A nickel-cobalt-manganese-aluminum quaternary precursor material and preparation method thereof and positive electrode material

Through the gradient structure design of the inner and outer layers of the nickel-cobalt-manganese-aluminum quaternary precursor material and Nb doping, the problem of lithium-nickel mixing and side reactions in high-nickel cathode materials is solved, the rate and cycle performance are improved, and the safety performance is enhanced.

CN116354418BActive Publication Date: 2024-10-11WUHU JIANA ENERGY TECHNOLOGY CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310577692.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-10-11
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

High-nickel ternary cathode materials are prone to lithium-nickel mixing, structural transformation and side reactions during the charge and discharge cycle, resulting in reduced cycle performance and rate performance, as well as safety risks.

Method used

It uses nickel, cobalt, manganese and aluminum quaternary precursor materials and is designed with a concentration gradient layered structure from inside to outside. The inner layer is high/ultra-high nickel, the middle layer is medium/high nickel, the outer layer is medium/low nickel, and the outer layer is made of medium/low nickel. The layers are doped with Nb metal to form a three-layer core-shell structure, which slows down structural transformation and side reactions and improves the stability and safety performance of the material.

Benefits of technology

The rate performance, cycle stability and safety performance of the nickel-cobalt-manganese-aluminum quaternary precursor material are improved, the lithium evolution phenomenon and side reactions are slowed down, and the structural stability and safety of the material are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354418B_ABST
    Figure CN116354418B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-ion batteries, and in particular to a nickel-cobalt-manganese-aluminum quaternary precursor material and a preparation method thereof and a positive electrode material. The nickel-cobalt-manganese-aluminum quaternary precursor material comprises an inner layer, an intermediate layer and an outer layer from the inside to the outside; the chemical formula of the inner layer is Ni a Co b Mn c Al 1‑a‑b‑c (OH)2, 0.94≥a≥0.8, b≥c≥1‑a‑b‑c>0; the chemical formula of the intermediate layer is Ni l Co m Mn n Al 1‑l‑m‑n (OH)2, 0.9≥l≥0.8, n≥m>0, 1‑l‑m‑n>0; the outer chemical formula is Ni w Co x Mn y Al z Nb 1‑w‑x‑y‑z (OH)2, 0.6≥w≥0.4, 0.1>x>0, 0.5≥y≥0.3, 0.2≥z≥0.05, 0.1≥1‑w‑x‑y‑z≥0.01; has excellent rate performance, cycle performance and safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a nickel-cobalt-manganese-aluminum quaternary precursor material and a preparation method thereof and a positive electrode material. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density and long life. They have become the mainstream direction of research and development in the field of new energy batteries and are developing very rapidly. However, as they develop rapidly, the performance requirements for lithium-ion batteries are becoming higher and higher. For example, in aerospace, military industry, electric vehicles and other fields, the requirements for the safety performance and rate performance of batteries and materials are becoming higher and higher.

[0003] Ternary cathode materials often use the method of increasing the nickel metal ratio in the precursor material to increase the energy density of the material. However, during the charge and discharge cycle of high-nickel ternary cathode materials, due to the 2+ Radius and Li + The radius is close, and Ni is very likely to occur 2+ Occupy Li + The situation at the point, that is, lithium-nickel mixing, cation mixing leads to a reduction in lattice spacing, which reduces the lithium ion channel and hinders the free insertion and extraction of lithium ions, thereby reducing the cycle performance and rate performance of the battery. The delithiation of electrode materials starts from the surface, and as the charging progresses, the surface structure shows the phenomenon of excessive delithiation. At the same time, the layered structure of high-nickel ternary materials changes to spinel structure and inert rock salt structure.

[0004] Structural changes and blocked transfer paths can also lead to lithium precipitation. In addition, the highly oxidizing high-valent transition metal ions on the surface react seriously with the electrolyte to produce gas, causing the battery to be filled with gas. The more severe the reaction is under conditions of excessive charge and discharge, the more safety risks will arise.

[0005] The quaternary nickel-cobalt-manganese-aluminum cathode material adds aluminum to the ternary material, and performs well on high-nickel and ultra-high-nickel cathode materials. Its performance is better than that of nickel-cobalt-manganese and nickel-cobalt-aluminum materials. The strength of the Al-O bond is stronger than that of the Ni(Co, Mn)-O bond, which can greatly improve the thermal stability of the material. However, the structural transformation caused by the mixing of lithium and nickel and the battery inflation caused by side reactions have not been significantly improved.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a nickel-cobalt-manganese-aluminum quaternary precursor material, which improves the crystal structure of the high-nickel positive electrode precursor material and improves the rate performance, cycle performance and safety performance.

[0008] The second object of the present invention is to provide a method for preparing the above-mentioned nickel-cobalt-manganese-aluminum quaternary precursor material, which can obtain a nickel-cobalt-manganese-aluminum quaternary precursor material with good sphericity, large specific surface area and consistent morphology.

[0009] The third object of the present invention is to provide a positive electrode material having excellent electrochemical performance and safety performance.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] The present invention provides a nickel-cobalt-manganese-aluminum quaternary precursor material, which includes an inner layer, a middle layer and an outer layer from the inside to the outside;

[0012] The chemical formula of the inner layer is Ni a Co b Mn c Al 1-a-b-c (OH)2, 0.94≥a≥0.8, b≥c≥1-abc>0;

[0013] The chemical formula of the intermediate layer is Ni l Co m Mn n Al 1-l-m-n (OH)2, 0.9≥l≥0.8, n≥m>0, 1-lmn>0;

[0014] The chemical formula of the outer layer is Ni w Co x Mn y Al z Nb 1-w-x-y-z (OH)2, 0.6≥w≥0.4, 0.1>x>0, 0.5≥y≥0.3, 0.2≥z≥0.05, 0.1≥1-wxyz≥0.01.

[0015] Furthermore, the thickness of the inner layer is 0.5 to 2 μm, the thickness of the middle layer is 3 to 12 μm, and the thickness of the outer layer is 1 to 4 μm.

[0016] Furthermore, the specific surface area of ​​the nickel-cobalt-manganese-aluminum quaternary precursor material is >50m 2 / g.

[0017] The present invention also provides a method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material as described above, comprising the following steps:

[0018] S1. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the bottom liquid to carry out a first coprecipitation reaction to obtain a reaction solution I;

[0019] S2. In an atmosphere containing oxygen, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the reaction solution I to carry out a second coprecipitation reaction to obtain a reaction solution II;

[0020] S3. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing Al source, a solution containing Nb source, a sodium hydroxide solution and ammonia water are introduced into the reaction solution II to carry out a third coprecipitation reaction, and the nickel-cobalt-manganese-aluminum quaternary precursor material is obtained after aging.

[0021] Furthermore, in step S1, the conditions of the first coprecipitation reaction are: the pH of the reaction system is 11.5-12.2, and the NH4 + The concentration is 6-8 g / L, the reaction temperature is 45-55°C, and the reaction time is 1-6 h.

[0022] Furthermore, in step S2, the volume percentage of oxygen in the oxygen-containing atmosphere is 3% to 8%.

[0023] Furthermore, in step S2, the conditions of the second coprecipitation reaction are: the pH of the reaction system is 11 to 12.5, and the NH4 + The concentration is 5-10 g / L, the reaction temperature is 50-60°C, and the reaction time is 12-76 h.

[0024] Further, in step S3, the conditions of the third coprecipitation reaction are: the pH of the reaction system is 10.8-12, and the NH4 + The concentration is 4-7 g / L, the reaction temperature is 48-58°C, and the reaction time is 8-24 h.

[0025] Furthermore, in step S1 and step S2, the sum of the metal concentration of the solution containing Ni salt, Co salt and Mn salt and the metal concentration of the solution containing Al source is 1.5-2 mol / L;

[0026] In step S3, the sum of the metal concentration of the solution containing Ni salt, Co salt and Mn salt, the metal concentration of the solution containing Al source and the metal concentration of the solution containing Nb source is 1.5-2 mol / L.

[0027] Preferably, the concentration of the sodium hydroxide solution is 6 to 12 mol / L.

[0028] Preferably, the concentration of the ammonia water is 5 to 10 mol / L.

[0029] Preferably, the Nb source includes at least one of Nb2O5, NbO2, Nb2O3 and NbO.

[0030] The present invention also provides a positive electrode material, which is mainly prepared from the nickel-cobalt-manganese-aluminum quaternary precursor material as described above.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention is a concentration gradient layered material with a high / ultra-high nickel inner layer, a medium / high nickel middle layer, and a medium / low nickel outer layer; from the inside to the outside, the Ni content gradually decreases, which is beneficial to improving the specific capacity of the precursor material, stabilizing its structure, and improving the rate performance and cycle stability of the material.

[0033] The outer layer of the nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention is a medium / low nickel material supported by a Nb metal structure. The doping of Nb metal can slow down the structural transformation of the crystal and the occurrence of lithium precipitation during the charge and discharge process, improve the crystal structure of the high-nickel positive electrode precursor material, and achieve the purpose of improving the cycle performance and rate performance; and the Nb-doped medium / low nickel outer layer structure isolates the internal high-nickel material from direct contact with the electrolyte, alleviates the safety problem caused by battery inflation caused by battery side reactions, and improves the safety performance.

[0034] The preparation method of the nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention can obtain a nickel-cobalt-manganese-aluminum quaternary precursor with good sphericity, consistent morphology and large specific surface area; during the generation of the intermediate layer, an appropriate amount of oxygen is introduced to increase the specific surface area of ​​the material, thereby improving the rate performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is a schematic flow chart of the method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material of Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0038] The following is a detailed description of a nickel-cobalt-manganese-aluminum quaternary precursor material, a preparation method thereof, and a positive electrode material according to an embodiment of the present invention.

[0039] In some embodiments of the present invention, a nickel-cobalt-manganese-aluminum quaternary precursor material is provided, which includes, from inside to outside, an inner layer, a middle layer, and an outer layer;

[0040] The chemical formula of the inner layer is Ni a Co b Mn c Al 1-a-b-c (OH)2, 0.94≥a≥0.8, b≥c≥1-abc>0;

[0041] The chemical formula of the middle layer is Ni l Co m Mn n Al 1-l-m-n (OH)2, 0.9≥l≥0.8, n≥m>0, 1-lmn>0;

[0042] The chemical formula of the outer layer is Ni w Co x Mn y Al z Nb 1-w-x-y-z (OH)2, 0.6≥w≥0.4, 0.1>x>0, 0.5≥y≥0.3, 0.2≥z≥0.05, 0.1≥1-wxyz≥0.01.

[0043] The nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention is a concentration gradient layered material with a high / ultra-high nickel inner layer, a medium / high nickel middle layer, and a medium / low nickel outer layer; it is a three-layer core-shell structure, and the Ni content gradually decreases from the inside to the outside; the internal nickel content is relatively high, providing the material with a high specific capacity; the nickel content gradually decreases from the inside to the outside, and the manganese content gradually increases, thereby improving the structural stability of the material; in addition, the doping of the outermost layer of niobium element inhibits the phase change after delithiation from the outside to the inside, thereby obtaining a gradient material with excellent comprehensive performance.

[0044] The outer layer of the nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention is a medium / low nickel material supported by a Nb metal structure. The doping of Nb metal can slow down the structural transformation and lithium precipitation of the crystal during the charge and discharge process, improve the crystal structure of the high-nickel positive electrode precursor material, and inhibit cation mixing and excessive lithium removal from the surface layer, thereby inhibiting the layered structure transformation of the high-nickel positive electrode precursor material, thereby achieving the purpose of improving the cycle performance and rate performance. The Nb-doped medium / low nickel outer layer structure prevents the high-nickel material (middle layer) inside the material from directly contacting the electrolyte, improves the side reaction of the material with the electrolyte, alleviates the safety problem caused by battery inflation caused by the battery side reaction, and improves the safety performance.

[0045] In some embodiments of the present invention, the thickness of the inner layer is 0.5-2 μm, the thickness of the middle layer is 3-12 μm, and the thickness of the outer layer is 1-4 μm; typically but not restrictively, for example, the thickness of the inner layer of the nickel-cobalt-manganese-aluminum quaternary precursor material may be 0.5 μm, 1 μm, 1.5 μm, 2 μm or a range consisting of any two thereof; the thickness of the middle layer of the nickel-cobalt-manganese-aluminum quaternary precursor material may be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm or a range consisting of any two thereof; the thickness of the outer layer of the nickel-cobalt-manganese-aluminum quaternary precursor material may be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or a range consisting of any two thereof.

[0046] The ultra-high nickel inner layer with a thickness of 0.5 to 2 μm provides a growth point for the middle layer, and exhibits a specific capacity that is better than that of the middle layer material; at the same time, the higher the nickel content, the more serious the lithium-nickel mixing. Therefore, the smaller the thickness of the inner layer, the more it can slow down the degree of lithium-nickel mixing that occurs under ultra-high nickel content.

[0047] The intermediate layer with a thickness of 3 to 12 μm is the main structural position for storing lithium ions and providing energy. Therefore, a relatively thick intermediate layer can achieve this purpose. In addition, the intermediate layer also plays a transitional role in reducing the nickel content from high nickel / ultra-high nickel to medium nickel / medium-low nickel.

[0048] The outer layer is the key structural position for modification, and its thickness mostly depends on the desired effect. The thicker the doping layer, the better the modification effect and the greater the reduction in specific capacity.

[0049] In some embodiments of the present invention, the (BET) specific surface area of ​​the nickel-cobalt-manganese-aluminum quaternary precursor material is greater than 50 m 2 / g.

[0050] In some embodiments of the present invention, the particle size of the nickel-cobalt-manganese-aluminum quaternary precursor material is 4.5 to 18 μm.

[0051] The nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention has a large specific surface area, which is beneficial to enhancing the rate performance of the material.

[0052] In some embodiments of the present invention, a method for preparing the above nickel-cobalt-manganese-aluminum quaternary precursor material is also provided, comprising the following steps:

[0053] S1. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the bottom liquid to carry out a first coprecipitation reaction to obtain a reaction solution I;

[0054] S2. In an atmosphere containing oxygen, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the reaction solution I to carry out a second coprecipitation reaction to obtain a reaction solution II;

[0055] S3. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing Al source, a solution containing Nb source, a sodium hydroxide solution and ammonia water are introduced into the reaction solution II to carry out a third coprecipitation reaction, and a nickel-cobalt-manganese-aluminum quaternary precursor material is obtained after aging.

[0056] The present invention firstly adopts a salt solution, a complexing agent and a precipitant to generate an inner layer, then adopts a salt solution, a complexing agent and a precipitant to coat the inner layer to generate an intermediate layer, and then adopts a salt solution, a solution containing a Nb source, a complexing agent and a precipitant to coat the intermediate layer to obtain an outer layer; and the reaction process is precisely controlled to obtain a nickel-cobalt-manganese-aluminum quaternary precursor with good sphericity, consistent morphology and large specific surface area.

[0057] In the second coprecipitation reaction, that is, the process of generating the intermediate layer, the present invention increases the specific surface area of ​​the material by introducing a proper amount of oxygen, thereby improving the rate performance of the material.

[0058] In some embodiments of the present invention, the base liquid includes water, NaOH and NH3·H2O. The base liquid is mainly obtained by mixing water, ammonia water and liquid alkali.

[0059] In some embodiments of the present invention, in step S1, the inert gas includes nitrogen. Nitrogen is used as a protective gas during the reaction.

[0060] In some embodiments of the present invention, in step S1, the conditions for the first coprecipitation reaction are: the pH of the reaction system is 11.5 to 12.2, and the NH4 + The concentration is 6-8 g / L, the reaction temperature is 45-55°C, and the reaction time is 1-6 h.

[0061] In some specific embodiments of the present invention, in step S1, the stirring rate of the first coprecipitation reaction is 400-600 rpm.

[0062] In some specific embodiments of the present invention, in step S1, the first coprecipitation reaction includes: continuously introducing a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and ammonia water into the bottom liquid for reaction for 1 to 6 hours, stopping the feeding and continuing stirring for 0.5 to 1 hour.

[0063] In some embodiments of the present invention, in step S2, the volume percentage of oxygen in the atmosphere containing oxygen is 3% to 8%; preferably, the atmosphere containing oxygen includes nitrogen and oxygen.

[0064] In some embodiments of the present invention, in step S2, the conditions for the second coprecipitation reaction are: the pH of the reaction system is 11 to 12.5, and the NH4 + The concentration is 5-10 g / L, the reaction temperature is 50-60°C, and the reaction time is 12-76 h.

[0065] In some specific embodiments of the present invention, in step S2, the stirring rate of the second coprecipitation reaction is 200-400 rpm.

[0066] In some specific embodiments of the present invention, in step S2, the second coprecipitation reaction includes: continuously introducing a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and an ammonia solution into the reaction solution I for 12 to 72 hours, stopping the feeding and continuing stirring for 2 to 4 hours.

[0067] In some embodiments of the present invention, in step S3, the inert gas includes nitrogen. Nitrogen is used as a protective gas during the reaction.

[0068] In some embodiments of the present invention, in step S3, the conditions for the third coprecipitation reaction are: the pH of the reaction system is 10.8-12, and the NH4 + The concentration is 4-7 g / L, the reaction temperature is 48-58°C, and the reaction time is 8-24 h.

[0069] In some specific embodiments of the present invention, in step S3, the stirring rate of the third coprecipitation reaction is 50-120 rpm.

[0070] In some specific embodiments of the present invention, in step S3, a solution containing Ni salt, Co salt and Mn salt, a solution containing Al source, a solution containing Nb source, sodium hydroxide solution and ammonia water are continuously introduced into the reaction liquid II to react for 8 to 24 hours, and then the feeding is stopped, and aging, filtering, washing and drying are carried out in sequence to obtain a nickel-cobalt-manganese-aluminum quaternary precursor material.

[0071] In some specific embodiments of the present invention, in step S3, the aging time is 20 to 36 hours; the filtering method includes filter pressing and / or centrifugation; the drying temperature is 100 to 130° C., and the drying time is 10 to 24 hours.

[0072] In some embodiments of the present invention, in step S1 and step S2, the sum of the metal concentration of the solution containing the Ni salt, the Co salt and the Mn salt and the metal concentration of the solution containing the Al source is 1.5-2 mol / L.

[0073] In some embodiments of the present invention, in step S1, the molar ratio of Ni, Co and Mn in the solution containing Ni salt, Co salt and Mn salt is a:b:c; the molar ratio of Ni in the solution containing Ni salt, Co salt and Mn salt to Al in the solution containing Al source is a:1-abc.

[0074] In some embodiments of the present invention, in step S2, the molar ratio of Ni, Co and Mn in the solution containing Ni salt, Co salt and Mn salt is 1:m:n; the molar ratio of Ni in the solution containing Ni salt, Co salt and Mn salt to Al in the solution containing Al source is 1:1-1mn.

[0075] In some embodiments of the present invention, in step S3, the sum of the metal concentrations of the solution containing Ni salt, Co salt and Mn salt, the metal concentration of the solution containing Al source and the metal concentration of the solution containing Nb source is 1.5-2 mol / L.

[0076] In some embodiments of the present invention, in step S3, the molar ratio of Ni, Co and Mn in the solution containing Ni salt, Co salt and Mn salt is w:x:y; the molar ratio of Ni in the solution containing Ni salt, Co salt and Mn salt to Al in the solution containing Al source is w:z; the molar ratio of Ni in the solution containing Ni salt, Co salt and Mn salt to Nb in the solution containing Nb source is w:1-wxyz.

[0077] In some embodiments of the present invention, the Ni salt includes at least one of nickel sulfate, nickel nitrate and nickel chloride.

[0078] In some embodiments of the present invention, the Co salt includes at least one of cobalt sulfate, cobalt nitrate and cobalt chloride.

[0079] In some embodiments of the present invention, the Mn salt includes at least one of manganese sulfate, manganese nitrate, and manganese chloride.

[0080] In some embodiments of the present invention, the solution containing the Al source includes a sodium aluminate solution; preferably, the solution containing the Al source is mainly obtained by mixing at least one of aluminum hydroxide, aluminum sulfate, aluminum chloride, aluminum nitrate and aluminum oxide with a sodium hydroxide solution.

[0081] In some embodiments of the present invention, the solution containing the Nb source is mainly obtained by mixing an aqueous solution of at least one of a carbonate and a hydroxide with a Nb source; the Nb source includes at least one of Nb2O5, NbO2, Nb2O3 and NbO; the carbonate includes sodium carbonate and / or potassium carbonate, and the hydroxide includes sodium hydroxide and / or potassium hydroxide.

[0082] In some embodiments of the present invention, in steps S1 to S3, the concentration of the sodium hydroxide solution is 6 to 12 mol / L.

[0083] In some embodiments of the present invention, in steps S1 to S3, the concentration of aqueous ammonia is 5 to 10 mol / L.

[0084] In some embodiments of the present invention, in steps S1 to S3, the feed rate of the solution containing Ni salt, Co salt and Mn salt is 200 to 500 L / h; the feed rate of the solution containing Al source is 20 to 100 L / h, and the feed rate of the solution containing Nb source is 20 to 100 L / h; the feed rate of sodium hydroxide solution is 120 to 200 L / h; and the feed rate of ammonia water is 10 to 60 L / h.

[0085] In some embodiments of the present invention, a positive electrode material is also provided, which is mainly prepared from the above-mentioned nickel-cobalt-manganese-aluminum quaternary precursor material.

[0086] In some embodiments of the present invention, a method for preparing a positive electrode material is also provided, comprising the following steps:

[0087] The nickel-cobalt-manganese-aluminum quaternary precursor material and lithium hydroxide are sintered.

[0088] In some embodiments of the present invention, the sintering includes pre-sintering at 400-600° C. for 5-10 hours in an oxygen-rich environment (oxygen concentration ≥ 99.99%) and then sintering at 680-900° C. for 15-24 hours.

[0089] In some embodiments of the present invention, typically but not limitatively, for example, the pre-sintering temperature is 400°C, 450°C, 500°C, 550°C, 600°C or a range consisting of any two thereof; the pre-sintering time is 5h, 6h, 7h, 8h, 9h, 10h or a range consisting of any two thereof; the sintering temperature is 700°C, 750°C, 800°C, 850°C, 900°C or a range consisting of any two thereof; the sintering time is 15h, 18h, 20h, 22h, 24h or a range consisting of any two thereof.

[0090] In some embodiments of the present invention, a lithium-ion battery is provided, comprising the above-mentioned positive electrode material.

[0091] Example 1

[0092] Solution A: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.94:0.02:0.02, and dissolved in pure water to prepare a 1.96 mol / L solution.

[0093] Solution B: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution A of 0.02:0.94, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.24 mol / L solution.

[0094] Solution C: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.89:0.01:0.08, and dissolved in pure water to prepare a 1.96 mol / L solution.

[0095] Solution D: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution C of 0.02:0.89, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.24 mol / L solution.

[0096] Solution E: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.6:0.03:0.3, and dissolved in pure water to prepare a 1.86 mol / L solution.

[0097] Solution F: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution E of 0.05:0.6, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 1.2 mol / L solution.

[0098] Solution G: Nb2O5 was weighed according to the molar ratio of Nb to Ni in solution E of 0.02:0.6, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.48 mol / L solution.

[0099] Base solution: obtained by mixing pure water, 8.3 mol / L ammonia water and 10.8 mol / L liquid alkali; the pH of the base solution is 12.1, and the ammonium concentration is 7 g / L.

[0100] The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this embodiment comprises the following steps:

[0101] S1. Under nitrogen atmosphere, solution A, solution B, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into a reactor containing a bottom liquid (the volume of the bottom liquid accounted for 50% of the volume of the reactor) at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out the first coprecipitation reaction (inner layer precipitation). The conditions of the first coprecipitation reaction were: the pH of the system was 12.1, the NH4 + The concentration is 7 g / L; the temperature is 50°C, the stirring speed is 600 rpm, and the reaction time is 6 h; then the feed is closed and stirring is continued for 1 h to obtain reaction solution I;

[0102] S2, compressed air and nitrogen were introduced, and in an atmosphere with an oxygen volume fraction of 8%, solution C, solution D, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the above reaction solution I at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out a second coprecipitation reaction (intermediate layer precipitation). The conditions for the second coprecipitation reaction were: the pH of the system was 11.8, and the NH4 + The concentration is 6 g / L; the temperature is 50°C, the stirring speed is 400 rpm, and the reaction time is 70 h; then the feed is closed and stirring is continued for 4 h to obtain reaction solution II;

[0103] S3. Under nitrogen atmosphere, solution E, solution F, solution G, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the reaction solution II at flow rates of 480 L / h, 40 L / h, 40 L / h, 178 L / h and 35 L / h, respectively, to carry out the third coprecipitation reaction. The conditions of the third coprecipitation reaction were as follows: the pH of the system was 10.8, and the NH4 + The concentration is 4g / L; the temperature is 55°C, the stirring speed is 50rmp, and the reaction time is 20h; then the feed is closed and transferred to the aging tank for aging for 24h. After the aging is completed, centrifugation, washing and drying at 125°C for 20h are carried out in sequence to obtain a nickel-cobalt-manganese-aluminum quaternary precursor material.

[0104] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:

[0105] The above-mentioned nickel-cobalt-manganese-aluminum quaternary precursor material and lithium hydroxide monohydrate were weighed according to a molar ratio of 1.09:1, pre-sintered at 400°C for 8h and sintered at 700°C for 24h in an oxygen-rich environment to obtain a positive electrode material.

[0106] The schematic diagram of the process for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material of this embodiment is as follows Figure 1 shown.

[0107] Example 2

[0108] Solution A: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.9:0.04:0.04, and dissolved in pure water to prepare a 1.96 mol / L solution.

[0109] Solution B: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution A of 0.02:0.9, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.24 mol / L solution.

[0110] Solution C: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.82:0.01:0.12, and dissolved in pure water to prepare a 1.9 mol / L solution.

[0111] Solution D: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution C of 0.01:0.82, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.6 mol / L solution.

[0112] Solution E: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to a molar ratio of Ni:Co:Mn=0.5:0.05:0.3 and dissolved in pure water to prepare a 1.7 mol / L solution.

[0113] Solution F: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution E of 0.1:0.5, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 2.4 mol / L solution.

[0114] Solution G: Nb2O5 was weighed according to the molar ratio of Nb to Ni in solution E of 0.05:0.5, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 1.2 mol / L solution.

[0115] Base solution: obtained by mixing pure water, 8.3 mol / L ammonia water and 10.8 mol / L liquid alkali; the pH of the base solution is 12.2, and the ammonium concentration is 8 g / L.

[0116] The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this embodiment comprises the following steps:

[0117] S1. Under nitrogen atmosphere, solution A, solution B, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into a reactor containing a bottom liquid (the volume of the bottom liquid accounted for 50% of the volume of the reactor) at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out the first coprecipitation reaction. The conditions of the first coprecipitation reaction were: the pH of the system was 12.2, the NH4 + The concentration is 8 g / L; the temperature is 54°C, the stirring speed is 600 rpm, and the reaction time is 4 h; then the feed is closed and stirring is continued for 1 h to obtain reaction solution I;

[0118] S2, in an atmosphere with an oxygen volume fraction of 6%, solution C, solution D, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the reaction solution I at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out a second coprecipitation reaction. The conditions for the second coprecipitation reaction were as follows: the pH of the system was 12.4, and the NH4 + The concentration is 9 g / L; the temperature is 58°C, the stirring speed is 300 rpm, and the reaction time is 54 h; then the feed is closed and stirring is continued for 3 h to obtain reaction solution II;

[0119] S3. Under nitrogen atmosphere, solution E, solution F, solution G, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the reaction solution II at flow rates of 480 L / h, 40 L / h, 40 L / h, 178 L / h and 35 L / h, respectively, to carry out the third coprecipitation reaction. The conditions of the third coprecipitation reaction were as follows: the pH of the system was 11.5, and the NH4 + The concentration is 7g / L; the temperature is 55°C, the stirring speed is 80rmp, and the reaction time is 15h; then the feed is closed and transferred into the aging tank for aging for 20h. After the aging is completed, centrifugation, washing and drying at 125°C for 20h are performed in sequence to obtain a nickel-cobalt-manganese-aluminum quaternary precursor material.

[0120] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:

[0121] The above nickel-cobalt-manganese-aluminum quaternary precursor material and lithium hydroxide monohydrate were weighed according to a molar ratio of 1.03:1, pre-sintered at 600°C for 6 hours and sintered at 760°C for 20 hours in an oxygen-rich environment to obtain a positive electrode material.

[0122] Example 3

[0123] Solution A: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.85:0.06:0.05, and dissolved in pure water to prepare a 1.92 mol / L solution.

[0124] Solution B: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution A of 0.04:0.85, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.48 mol / L solution.

[0125] Solution C: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.8:0.02:0.12, and dissolved in pure water to prepare a 1.88 mol / L solution.

[0126] Solution D: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution C of 0.06:0.8, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 0.72 mol / L solution.

[0127] Solution E: Nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.4:0.03:0.4, and dissolved in pure water to prepare a 1.66 mol / L solution.

[0128] Solution F: Aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution E of 0.1:0.4, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 2.4 mol / L solution.

[0129] Solution G: Nb2O5 was weighed according to the molar ratio of Nb to Ni in solution E of 0.07:0.4, dissolved in 6 mol / L sodium hydroxide solution, and a certain amount of pure water was added to prepare a 1.68 mol / L solution.

[0130] Base solution: obtained by mixing pure water, 8.3 mol / L ammonia water and 10.8 mol / L liquid alkali; the pH of the base solution is 11.8, and the ammonium concentration is 6 g / L.

[0131] The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this embodiment comprises the following steps:

[0132] S1. Under nitrogen atmosphere, solution A, solution B, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into a reactor containing a bottom liquid (the volume of the bottom liquid accounted for 50% of the volume of the reactor) at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out the first coprecipitation reaction. The conditions of the first coprecipitation reaction were as follows: the pH of the system was 11.8, the NH4 +The concentration is 6 g / L; the temperature is 48°C, the stirring speed is 400 rpm, and the reaction time is 2 h; then the feed is closed and stirring is continued for 0.5 h to obtain reaction solution I;

[0133] S2, in an atmosphere with an oxygen volume fraction of 4%, solution C, solution D, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the reaction solution I at flow rates of 480 L / h, 80 L / h, 178 L / h and 35 L / h, respectively, to carry out a second coprecipitation reaction. The conditions for the second coprecipitation reaction were as follows: the pH of the system was 12, the NH4 + The concentration is 7 g / L; the temperature is 52°C, the stirring speed is 200 rpm, and the reaction time is 36 h; then the feed is closed and stirring is continued for 2 h to obtain reaction solution II;

[0134] S3. Under nitrogen atmosphere, solution E, solution F, solution G, 10.8 mol / L sodium hydroxide solution and 8.3 mol / L ammonia water were introduced into the reaction solution II at flow rates of 480 L / h, 40 L / h, 40 L / h, 178 L / h and 35 L / h, respectively, to carry out the third coprecipitation reaction. The conditions of the third coprecipitation reaction were as follows: the pH of the system was 11.2, and the NH4 + The concentration is 5g / L; the temperature is 48°C, the stirring speed is 100rmp, and the reaction time is 10h; then the feed is closed and transferred to the aging tank for aging for 24h. After the aging is completed, centrifugation, washing and drying at 125°C for 20h are performed in sequence to obtain a nickel-cobalt-manganese-aluminum quaternary precursor material.

[0135] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:

[0136] The above nickel-cobalt-manganese-aluminum quaternary precursor material and lithium hydroxide monohydrate were weighed according to a molar ratio of 1.06:1, pre-sintered at 500° C. for 9 h and sintered at 850° C. for 20 h in an oxygen-rich environment to obtain a positive electrode material.

[0137] Comparative Example 1

[0138] The preparation method of the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this comparative example refers to Example 3, except that in step S3, solution G is not introduced.

[0139] The preparation method of the positive electrode material provided in this comparative example refers to Example 3, the only difference being that the nickel-cobalt-manganese-aluminum quaternary precursor material of this comparative example is used.

[0140] Comparative Example 2

[0141] The preparation method of the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this comparative example refers to Example 3, except that in solution A, nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate are weighed according to a molar ratio of Ni:Co:Mn=0.6:0.5:0.15; in solution B, aluminum hydroxide is weighed according to a molar ratio of Al to Ni in solution A of 0.2:0.6; in solution C, nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate monohydrate are weighed according to a molar ratio of Ni:Co:Mn=0.4:0.15:0.3 In solution D, aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution C of 0.15:0.4; in solution E, nickel sulfate hexahydrate, cobalt sulfate heptahydrate and manganese sulfate monohydrate were weighed according to the molar ratio of Ni:Co:Mn=0.7:0.05:0.05; in solution F, aluminum hydroxide was weighed according to the molar ratio of Al to Ni in solution E of 0.15:0.7; in solution G, Nb2O5 was weighed according to the molar ratio of Nb to Ni in solution E of 0.05:0.7.

[0142] The preparation method of the positive electrode material provided in this comparative example refers to Example 3, the only difference being that the nickel-cobalt-manganese-aluminum quaternary precursor material of this comparative example is used.

[0143] Comparative Example 3

[0144] The preparation method of the nickel-cobalt-manganese-aluminum quaternary precursor material provided in this comparative example refers to Example 3, with the only difference being that in step S2, the atmosphere with an oxygen volume fraction of 8% is replaced by a nitrogen atmosphere.

[0145] The preparation method of the positive electrode material provided in this comparative example refers to Example 3, the only difference being that the nickel-cobalt-manganese-aluminum quaternary precursor material of this comparative example is used.

[0146] Test Example 1

[0147] The nickel-cobalt-manganese-aluminum quaternary precursor materials of Examples 1 to 3 and Comparative Examples 1 to 3 were characterized, and the results are shown in Table 1.

[0148] Table 1

[0149]

[0150] It can be seen from Table 1 that the nickel-cobalt-manganese-aluminum quaternary precursor material of the present invention has the advantage of a large specific surface area.

[0151] Test Example 2

[0152] The electrochemical properties of the positive electrode materials of Examples 1 to 3 and Comparative Examples 1 to 3 were tested, and the results are shown in Table 2.

[0153] The positive electrode material, PVDF and acetylene black were mixed in a mass ratio of 8:1:1 to prepare slurry. The organic solvent, electrolyte LiPF6 and additives were mixed in a mass ratio of 0.85:0.1:0.05, wherein the organic solvent was an organic mixture of ethyl methyl carbonate, ethylene carbonate and dimethyl carbonate in a mass ratio of 0.5:0.3:0.2. The negative electrode was graphite and the separator was polyethylene.

[0154] The above materials were assembled into 2032 button cells in a glove box and tested on the LAND battery testing system.

[0155] Table 2

[0156]

[0157]

[0158] It can be seen from Table 2 that the positive electrode material of the present invention has excellent rate performance, cycle performance and safety performance.

[0159] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A nickel-cobalt-manganese-aluminum quaternary precursor material, characterized in that: From inside to outside, it includes inner layer, middle layer and outer layer; The chemical formula of the inner layer is Ni a Co b Mn c Al 1-a-b-c (OH)2, 0.94≥a≥0.8, b≥c≥1-abc>0; The chemical formula of the intermediate layer is Ni l Co m Mn n Al 1-l-m-n (OH)2, 0.9≥l≥0.8, n≥m>0, 1-lmn>0; The chemical formula of the outer layer is Ni w Co x Mn y Al z Nb 1-w-x-y-z (OH)2, 0.6≥w≥0.4, 0.1>x>0, 0.5≥y≥0.3, 0.2≥z≥0.05, 0.1≥1-wxyz≥0.01; The thickness of the inner layer is 0.5-2 μm, the thickness of the middle layer is 5-12 μm, and the thickness of the outer layer is 1-4 μm; The specific surface area of ​​the nickel-cobalt-manganese-aluminum quaternary precursor material is greater than 50 m 2 / g.

2. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 1, characterized in that: The steps include: S1. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the bottom liquid to carry out a first coprecipitation reaction to obtain a reaction solution I; S2. In an atmosphere containing oxygen, a solution containing Ni salt, Co salt and Mn salt, a solution containing an Al source, a sodium hydroxide solution and aqueous ammonia are introduced into the reaction solution I to carry out a second coprecipitation reaction to obtain a reaction solution II; S3. Under an inert atmosphere, a solution containing Ni salt, Co salt and Mn salt, a solution containing Al source, a solution containing Nb source, a sodium hydroxide solution and aqueous ammonia are introduced into the reaction solution II to carry out a third coprecipitation reaction, and the nickel-cobalt-manganese-aluminum quaternary precursor material is obtained after aging; In step S2, the volume percentage of oxygen in the oxygen-containing atmosphere is 3% to 8%; In step S1 and step S2, the sum of the metal concentration of the solution containing Ni salt, Co salt and Mn salt and the metal concentration of the solution containing Al source is 1.5-2 mol / L; In step S3, the sum of the metal concentration of the solution containing Ni salt, Co salt and Mn salt, the metal concentration of the solution containing Al source and the metal concentration of the solution containing Nb source is 1.5-2 mol / L.

3. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: In step S1, the conditions of the first coprecipitation reaction are: the pH of the reaction system is 11.5-12.2, and the NH4 + The concentration is 6~8g / L, the reaction temperature is 45~55℃, and the reaction time is 1~6h.

4. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: In step S2, the conditions of the second coprecipitation reaction are: the pH of the reaction system is 11-12.5, the NH4 + The concentration is 5~10g / L, the reaction temperature is 50~60℃, and the reaction time is 12~76h.

5. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: In step S3, the conditions of the third coprecipitation reaction are: the pH of the reaction system is 10.8-12, and the NH4 + The concentration is 4~7g / L, the reaction temperature is 48~58℃, and the reaction time is 8~24h.

6. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: The concentration of the sodium hydroxide solution is 6-12 mol / L.

7. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: The concentration of the ammonia water is 5-10 mol / L.

8. The method for preparing the nickel-cobalt-manganese-aluminum quaternary precursor material according to claim 2, characterized in that: In step S3, the Nb source includes at least one of Nb2O5, NbO2, Nb2O3 and NbO.

9. A positive electrode material, characterized in that: It is prepared from the nickel-cobalt-manganese-aluminum quaternary precursor material described in claim 1.

Citation Information

Cited By

  • Preparation method of cerium-tungsten composite modified core-shell lithium-rich manganese-based positive electrode material