ratio of the niobium pentoxide electrode in Example 1 of the present invention;

[0032] Figure 8 is the second type rectification ratio of the niobium pentoxide electrode in Example 1 of the present invention;

[0033] Fig. 9 is the mass specific capacitance of the niobium pentoxide electrode in Example 1 of the present invention;

[0034] Fig.10 This is the cyclic voltammetry curve of the niobium pentoxide-based capacitive ion diode in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] A first aspect of the present invention provides a method for preparing a metal oxide-based capacitive ion diode, comprising:

[0036] Step 1: prepare a metal oxide-based working electrode and a porous carbon-based counter electrode, wherein the metal oxide used in the metal oxide-based working electrode is a metal oxide having intercalation pseudocapacitive behavior.

[0037] In the embodiments of the present invention, two schemes can be used to prepare the metal oxide-based working electrode:

[0038] The first solution is to mix the metal oxide material with the conductive agent and the binder in a certain proportion, then add a certain amount of dispersant and place the slurry on the current collector, and then fully dry it in a vacuum oven and cut it to obtain the metal oxide-based working electrode.

[0039] The second option is to mix the metal oxide material and the conductive agent in a certain proportion, and then add a certain amount of dispersant to prepare a self-supporting metal oxide-based working electrode, which can then be assembled into a flexible diode.

[0040] The metal oxide material in the embodiment of the present invention is at least one of intercalation pseudocapacitor materials such as niobium pentoxide (Nb2O5), molybdenum trioxide (MoO3), tungsten trioxide (WO3), and titanium dioxide (TiO2). Exemplarily, the metal oxide material may be one of niobium pentoxide (Nb2O5), tungsten trioxide (WO3), and titanium dioxide (TiO2), or a combination of molybdenum trioxide (MoO3) and at least one of niobium pentoxide (Nb2O5), tungsten trioxide (WO3), and titanium dioxide (TiO2). The above materials can selectively store anions and cations in the electrolyte, so that the unidirectional energy storage density of the metal oxide-based capacitive ion diode is high.

[0041] The conductive agent in the embodiment of the present invention includes but is not limited to conductive carbon black (Super-P), Ketjen black, acetylene black, single-walled or multi-walled carbon nanotubes, graphene nanosheets, and high-crystalline graphite powder; the binder includes but is not limited to polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyacrylonitrile, sodium carboxymethyl cellulose, polyacrylic acid, polyethylene oxide, styrene-butadiene rubber, and sodium alginate; the dispersant includes but is not limited to deionized water, ethanol, ethylene glycol, acetone, acetonitrile, propylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide. The conductive agent, binder, and dispersant of the above-mentioned ingredients cooperate with the metal oxide material and work synergistically, so as to ensure that the metal oxide-based working electrode selectively stores anions and cations in the electrolyte, so that the metal oxide-based capacitive ion diode has high unidirectional energy storage density, high rectification ratio, and high stability.

[0042] The mass ratio of the above-mentioned metal oxide material, conductive agent, and binder is 6 to 9:1 to 3:1, for example, 6:1:1, 6:2:1, 6:3:1, 7:1:1, 7:2:1, 7:3:1, 8:1:1, 8:2:1, 8:3:1, 9:1:1, 9:2:1 or 9:3:1, etc., preferably 8:1:1. The unidirectional energy storage density, mass specific capacitance, and volume specific capacitance of the metal oxide-based capacitive ion diode prepared at this content are all high, which can ensure that the prepared metal oxide-based capacitive ion diode works efficiently and stably for a long time. When the second scheme is adopted, the mass ratio of the metal oxide material to the conductive agent is 6 to 9:1 to 3.

[0043] In an embodiment of the present invention, the method of setting the slurry on the current collector can be a coating method, and a self-supporting electrode can also be prepared by methods such as electrospinning, interfacial assembly, and vacuum filtration. The above method is simple, highly operable, low cost, and the stability of the resulting working electrode is good. The current collector includes but is not limited to aluminum foil, copper foil, titanium foil, nickel foil, gold sheet, platinum sheet, stainless steel mesh, nickel foam, copper foam, graphite foil, carbon paper, and carbon cloth. The current collector of the above material itself has a small internal resistance, and the current generated by the metal oxide material can be collected to form a larger current for external output.

[0044] In the embodiment of the present invention, two schemes can be used to prepare the porous carbon-based counter electrode:

[0045] The first scheme is: the porous carbon material is mixed with a conductive agent and a binder and then a dispersant is added to obtain a slurry;

[0046] The slurry is placed on a current collector and then fully dried in a vacuum oven and cut to obtain a porous carbon-based counter electrode.

[0047] The second option is to add a certain amount of dispersant to the porous carbon material to prepare a self-supporting porous carbon-based counter electrode, which can then be assembled with a metal oxide-based working electrode to obtain a flexible diode.

[0048] The porous carbon material used in the embodiment of the present invention can be at least one of commercial activated carbon, biomass carbon, polymer derived carbon, organic small molecule derived carbon, graphene, graphyne, carbon nanotubes, etc. The above porous carbon material is easy to obtain, and the performance of the electrode prepared using it is stable.

[0049] The conductive agent in the embodiment of the present invention includes but is not limited to conductive carbon black (Super-P), Ketjen black, acetylene black, single-walled or multi-walled carbon nanotubes, graphene nanosheets, and high-crystalline graphite powder; the binder includes but is not limited to polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyacrylonitrile, sodium carboxymethyl cellulose, polyacrylic acid, polyethylene oxide, styrene-butadiene rubber, and sodium alginate; the dispersant includes but is not limited to deionized water, ethanol, ethylene glycol, acetone, acetonitrile, propylene carbonate, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide. The conductive agent, binder, and dispersant of the above ingredients are combined with the porous carbon material and act synergistically, so that the prepared porous carbon-based electrode has good conductivity and many holes, which is convenient for the transfer of electrons and the transmission of ions.

[0050] The mass ratio of the porous carbon material, the conductive agent and the binder is 6 to 9:1 to 3:1, for example, it can be 6:1:1, 6:2:1, 6:3:1, 7:1:1, 7:2:1, 7:3:1, 8:1:1, 8:2:1, 8:3:1, 9:1:1, 9:2:1 or 9:3:1, etc., preferably 8:1:1. The porous carbon-based electrode prepared at this content has good conductivity and many pores, which facilitates the transfer of electrons and the transmission of ions, thereby making the unidirectional energy storage density, mass specific capacitance and volume specific capacitance of the metal oxide-based capacitive ion diode relatively high, so that the metal oxide-based capacitive ion diode can operate efficiently and stably for a long time.

[0051] In an embodiment of the present invention, the method of setting the slurry on the current collector can be a coating method, and the self-supporting electrode can also be prepared by methods such as electrospinning, interfacial assembly, and vacuum filtration. The above method is simple, highly operable, low cost, and the stability of the obtained electrode is good. The current collector includes but is not limited to aluminum foil, copper foil, titanium foil, nickel foil, gold sheet, platinum sheet, stainless steel mesh, nickel foam, copper foam, graphite foil, carbon paper, and carbon cloth. The current collector of the above material itself has a small internal resistance, and the current generated by the porous carbon material can be collected to form a larger current for external output.

[0052] To ensure that the capacitive ion diode finally constructed can work efficiently, the loading amount of the porous carbon-based counter electrode active material in the embodiment of the present invention is 1 to 10 times, preferably 1 to 2 times, the loading amount of the metal oxide-based working electrode active material.

[0053] Step 2: prepare an electrolyte, in which only one type of ions among the anions and cations in the electrolyte can be stored in the metal oxide.

[0054] In the embodiment of the present invention, in combination with the crystal structure and electrochemical properties of the metal oxide, the electrolyte in the electrolyte used is an inorganic salt or an organic salt, and then the electrolyte is dissolved in a solvent to obtain the electrolyte of the present application. The embodiment of the present invention can also directly use ionic liquids as electrolytes. The selection criteria for the above-mentioned inorganic salts or organic salts are that there is only one ion in the anions and cations that can be efficiently stored in the working electrode active material; the selection criteria for the solvent are that it has a good solubility for the above-mentioned inorganic salts or organic salts, and at the same time has good resistance to electrochemical oxidation or reduction; the selection criteria for the concentration of the electrolyte is to try to make the prepared electrolyte have a higher ionic conductivity and a wider electrochemical window.

[0055] The inorganic salts include, but are not limited to, sulfates, nitrates, phosphates, perchlorates, tetrafluoroborate, hexafluorophosphate, bisfluorosulfonyl imide salts, trifluoromethanesulfonyl imide salts, chlorides, bromides, and iodides of lithium, sodium, potassium, zinc, magnesium, calcium, and aluminum; the organic salts include, but are not limited to, tetrafluoroborate, hexafluorophosphate, trifluoromethanesulfonyl imide salts, chlorides, bromides, and iodides of quaternary ammonium, imidazole, pyrrole, and quaternary phosphonium cations. The selection is based on the fact that only one of the anions and cations of the inorganic or organic salt can be efficiently stored in the metal oxide material.

[0056] In the embodiment of the present invention, the solvent used to prepare the electrolyte includes but is not limited to water, acetonitrile, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and 1,3-dioxolane. In order to make the prepared electrolyte have good electrochemical stability and high ionic conductivity, the choice of solvent is not limited to a single solvent, and two or more mixed solvents can be selected according to needs, and organic small molecules or inorganic salt additives with specific functions can also be introduced.

[0057] Furthermore, the concentration of the electrolyte in the embodiment of the present invention is 0.001-10 mol / L. Within this concentration range, the prepared electrolyte has both good electrochemical stability and high ionic conductivity.

[0058] Step 3: Assemble the metal oxide-based working electrode and the porous carbon-based counter electrode, place them in an electrolyte, and then package them to obtain a metal oxide-based capacitive ion diode. Specifically:

[0059] The metal oxide-based working electrode and the porous carbon-based counter electrode are assembled in a stacked or wound manner, and the prepared electrolyte is injected therein, and then the entire device is packaged to obtain a metal oxide-based capacitive ion diode.

[0060] The device morphology of the metal oxide-based capacitive ion diode obtained by the present invention includes but is not limited to a button type, a sandwich type, a soft package type and a planar interdigital type.

[0061] Based on an in-depth analysis of the working principle of porous carbon-based capacitive ion diodes, the present invention proposes that the key to unidirectional energy storage of capacitive ion diodes lies in the selective storage of anions and cations by electrode materials, and innovatively utilizes the screening effect of metal oxide materials on anions and cations to develop higher performance capacitive ion diodes, breaking the limitations of the material system on the various performance of capacitive ion diodes.

[0062] The metal oxide material and porous carbon material used in the method of the present invention have mature preparation technology, are simple and easy to obtain, have low cost, and are suitable for mass production;

[0063] The electrode preparation method used in the method of the present invention has a mature process route, is highly compatible with various types of electrode materials and existing electrode production lines, is suitable for large-scale production and preparation, and has low cost.

[0064] A second aspect of the present invention provides a metal oxide-based capacitive ion diode, which is prepared using the above-mentioned method for preparing the metal oxide-based capacitive ion diode.

[0065] The metal oxide-based capacitive ion diode of the embodiment of the present invention comprises at least a metal oxide-based working electrode, a porous carbon-based counter electrode and a wide potential window electrolyte. The working principle of the unidirectional energy storage is mainly based on the selective storage behavior of the metal oxide electrode for the anions and cations of the electrolyte, that is, the ion screening effect.

[0066] The metal oxide-based capacitive ion diode constructed by the method of the present invention has high rectification ratio, high specific capacitance, high energy density and excellent cycle stability, and its comprehensive performance is far superior to the existing porous carbon-based capacitive ion diode, achieving a leap-forward improvement in the comprehensive performance of the capacitive ion diode.

[0067] The third aspect of the present invention provides an ion / electron coupling circuit, in which the above-mentioned metal oxide-based capacitive ion diode is used. The ion / electron coupling circuit using the metal oxide-based capacitive ion diode has a very broad practical application prospect in the technical fields of in vivo diagnosis and treatment, human-machine interface, neural network interaction, etc.

[0068] The technical solution of the present invention is described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto. The materials, reagents, etc. used in the following embodiments, unless otherwise specified, can be obtained from commercial sources.

[0069] In all the following examples, the niobium pentoxide material is prepared by a "hydrothermal + annealing" method, and the specific preparation process is as follows:

[0070] Dissolve 400 mg of niobium pentachloride (NbCl5) in 40 mL of ethylene glycol, and dissolve 800 mg of hexamethylenetriamine in 40 mL of deionized water. Mix the two solutions under magnetic stirring and continue stirring for 20 minutes, then transfer the mixture to a 100 mL hydrothermal kettle, keep it at 200 ° C for 12 hours, and then cool it naturally to room temperature. The resulting product is repeatedly centrifuged and washed with ethanol and deionized water, and then dried in a 60 ° C forced air oven to obtain a light yellow powder. The light yellow powder is heated to 600 ° C in an air atmosphere and maintained for 2 hours, and white Nb2O5 powder is obtained after it is naturally cooled to room temperature.

[0071] In all the following examples, the characterization and testing methods used are as follows:

[0072] 1) Scanning electron microscope: observe the microscopic morphology of niobium pentoxide material.

[0073] 2) X-ray diffractometer: to test the X-ray diffraction pattern of niobium pentoxide material.

[0074] 3) Electrochemical workstation: Test the cyclic voltammetry curve and constant current charge-discharge curve of niobium pentoxide electrode and niobium pentoxide-based capacitive ion diode.

[0075] Example 1

[0076] In the first step, the prepared niobium pentoxide powder material, Super-P and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a ratio of 8:1:1, and then the slurry was evenly coated on the titanium foil and the loading amount of the active material was controlled to 1 mg / cm 2 , dried in a vacuum oven and cut to obtain a niobium pentoxide-based working electrode.

[0077] In the second step, commercial activated carbon, acetylene black and polytetrafluoroethylene were mixed in ethanol at a ratio of 8:1:1, and then the slurry was evenly coated on a stainless steel mesh and the loading amount of active substances was controlled to 2 mg / cm 2 , dried in a vacuum oven and cut to obtain an activated carbon-based counter electrode.

[0078] In the third step, lithium hexafluorophosphate (LiPF6) was selected as the electrolyte, and a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate (volume ratio 1:1:1) was used as the solvent to prepare a 1 mol / L electrolyte; in this electrolyte, there is only Li + It can be efficiently stored in the niobium pentoxide electrode, so the niobium pentoxide electrode can exhibit obvious anion and cation screening effect.

[0079] In the fourth step, the niobium pentoxide-based working electrode and the activated carbon-based counter electrode are assembled into a button battery, and the prepared lithium hexafluorophosphate electrolyte is injected therein, and then the entire device is packaged with a battery sealing machine to obtain a niobium pentoxide-based capacitive ion diode.

[0080] like Figure 2 As shown in the figure, the niobium pentoxide prepared by the method described in this embodiment has a microscopic morphology of nanoflowers with a very uniform size of about 2 to 3 microns in diameter. From the magnified scanning electron microscope image, it can be seen that the niobium pentoxide nanoflowers are assembled from highly curved and wrinkled nanosheets ( Figure 3 ), giving it a higher specific surface area so that it can fully contact with the electrolyte. Further X-ray diffraction tests revealed that ( Figure 4 ), the crystalline form of niobium pentoxide is orthorhombic phase, namely T-Nb2O5, which is a typical intercalation pseudocapacitor material. Figure 5 It can be seen from the cyclic voltammetry curve shown that the niobium pentoxide electrode exhibits a very significant ion screening effect, that is, it exhibits a high charge storage current in the low potential range (1-2.5V), indicating that the lithium ions in the electrolyte can be stored efficiently. In the high potential range (2.5-4V), the niobium pentoxide electrode only exhibits a very weak double-layer capacitance, indicating that the hexafluorophosphate ions in the electrolyte cannot be effectively stored inside the niobium pentoxide electrode due to the ion screening effect. Figure 6 The constant current charge-discharge curves shown in the figure show that the charge storage capacity of the niobium pentoxide electrode is mainly concentrated in the low potential range where lithium ions contribute to the capacity. This phenomenon further shows that the niobium pentoxide electrode has good selective storage behavior for anions and cations in the electrolyte. According to the cyclic voltammetry curve, it can be calculated that the first-class rectification ratio of the niobium pentoxide electrode is as high as 79 ( Figure 7 ), which is much higher than the previous porous carbon system (~10). The second type rectification ratio calculated from the constant current charge and discharge curve is also as high as 97.6% ( Figure 8 ), which is still higher than the porous carbon system (~80%). At the same time, the niobium pentoxide electrode exhibited an ultra-high mass specific capacitance of 659C / g at a current density of 0.1A / g. Fig. 9 ), which is also higher than the previous porous carbon system (<100C / g). These excellent ion rectification properties make the capacitive ion diode assembled from niobium pentoxide electrodes exhibit ideal unidirectional energy storage behavior ( Fig.10 ), and its operating voltage can reach ±2V, which has good practical application prospects in the future technical fields such as smart grid, in vivo diagnosis and treatment, human-computer interface, neural network interaction, etc. based on ion / electron coupling circuits.

[0081] Example 2

[0082] In the first step, the prepared niobium pentoxide powder material, Ketjen black and sodium alginate were dispersed in deionized water at a ratio of 7:2:1. The slurry was then evenly coated on graphite foil and the loading amount of active substances was controlled to be 2 mg / cm 2 , dried in a blast oven and cut to obtain a niobium pentoxide-based working electrode.

[0083] In the second step, commercial carbon nanotubes, Super-P, and sodium carboxymethyl cellulose were mixed in deionized water at a ratio of 7:2:1, and then the slurry was evenly coated on titanium foil and the loading amount of active substances was controlled to 3 mg / cm 2 , dried in a forced air oven and cut to obtain a carbon nanotube-based electrode.

[0084] In the third step, lithium trifluoromethanesulfonyl imide (LiTFSI) was selected as the electrolyte and deionized water was used as the solvent to prepare a high-concentration salt electrolyte of 21 mol / kg. In this electrolyte, there is only Li + It can be stored efficiently in the niobium pentoxide electrode, so the niobium pentoxide electrode can exhibit obvious anion and cation screening effect.

[0085] In the fourth step, the niobium pentoxide-based working electrode and the carbon nanotube-based counter electrode are assembled in a stacked manner, and the prepared high-concentration lithium trifluoromethanesulfonyl imide salt electrolyte is injected therein, and then the entire device is encapsulated with a sealing film to obtain a niobium pentoxide-based capacitive ion diode.

[0086] The niobium pentoxide electrode prepared by the method described in this embodiment has a very significant ion screening effect in the trifluoromethanesulfonyl imide lithium electrolyte, that is, it exhibits a higher charge storage current in the low potential range, and only exhibits a very weak double-layer capacitance in the high potential range, indicating that the trifluoromethanesulfonyl imide ions in the electrolyte cannot be effectively stored inside the niobium pentoxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the niobium pentoxide electrode is mainly concentrated in the low potential range where the lithium ion contributes capacity, which further indicates that the niobium pentoxide electrode has good selective storage behavior for anions and cations in the electrolyte. According to calculations, the first-class rectification ratio of the niobium pentoxide electrode in the trifluoromethanesulfonyl imide lithium electrolyte is as high as 95, the second-class rectification ratio is as high as 98.5%, and the mass specific capacitance is as high as 575C / g, all of which are much higher than the previously reported porous carbon system. Such excellent ion rectification performance makes the capacitive ion diode assembled by niobium pentoxide electrodes exhibit ideal unidirectional energy storage behavior, and can be widely used in technical fields such as smart grids based on ion / electron coupling circuits, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc.

[0087] Example 3

[0088] In the first step, the prepared niobium pentoxide powder material, acetylene black and styrene-butadiene rubber were mixed in deionized water at a ratio of 7:2:1, and then the slurry was evenly coated on the gold sheet and the loading amount of the active substance was controlled to be 2 mg / cm 2 , and then dried in a blast oven to obtain a niobium pentoxide-based working electrode.

[0089] In the second step, the polymer derived carbon, Super-P and polytetrafluoroethylene were mixed in ethanol at a ratio of 8:1:1 and then the slurry was evenly coated on the nickel foam and the loading amount of the active substance was controlled to 4 mg / cm 2 , dried in a blast oven and cut to obtain a polymer-derived carbon-based counter electrode.

[0090] The third step is to select lithium perchlorate (LiClO4) as the electrolyte and a mixture of ethylene carbonate and propylene carbonate (volume ratio 1:1) as the solvent to prepare a 2 mol / L electrolyte; in this electrolyte, there is only Li + It can be stored efficiently in the niobium pentoxide electrode, so the niobium pentoxide electrode can exhibit obvious anion and cation screening effect.

[0091] The fourth step is to assemble the above-mentioned niobium pentoxide-based working electrode and polymer-derived carbon-based counter electrode into a button battery, and inject the prepared lithium perchlorate electrolyte into it, and then package the entire device with a battery sealing machine to obtain a niobium pentoxide-based capacitive ion diode.

[0092] The niobium pentoxide electrode prepared by the method described in this embodiment has a very significant ion screening effect in the lithium perchlorate electrolyte, that is, it exhibits a higher charge storage current in the low potential range, and only exhibits a very weak double-layer capacitance in the high potential range, indicating that the perchlorate ions in the electrolyte cannot be effectively stored inside the niobium pentoxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the niobium pentoxide electrode is mainly concentrated in the low potential range where the lithium ion contributes capacity, which further indicates that the niobium pentoxide electrode has good selective storage behavior for anions and cations in the electrolyte. According to calculations, the first-class rectification ratio of the niobium pentoxide electrode in the lithium perchlorate electrolyte is as high as 128, the second-class rectification ratio is as high as 97.8%, and the mass specific capacitance is as high as 712C / g, all of which are much higher than the previously reported porous carbon system. Such excellent ion rectification performance makes the capacitive ion diode assembled by niobium pentoxide electrodes exhibit ideal unidirectional energy storage behavior, and can be widely used in technical fields such as smart grids based on ion / electron coupling circuits, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc.

[0093] Example 4

[0094] In the first step, the prepared niobium pentoxide powder material, graphene nanosheets, and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a ratio of 7:2:1. The slurry was then evenly coated on copper foil and the loading amount of active substances was controlled to 2 mg / cm 2 , dried in a blast oven and cut to obtain a niobium pentoxide-based working electrode.

[0095] In the second step, commercial activated carbon, Super-P, and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a ratio of 7:2:1, and then the slurry was evenly coated on aluminum foil and the loading amount of active substances was controlled to 3 mg / cm 2 , dried in a forced air oven and cut to obtain an activated carbon-based counter electrode.

[0096] In the third step, lithium bis(fluorosulfonyl)imide (LiFSI) was selected as the electrolyte, and a mixture of diethylene glycol dimethyl ether and 1,3-dioxolane (volume ratio 1:1) was used as the solvent to prepare a 1 mol / L electrolyte. In this electrolyte, there is only Li + It can be stored efficiently in the niobium pentoxide electrode, so the niobium pentoxide electrode can exhibit obvious anion and cation screening effect.

[0097] The fourth step is to assemble the niobium pentoxide-based working electrode and the activated carbon-based counter electrode into a button battery, and inject the prepared lithium bis(fluorosulfonyl)imide electrolyte into it, and then seal the entire device with a battery sealing machine to obtain a niobium pentoxide-based capacitive ion diode.

[0098] The niobium pentoxide electrode prepared by the method described in this embodiment has a very significant ion screening effect in the bis(fluorosulfonyl)imide lithium electrolyte, that is, it exhibits a higher charge storage current in the low potential range, and only exhibits a very weak double-layer capacitance in the high potential range, indicating that the bis(fluorosulfonyl)imide ions in the electrolyte cannot be effectively stored inside the niobium pentoxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the niobium pentoxide electrode is mainly concentrated in the low potential range where the lithium ions contribute to the capacity, which further indicates that the niobium pentoxide electrode has good selective storage behavior for anions and cations in the electrolyte. According to calculations, the first-class rectification ratio of the niobium pentoxide electrode in the bis(fluorosulfonyl)imide lithium electrolyte is as high as 72, the second-class rectification ratio is as high as 96.6%, and the mass specific capacitance is as high as 616C / g, all of which are much higher than the previously reported porous carbon systems. Such excellent ion rectification performance makes the capacitive ion diode assembled by niobium pentoxide electrodes exhibit ideal unidirectional energy storage behavior, and can be widely used in technical fields such as smart grids based on ion / electron coupling circuits, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc.

[0099] Example 5

[0100] In the first step, the prepared molybdenum trioxide powder material, Super-P and polytetrafluoroethylene were mixed in ethanol at a ratio of 8:1:1, and then the slurry was evenly coated on the titanium foil and the loading amount of the active substance was controlled to 1 mg / cm 2 , dried in a blast oven and cut to obtain a molybdenum trioxide-based working electrode.

[0101] In the second step, commercial activated carbon, Super-P and polytetrafluoroethylene were mixed in ethanol at a ratio of 8:1:1, and then the slurry was evenly coated on the graphite foil and the loading amount of active substances was controlled to 2 mg / cm 2 , dried in a forced air oven and cut to obtain an activated carbon-based counter electrode.

[0102] The third step is to select sodium perchlorate (NaClO4) as the electrolyte and deionized water as the solvent to prepare a 17 mol / kg high-concentration salt electrolyte; in this electrolyte, there is only Na + It can be efficiently stored in the molybdenum trioxide electrode, so the molybdenum trioxide electrode can exhibit obvious anion and cation screening effect.

[0103] In the fourth step, the molybdenum trioxide-based working electrode and the activated carbon-based counter electrode are assembled in a stacked manner, and the prepared sodium perchlorate high-concentration salt electrolyte is injected therein, and then the entire device is encapsulated with a sealing film to obtain a molybdenum trioxide-based capacitive ion diode.

[0104] The molybdenum trioxide-based working electrode prepared by the method described in this embodiment has a very significant ion screening effect in the sodium perchlorate electrolyte, that is, it shows a higher charge storage current in the low potential interval, and only shows a very weak double-layer capacitance in the high potential interval, indicating that the perchlorate ions in the electrolyte cannot be effectively stored inside the molybdenum trioxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the molybdenum trioxide electrode is mainly concentrated in the low potential interval of the sodium ion contribution capacity, which further shows that the molybdenum trioxide electrode has good selective storage behavior for the anions and cations in the electrolyte. It is calculated that the first type of rectification ratio of the molybdenum trioxide electrode in the sodium perchlorate electrolyte is as high as 136, the second type of rectification ratio is as high as 97.2%, and the mass specific capacitance is as high as 448C / g, which are much higher than the porous carbon system reported previously. Such excellent ion rectification performance makes the capacitive ion diode assembled by the molybdenum trioxide electrode show an ideal unidirectional energy storage behavior, which can be widely used in the technical fields of smart grids, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc. based on ion / electronic coupling circuits.

[0105] Example 6

[0106] In the first step, the prepared molybdenum trioxide powder material and carbon nanotubes were mixed in a ratio of 9:1 and ultrasonically dispersed in N,N-dimethylformamide. After vacuum filtration, a self-supporting molybdenum trioxide film electrode was obtained. The loading amount of active substances was controlled to be 2 mg / cm 2 , dried in a blast oven and cut to obtain a molybdenum trioxide-based working electrode.

[0107] In the second step, commercial carbon nanotubes were ultrasonically dispersed in N,N-dimethylformamide, and then the same vacuum filtration method was used to obtain a self-supporting carbon nanotube film electrode, and the loading amount of active substances was controlled to 4 mg / cm 2 , dried in a forced air oven and cut to obtain a carbon nanotube-based electrode.

[0108] In the third step, lithium chloride (LiCl) is selected as the electrolyte, deionized water is used as the solvent, and polyvinyl alcohol is introduced to gel the electrolyte to prepare a 1 mol / L gel electrolyte; in this gel electrolyte, there is only Li + It can be efficiently stored in the molybdenum trioxide film electrode, so the molybdenum trioxide film electrode can exhibit obvious anion and cation screening effect.

[0109] In the fourth step, the self-supporting molybdenum trioxide-based working electrode and the self-supporting carbon nanotube-based counter electrode are assembled in a stacked manner, and a lithium chloride gel electrolyte is coated between the two electrodes. After that, the entire device is encapsulated with a sealing film to obtain a flexible molybdenum trioxide-based capacitive ion diode.

[0110] The molybdenum trioxide film electrode prepared by the method described in this embodiment has a very significant ion screening effect in the lithium chloride gel electrolyte, that is, it shows a higher charge storage current in the low potential range, and only shows a very weak double-layer capacitance in the high potential range, indicating that the chloride ions in the gel electrolyte cannot be effectively stored inside the molybdenum trioxide film electrode due to the ion screening effect. At the same time, the charge storage capacity of the molybdenum trioxide film electrode is mainly concentrated in the low potential range of the lithium ion contribution capacity, which further shows that the molybdenum trioxide film electrode has good selective storage behavior for the anions and cations in the gel electrolyte. According to calculations, the first type of rectification ratio of the molybdenum trioxide film electrode in the lithium chloride gel electrolyte is as high as 58, the second type of rectification ratio is as high as 94.8%, and the mass specific capacitance is as high as 628C / g, which are much higher than the previously reported porous carbon system. Such excellent ion rectification performance makes the capacitive ion diode assembled by the molybdenum trioxide film electrode show an ideal unidirectional energy storage behavior, which can be widely used in the technical fields of smart grids, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc. based on ion / electron coupling circuits.

[0111] Example 7

[0112] In the first step, the prepared titanium dioxide powder material, Super-P and polytetrafluoroethylene were mixed in ethanol at a ratio of 6:3:1, and then the slurry was evenly coated on the graphite foil and the loading amount of the active substance was controlled to 2 mg / cm 2 , dried in a forced air oven and cut to obtain a titanium dioxide-based working electrode.

[0113] In the second step, commercial activated carbon, acetylene black and polytetrafluoroethylene were mixed in ethanol at a ratio of 8:1:1, and then the slurry was evenly coated on the graphite foil and the loading amount of active substances was controlled to 4 mg / cm 2 , dried in a forced air oven and cut to obtain an activated carbon-based counter electrode.

[0114] In the third step, lithium trifluoromethanesulfonyl imide (LiTFSI) was selected as the electrolyte and deionized water was used as the solvent to prepare a high-concentration salt electrolyte of 21 mol / kg. In this electrolyte, there is only Li + It can be stored efficiently in the titanium dioxide electrode, so the titanium dioxide electrode can exhibit obvious anion and cation screening effect.

[0115] In the fourth step, the titanium dioxide-based working electrode and the activated carbon-based counter electrode are assembled in a stacked manner, and the prepared high-concentration lithium trifluoromethanesulfonyl imide salt electrolyte is injected therein, and then the entire device is encapsulated with a sealing film to obtain a titanium dioxide-based capacitive ion diode.

[0116] The titanium dioxide electrode prepared by the method described in this embodiment has a very significant ion screening effect in the trifluoromethanesulfonyl imide lithium electrolyte, that is, it exhibits a higher charge storage current in the low potential range, and only exhibits a very weak double-layer capacitance in the high potential range, indicating that the trifluoromethanesulfonyl imide ions in the electrolyte cannot be effectively stored inside the titanium dioxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the titanium dioxide electrode is mainly concentrated in the low potential range where the lithium ion contributes capacity, which further indicates that the niobium pentoxide electrode has good selective storage behavior for anions and cations in the electrolyte. According to calculations, the first-class rectification ratio of the titanium dioxide electrode in the trifluoromethanesulfonyl imide lithium electrolyte is as high as 188, the second-class rectification ratio is as high as 98.5%, and the mass specific capacitance is as high as 484C / g, all of which are much higher than the previously reported porous carbon system. Such excellent ion rectification performance makes the capacitive ion diode assembled by titanium dioxide electrodes exhibit ideal unidirectional energy storage behavior, and can be widely used in technical fields such as smart grids based on ion / electron coupling circuits, in vivo diagnosis and treatment, human-computer interfaces, neural network interactions, etc.

[0117] Example 8

[0118] In the first step, the prepared titanium dioxide powder material, Ketjen black and sodium carboxymethyl cellulose were mixed in deionized water at a ratio of 6:3:1, and then the slurry was evenly coated on the copper foil and the loading amount of the active substance was controlled to be 1 mg / cm 2 , dried in a forced air oven and cut to obtain a titanium dioxide-based working electrode.

[0119] In the second step, commercial activated carbon, Super-P and sodium alginate were mixed in deionized water at a ratio of 7:2:1, and then the slurry was evenly coated on aluminum foil and the loading amount of active substances was controlled to 2 mg / cm 2 , dried in a forced air oven and cut to obtain an activated carbon-based counter electrode.

[0120] In the third step, lithium hexafluorophosphate (LiPF6) was selected as the electrolyte, and a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate (volume ratio 1:1:1) was used as the solvent to prepare a 1 mol / L electrolyte; in this electrolyte, there is only Li + It can be stored efficiently in the titanium dioxide electrode, so the titanium dioxide electrode can exhibit obvious anion and cation screening effect.

[0121] The fourth step is to assemble the titanium dioxide-based working electrode and the activated carbon-based counter electrode into a button battery, and inject the prepared lithium hexafluorophosphate electrolyte into it, and then package the entire device with a battery sealing machine to obtain a titanium dioxide-based capacitive ion diode.

[0122] The titanium dioxide electrode prepared by the method described in this embodiment has a very significant ion screening effect in the lithium hexafluorophosphate electrolyte, that is, it shows a higher charge storage current in the low potential range, and only shows a very weak double-layer capacitance in the high potential range, indicating that the hexafluorophosphate ions in the electrolyte cannot be effectively stored inside the titanium dioxide electrode due to the ion screening effect. At the same time, the charge storage capacity of the titanium dioxide electrode is mainly concentrated in the low potential range of the lithium ion contribution capacity, which further shows that the titanium dioxide electrode has good selective storage behavior for the anions and cations in the electrolyte. According to calculations, the first type rectification ratio of the titanium dioxide electrode in the lithium hexafluorophosphate electrolyte is as high as 163, the second type rectification ratio is as high as 97.6%, and the mass specific capacitance is as high as 518C / g, which are much higher than the previously reported porous carbon system. Such excellent ion rectification performance makes the capacitive ion diode assembled from titanium dioxide electrodes show ideal unidirectional energy storage behavior, which can be widely used in technical fields such as smart grids, in vivo diagnosis and treatment, human-computer interfaces, and neural network interactions based on ion / electronic coupling circuits.

[0123] According to the disclosure and guidance of the above description, those skilled in the art to which the present invention belongs may also make changes and modifications to the above implementation modes. Therefore, the present invention includes but is not limited to the above embodiments, and any equivalent replacement or partial improvement made under the device construction principle of the present invention will fall within the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for convenience of description and do not constitute any limitation to the present invention.

Claims

1. A method for preparing a metal oxide based capacitive ion diode, characterized in that: include: A metal oxide-based working electrode and a porous carbon-based counter electrode are prepared, wherein the metal oxide used in the metal oxide-based working electrode is a metal oxide having intercalation pseudocapacitive behavior; Prepare an electrolyte, wherein only one type of ions among the anions and cations of the electrolyte can be stored in the metal oxide; the electrolyte in the electrolyte is an inorganic salt or an organic salt; The metal oxide-based working electrode and the porous carbon-based counter electrode are assembled and placed in the electrolyte, and then packaged to obtain a metal oxide-based capacitive ion diode.

2. The method for preparing a metal oxide based capacitive ion diode according to claim 1, characterized in that: The loading amount of the porous carbon-based counter electrode active material is 1 to 10 times the loading amount of the metal oxide-based working electrode active material.

3. The method for preparing a metal oxide based capacitive ion diode according to claim 1, characterized in that: The method comprises preparing a metal oxide-based working electrode, comprising: The metal oxide material is mixed with a conductive agent and a binder, and then a dispersant is added to obtain a slurry; The slurry is disposed on a current collector to obtain a metal oxide-based working electrode.

4. The method for preparing a metal oxide based capacitive ion diode according to claim 3, characterized in that: The mass ratio of the metal oxide material, the conductive agent and the binder is 6-9:1-3:

1.

5. The method for preparing a metal oxide based capacitive ion diode according to claim 3, characterized in that: The metal oxide material is at least one of niobium pentoxide, molybdenum trioxide, tungsten trioxide and titanium dioxide.

6. The method for preparing a metal oxide based capacitive ion diode according to claim 1, characterized in that: The method comprises preparing a porous carbon-based counter electrode, specifically comprising: The porous carbon material is mixed with a conductive agent and a binder, and then a dispersant is added to obtain a slurry; The slurry is disposed on a current collector to obtain a porous carbon-based counter electrode.

7. The method for preparing a metal oxide based capacitive ion diode according to claim 6, characterized in that: The mass ratio of the porous carbon material, the conductive agent and the binder is 6-9:1-3:

1.

8. The method for preparing a metal oxide based capacitive ion diode according to claim 1, characterized in that: The concentration of the electrolyte is 0.001~10 mol / L.

9. A metal oxide based capacitive ion diode prepared by the method for preparing a metal oxide based capacitive ion diode according to any one of claims 1 to 8.