Method for preparing laminated solar cell and laminated solar cell

By using transparent conductive thin film precursor solution/slurry with adjustable work function in laminated solar cells, a multi-layer structure with high conductivity and high light transmission is prepared, which solves the problem of work function fixation of the intermediate transparent conductive layer and improves the battery Efficiency and carrier transmission improve the performance of stacked batteries.

CN116364332BActive Publication Date: 2024-11-29嘉兴阿特斯阳光能源科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111579237.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-11-29
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

In stacked solar cells, the work function of the transparent conductive layer in the middle in the prior art is fixed, resulting in low battery efficiency and inability to effectively match the energy levels of the batteries on both sides, increasing contact resistance and reducing conversion efficiency.

Method used

Using a transparent conductive thin film precursor solution/slurry, an interjunction conductive layer with adjustable work function is prepared by changing the components and order of conductive substances, using conductive polymers, micro-nano conductive particles and metal nanoconductive materials, combined with pairs Coupling agent and thickening agent are prepared by solution method with a highly conductive and highly transmissive multi-layer structure, matching the energy levels of the batteries on both sides and reducing contact resistance.

Benefits of technology

The work function of the conductive layer between the junctions is adjusted, matching the battery energy levels on both sides, reducing contact resistance, improving carrier transmission, improving battery filling factor (FF) and conversion efficiency, and improving the overall performance of the stacked battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116364332B_ABST
    Figure CN116364332B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a laminated solar cell and a laminated solar cell. The transparent conductive film precursor solution / slurry in the method for preparing the laminated solar cell comprises 0.1wt% to 30wt% of a first conductive material, 1wt% to 30wt% of a second conductive material, 0 to 3wt% of a coupling agent, 0 to 10wt% of a thickener, and 20wt% to 90wt% of a solvent, and the sum of the weight percentages of the above components is 100%. The present invention can prepare a highly conductive, highly transparent, multi-layer structured interjunction conductive layer by a solution method, realize an adjustable work function of the interjunction conductive layer, can well match the battery energy levels on both sides, and make the transition of the energy band from the bottom battery to the top battery more continuous, thereby reducing the contact resistance with the batteries on both sides, helping to improve carrier transmission, increase battery FF, and effectively improve battery conversion efficiency, which is of great significance to the development of laminated batteries and the photovoltaic industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the photovoltaic field, and in particular to a method for preparing a laminated solar cell and a laminated solar cell. Background Art

[0002] With the continuous progress of silicon-based tandem solar cell technology, especially the continuous development of heterojunction cell (HJT) technology, single-junction silicon-based cells have approached their theoretical limit (~29%). In order to further improve the efficiency of cells, tandem cell technology has gradually been favored by developers. In the selection of top cells for silicon-based heterojunction tandem cells, perovskite cells can be called the preferred material for silicon-based tandem cells due to their high conversion efficiency, wide band gap of light-absorbing materials, and battery current density and voltage that are more compatible with silicon-based cells. They have been widely studied in recent years.

[0003] In general stacked cell design, two-junction cells usually use physical or chemical vapor deposition methods to prepare thin films made of ITO, ZnO and other materials as the middle transparent conductive layer. The work function of these films is generally 4.0eV to 4.8eV, which is not adjustable and forms a large potential barrier with the cells on both sides, thereby increasing the series resistance of the battery and reducing the conversion efficiency.

[0004] In view of this, it is necessary to provide a method for preparing a stacked solar cell and a stacked solar cell to solve the above technical problems. Summary of the invention

[0005] An object of the present invention is to provide a stacked solar cell with low inter-contact resistance.

[0006] A transparent conductive film precursor solution / slurry comprises 1wt% to 30wt% of a first conductive material, 0.1wt% to 30wt% of a second conductive material, 0 to 3wt% of a coupling agent, 0 to 10wt% of a thickener, and 20wt% to 90wt% of a solvent, wherein the total weight percentage of the above components is 100%, and the work functions of the first conductive material and the second conductive material are different.

[0007] Furthermore, the first conductive material includes one or more combinations of conductive polymers, micro-nano conductive particles, graphene, graphene oxide, carbon nanotubes, C60 and its derivatives, C70 and its derivatives.

[0008] Further, the conductive polymer includes one or more combinations of polyacetylene, poly(p-phenylene sulfide), poly(p-phenylene), polypyrrole, polythiophene, polyaniline, poly-3,4-ethylenedioxythiophene:polystyrene sulfonate (PEDOT:PSS);

[0009] And / or, the micro-nano conductive particles include one or more combinations of metal oxides such as zinc oxide, molybdenum oxide, tungsten oxide, and titanium oxide.

[0010] Furthermore, the second conductive material is a metal nano-conductive material, such as one or more of silver nanowires, silver nanoparticles, silver nanosheets, copper nanowires, gold nanoparticles, and the like.

[0011] Furthermore, the coupling agent is one or more of a silane coupling agent, an epoxy resin coupling agent, a titanate coupling agent, etc.;

[0012] And / or, the thickener is one or more of xanthan gum, guar gum, cationic guar gum, hydroxypropyl guar gum, magnesium aluminum silicate, silicon dioxide, sodium magnesium silicate, hydrated silicon dioxide, montmorillonite, sodium lithium magnesium silicate, and hectorite;

[0013] And / or, the solvent is one or more of water, methanol, ethanol, isopropanol, formic acid, acetic acid, ether, etc.

[0014] A method for preparing a transparent conductive film precursor solution / slurry comprises the following steps:

[0015] S1. According to the components and contents of the transparent conductive film precursor solution / slurry according to any one of claims 1 to 5, other components are sequentially and intermittently added to the solvent during heating and stirring, and the order of adding the other components is the first conductive substance, the second conductive substance, the coupling agent, and the thickener, or the order of adding the other components is the second conductive substance, the first conductive substance, the coupling agent, and the thickener;

[0016] S2 sieves the solution, and the sieve aperture size is 1 μm to 150 μm.

[0017] Furthermore, in step S1, the heating temperature is 30-80°C, the stirring speed is 10 rpm to 1000 rpm, and the stirring time is 1 min to 360 min.

[0018] A method for preparing a stacked solar cell comprises the following steps:

[0019] preparing a bottom battery;

[0020] Using the transparent conductive film precursor solution / paste according to any one of claims 1 to 5, the interjunction conductive layer is prepared by spin coating, spraying, coating, roll-to-roll printing or screen printing;

[0021] preparing a top cell;

[0022] Preparation of metal electrodes.

[0023] Further preparing the interjunction conductive layer comprises:

[0024] A lower transparent conductive film is prepared by using a first precursor solution;

[0025] preparing an upper transparent conductive film by using a second precursor solution;

[0026] The work functions of the first conductive material in the first precursor solution and the first conductive material in the second precursor solution are different.

[0027] Furthermore, the first conductive substance in the first precursor solution has a lower work function than the first conductive substance in the second precursor solution.

[0028] Further, in the first precursor solution, the first conductive material is magnesium-doped zinc oxide (ZnO:Mg), and its proportion is 5wt%; the second conductive material is silver nanowires, and its proportion is 0.5wt%; the coupling agent is a silane coupling agent, and its proportion is 0.1%; the proportion of the thickener is 0; and the remainder is the solvent;

[0029] In the second precursor solution, the first conductive material is PEDOT:PSS, and its proportion is 8wt%; the second conductive material is silver nanowire, and its proportion is 0.3wt%; the coupling agent is silane coupling agent, and its proportion is 0.1%; the thickener proportion is 0; and the remainder is solvent.

[0030] Furthermore, the solvent of the first precursor solution is a mixture of deionized water and isopropanol, deionized water accounts for 95wt% of the solvent, and isopropanol accounts for 5wt% of the solvent; the solvent of the second precursor solution is a mixture of deionized water and isopropanol, deionized water accounts for 97wt% of the solvent, and isopropanol accounts for 3wt% of the solvent.

[0031] A laminated solar cell is prepared by the laminated solar cell preparation method.

[0032] In order to solve one of the above technical problems, the present invention adopts the following technical solution:

[0033] The beneficial effects of the present invention are as follows: compared with the prior art, the present invention provides a transparent conductive film precursor solution / slurry, which can be used to prepare a highly conductive, highly transmittance, multi-layer interjunction conductive layer by a solution method, so as to achieve adjustable work function of the interjunction conductive layer, which can well match the battery energy levels on both sides, and make the transition of the energy band from the bottom battery to the top battery more continuous, thereby reducing the contact resistance with the batteries on both sides, helping to improve carrier transport, enhance battery FF, and effectively improve battery conversion efficiency, which is of great significance to the development of stacked batteries and the photovoltaic industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a schematic structural diagram of a stacked solar cell of the present invention;

[0035] Figure 2 It is a preparation flow chart of the stacked solar cell of the present invention.

[0036] Among them, 100-stacked solar cell, 1-back metal electrode, 2-bottom cell, 21-crystalline silicon layer, 22-first intrinsic amorphous silicon layer, 23-first doped amorphous silicon layer, 24-back transparent conductive layer, 25-second intrinsic crystalline silicon layer, 26-second doped amorphous silicon layer, 3-interjunction conductive layer, 31-lower transparent conductive film, 32-upper transparent conductive film, 4-top cell, 41-perovskite light absorption layer, 42-hole transport layer, 43-electron transport layer, 44-top transparent conductive layer, 5-front metal electrode. DETAILED DESCRIPTION

[0037] The present invention will be described in detail below in conjunction with the specific embodiments shown in the accompanying drawings. However, these embodiments do not limit the present invention, and any structural, methodological, or functional changes made by a person skilled in the art based on these embodiments are all within the scope of protection of the present invention.

[0038] In various drawings of the present invention, for the convenience of illustration, some sizes of structures or parts are exaggerated relative to other structures or parts, and thus, only the basic structure of the subject matter of the present invention is illustrated.

[0039] Please refer to Figure 1 As shown, the stacked solar cell 100 optimally designed for the present invention includes a back metal electrode 1, a bottom battery 2, an interjunction conductive layer 3, a top battery 4, and a front metal electrode 5 arranged from bottom to top.

[0040] The bottom cell 2 is a silicon-based cell, which includes but is not limited to an emitter cell, a PERC back passivation cell, a silicon heterojunction cell, a PERT cell, an IBC cell, a MWT cell or a Top-con cell.

[0041] Preferably, the silicon-based battery is a silicon heterojunction battery, which includes a crystalline silicon layer 21, a first intrinsic amorphous silicon layer 22, a first doped amorphous silicon layer 23, and a back transparent conductive layer 24 arranged in sequence on the back side of the crystalline silicon layer 21; and a second intrinsic crystalline silicon layer 25 and a second doped amorphous silicon layer 26 arranged in sequence on the front side of the crystalline silicon layer 21.

[0042] The crystalline silicon layer 21 may be an N-type or P-type crystalline silicon wafer with a thickness of 80 μm to 300 μm.

[0043] The thickness of the first intrinsic amorphous silicon layer 22 and the second intrinsic amorphous silicon layer 21 is 2 nm-60 nm, which has a good passivation effect on the crystalline silicon layer 21 .

[0044] The first doped amorphous silicon layer 23 and the second doped amorphous silicon layer 26 have different doping types, and the two can be interchangeable, which can be determined according to the battery design. For example, the crystalline silicon layer 21 can be an N-type crystalline silicon wafer, the first doped amorphous silicon layer 23 is a P-type doped crystalline silicon layer, and the second doped amorphous silicon layer 26 is an N-type doped crystalline silicon layer; or, the crystalline silicon layer 21 is a P-type crystalline silicon wafer, the first doped amorphous silicon layer 23 is an N-type doped crystalline silicon layer, and the second doped amorphous silicon layer 26 is a P-type doped crystalline silicon layer.

[0045] In the present invention, the thickness of the first doped amorphous silicon layer 23 and the second doped amorphous silicon layer 26 are 3nm to 30nm, and the doping concentration is 1e 18 ~1e 23 .

[0046] The thickness of the back transparent conductive layer 24 is 10nm to 500nm, and the material is transparent conductive oxide or conductive polymer. The transparent conductive oxide includes but is not limited to one or more of indium tin oxide, indium tungsten oxide, tungsten oxide, titanium oxide, zinc oxide and zirconium oxide; the conductive polymer includes but is not limited to one or more of PEDOT:PSS, P3HT, etc.

[0047] The back transparent conductive layer 24 can be prepared by any method commonly used to prepare transparent conductive films, including but not limited to one or more deposition methods such as chemical vapor deposition, magnetron sputtering deposition, reactive plasma deposition, spin coating, spray coating or roll-to-roll printing.

[0048] The top cell 4 is a perovskite cell, which can be an upright structure or an inverted structure.

[0049] Taking the inverted structure as an example, the perovskite cell includes a perovskite light absorption layer 41, a hole transport layer 42 disposed on the back of the perovskite light absorption layer 41, an electron transport layer 43 disposed on the front of the perovskite light absorption layer 41, and a top transparent conductive layer 44. In certain specific cases, the electron transport layer 43 can also be combined with the top transparent conductive layer 44 into one layer.

[0050] The perovskite light absorption layer 41 has a thickness of 80 nm to 500 nm, and the material has an ABX3 structure, wherein: A is a monovalent cation, including but not limited to K + 、Na + , Cs + , Rb + 、HN=CHNH3 + (expressed as FA), CH3NH2 + (expressed as MA) or more; B is a divalent cation, including but not limited to Sn 2+ , Pb2+ One or more of; X includes a halogen anion, and the halogen ion includes F - , Cl - Br - and I - etc.; or other ions, such as O2 - 、O2 - One or more of the .

[0051] The material band gap of the perovskite light absorbing layer 41 is 1.2 eV to 2.2 eV, and can be prepared by one or more methods such as thermal evaporation, spin coating, spray coating or roll-to-roll printing.

[0052] The hole transport layer 42 refers to a film layer that collects and transports the photogenerated holes in the perovskite light absorption layer 41. The material may be one or more of PEDOT:PSS, nickel oxide, molybdenum oxide, tungsten oxide, graphite, etc., with a thickness of 5nm to 100nm. The preparation method adopts one or more of chemical vapor deposition, magnetron sputtering deposition, reactive plasma deposition, spin coating, spray coating or roll-to-roll printing.

[0053] The electron transport layer 43 refers to a film layer that collects and transports photogenerated electrons in the perovskite light absorption layer 41. Its material can be one or more of lithium fluoride, titanium dioxide, zinc oxide, tin oxide, polyethyleneimine (PEI), fullerene and its derivatives (PCBM), etc., with a thickness of 5nm to 100nm. The preparation method adopts one or more of chemical vapor deposition, magnetron sputtering deposition, reactive plasma deposition, spin coating, spray coating or roll-to-roll printing.

[0054] The preparation method and materials of the top transparent conductive layer 44 are consistent with those of the back transparent conductive layer 24 in the silicon-based battery, and are not described in detail here.

[0055] It should be noted that the film layers in the upright structure and the inverted structure are the same, and the only difference is the upper and lower position relationship, which will not be elaborated here.

[0056] The bottom battery 2 and the top battery 4 are stacked in series, and the interjunction conductive layer 3 is located between the bottom battery 2 and the top battery 4, and mainly serves to collect currents of the batteries on both sides and improve interface contact.

[0057] In the present invention, the interjunction conductive layer 3 can be a single-layer structure, preferably including at least two layers of transparent conductive films. Different transparent conductive films have different work functions, which can well match the battery energy levels on both sides and make the energy band transition from the bottom battery 2 to the top battery 4 more continuous, which helps to improve carrier transport and enhance battery FF.

[0058] Furthermore, the work functions of at least two layers of the transparent conductive film gradually increase or decrease from bottom to top, and the energy levels are stepped, which has a high degree of matching with the energy levels of the batteries on both sides, and can reduce the contact resistance between the bottom battery 2 and the top battery 4, which can effectively improve the battery conversion efficiency, and is of great significance to the development of stacked batteries and the photovoltaic industry.

[0059] The work function of the interjunction conductive layer 3 is in the range of 3.0 eV to 9.0 eV, and the work functions of the multi-layer transparent conductive film are located in different intervals within this range.

[0060] Preferably, the thickness of the transparent conductive film is between 5 nm and 200 nm; on the one hand, it protects the conductive properties of the inherent film layer, and on the other hand, it can protect itself from being damaged when preparing other film layers.

[0061] The present invention also provides a method for preparing a thin film of the interjunction conductive layer with high conductivity, high light transmittance and multi-layer structure by a solution method. Specifically, the transparent conductive film is prepared by a transparent conductive film precursor solution / slurry by spin coating, spraying, coating, roll-to-roll printing or screen printing.

[0062] The transparent conductive film precursor solution / slurry includes the following raw material components and their weight percentages: 1wt% to 30wt% of a first conductive material; 0.1wt% to 30wt% of a second conductive material; 0 to 3wt% of a coupling agent; 0 to 10wt% of a thickener; and 20wt% to 90wt% of a solvent; the total weight percentage of the above components is 100%.

[0063] The first conductive material has the function of adjusting the work function of the transparent conductive film in addition to the conductive function. The first conductive material is a combination of one or more of conductive polymers, micro-nano conductive particles, graphene, graphene oxide, carbon nanotubes, C60 and its derivatives, C70 and its derivatives.

[0064] The conductive polymer includes one or more combinations of polyacetylene, poly(p-phenylene sulfide), poly(p-phenylene), polypyrrole, polythiophene, polyaniline, poly-3,4-ethylenedioxythiophene:polystyrene sulfonate (PEDOT:PSS).

[0065] The micro-nano conductive particles include one or more combinations of metal oxides such as zinc oxide, molybdenum oxide, tungsten oxide, and titanium oxide.

[0066] The second conductive material is mainly used to increase the conductivity of the transparent conductive film layer, and is preferably a metal nano-conductive material, such as one or more of silver nanowires, silver nanoparticles, silver nanosheets, copper nanowires, gold nanoparticles, etc.

[0067] The present invention can change the work function and conductivity of the formed transparent conductive film layer by changing various conductive components of the solution, and can prepare an interjunction conductive layer with a continuously adjustable work function. In other words, the present invention can select the first conductive material and the second conductive material according to the work function and conductivity requirements of the transparent conductive film layer.

[0068] The coupling agent is used to increase the bonding force between the transparent conductive film layer being prepared and the underlying material, and prevent the underlying transparent conductive film layer from being dissolved or destroyed by the upper transparent conductive film layer during the preparation of the multilayer film. Preferably, the coupling agent is one or more of a silane coupling agent, an epoxy resin coupling agent, a titanate coupling agent, etc., and has no effect on the conductivity of the transparent conductive film layer.

[0069] The thickener is used to improve the viscosity of the transparent conductive film precursor solution / paste so that it can be used in methods such as screen printing. The thickener is one or more of xanthan gum, guar gum, cationic guar gum, hydroxypropyl guar gum, magnesium aluminum silicate, silicon dioxide, sodium magnesium silicate, hydrated silicon dioxide, montmorillonite, sodium lithium magnesium silicate, and hectorite.

[0070] The solvent is mainly one or more of water, methanol, ethanol, isopropanol, formic acid, acetic acid, ether and the like.

[0071] The present invention provides a method for preparing a transparent conductive film precursor solution / slurry, comprising the following steps: S1, according to the components and contents of the transparent conductive film precursor solution / slurry, other components are sequentially and intermittently added into a solvent during heating and stirring, wherein the order of adding the other components is a first conductive substance, a second conductive substance, a coupling agent, and a thickener, or the order of adding the other components is a second conductive substance, a first conductive substance, a coupling agent, and a thickener; S2, sieving the solution, wherein the sieve aperture is 1 μm to 150 μm.

[0072] In step S1, the heating temperature is 30-80°C, the stirring speed is 10rpm-1000rpm, and the stirring time is 1min-360min. The purpose of adding the components in sequence is to prevent the components from agglomerating. Adding at intervals means that each component is added and stirred evenly before adding the next component, with an interval time of about 10s-20s to avoid uneven mixing of the solution.

[0073] The present invention also provides a method for preparing a stacked battery, comprising the following steps: preparing a bottom battery; using the above-mentioned transparent conductive film precursor solution / slurry to prepare an interjunction conductive layer by spin coating, spraying, coating, roll-to-roll printing or screen printing; preparing a top battery; and preparing a metal electrode.

[0074] The present invention is described in detail below with reference to specific embodiments.

[0075] Embodiment 1:

[0076] The bottom battery 2 is a silicon-based battery, and the second doped amorphous silicon layer 26 is an N-type doped crystalline silicon layer; the top battery 4 is a perovskite battery, and the hole transport layer 42 is located on the back of the perovskite light absorption layer 41; the interjunction conductive layer 3 includes at least two layers of the transparent conductive film, and the work function of at least two layers of the transparent conductive film gradually increases from bottom to top.

[0077] Taking the interjunction conductive layer 3 as a two-layer structure as an example, the work function of the lower transparent conductive film 31 is smaller than the work function of the upper transparent conductive film 32. For example, the work function of the lower transparent conductive film 31 is 3.5eV to 4.3eV, and the work function of the upper transparent conductive film 32 is 4.9eV to 8.6eV.

[0078] The precursor solution used to prepare the lower transparent conductive film 31 is recorded as the first precursor solution, and its raw material components and weight percentages are as follows: the first conductive material is magnesium-doped zinc oxide (ZnO:Mg), and its proportion is 5wt%; the second conductive material is silver nanowires, and its proportion is 0.5wt%; the coupling agent is a silane coupling agent (COATOSIL*2287), and its proportion is 0.1%; no thickener is added; the remainder is solvent. The solvent is a mixture of deionized water and isopropyl alcohol, specifically, deionized water accounts for 95wt% of the solvent, and isopropyl alcohol accounts for 5wt% of the solvent.

[0079] The above raw material components were added to the solvent in sequence, and the formed solution was stirred at 50° C. and 300 rpm for 10 min, after which the solution was filtered using a 5 μm polyester mesh.

[0080] The precursor solution used to prepare the upper transparent conductive film 32 is recorded as the second precursor solution, and its raw material components and weight percentages are as follows: the first conductive material is PEDOT:PSS, and its proportion is 8wt%; the second conductive material is silver nanowires, and its proportion is 0.3wt%; the coupling agent is a silane coupling agent (COATOSIL*2287), and its proportion is 0.1%; no thickener is added; the remainder is solvent. The solvent is a mixture of deionized water and isopropyl alcohol, specifically, deionized water accounts for 97wt% of the solvent, and isopropyl alcohol accounts for 3wt% of the solvent.

[0081] The lower transparent conductive film 31 is located on the second doped amorphous silicon layer 26, and the hydrophilicity of the second doped amorphous silicon layer 26 is slightly poor, so the concentration of isopropyl alcohol in the first precursor solution is large. The upper transparent conductive film 32 is located on the lower transparent conductive film 31, and the hydrophilicity of the lower transparent conductive film 31 is stronger than that of the second doped amorphous silicon layer 26, so the concentration of isopropyl alcohol in the second precursor solution is lower than that of the first precursor solution.

[0082] The above raw material components were added to the solvent in sequence, and the formed solution was stirred at 50° C. and 300 rpm for 10 min, after which the solution was filtered using a 10 μm polyester mesh.

[0083] Please refer to Figure 2 As shown, the preparation method of the stacked battery is:

[0084] Preparation of the bottom battery 1: an N-type single crystal silicon wafer with a thickness of about 130nm and a resistivity of 0.5Ω·cm to 5Ω·cm is textured to form a pyramid texture surface on the surface; a 2nm to 10nm intrinsic amorphous silicon layer is deposited on the front and back sides of the silicon wafer using PECVD; a p-type doped amorphous silicon layer with a thickness of 5nm to 20nm is deposited on the back side; an n-type doped amorphous silicon layer 21 with a thickness of 5nm to 20nm is deposited on the front side; and ITO is deposited on the back side as the back transparent conductive layer 24 with a thickness of 50nm to 100nm and a square resistance of 30Ω / □ to 100Ω / □.

[0085] Preparation of the interjunction conductive layer 3: Take 100 ml of the first precursor solution, spread it evenly on the surface of the silicon wafer, spin-coat it at a speed of 2000 rpm to form a film, and then anneal it at 80° C. to 200° C. for 5 min to 20 min.

[0086] The second precursor solution is taken and evenly spread on the lower transparent conductive film 31, and is spin-coated at a speed of 2500 rpm to form a film, and then annealed at 80° C. to 200° C. for 5 min to 20 min.

[0087] Preparation of the top battery 4: MoO3 is vacuum-deposited as a hole transport layer 42 on the interjunction conductive layer 3, with a film thickness of 50nm~100nm and a square resistance of 30Ω / □~100Ω / □; the perovskite light absorption layer 41 is prepared on it by spin coating, and its material is CH3NH2PbCl3; an electron transport layer 43 is prepared on it, and a PCBM film is prepared by spin coating, with a film thickness of 5nm~20nm; and ITO is deposited on it by PVD as a top transparent conductive layer 44, with a thickness of 50nm~100nm and a square resistance of 30Ω / □~100Ω / □.

[0088] Preparation of metal electrodes: The front metal electrode 5 and the back metal electrode 1 are prepared by screen printing silver grid lines.

[0089] Example 2: The interjunction conductive layer in Example 2 adopts a single-layer film structure, and its preparation method refers to the lower transparent conductive film 32 in Example 1, with a film thickness of 50 to 100 nm and a square resistance of 50Ω / □ to 200Ω / □; the remaining steps are the same as in Example 1.

[0090] Comparative Example 1: The only difference from Example 1 is that the interjunction conductive layer 3 is prepared using a single layer of ITO with a work function of 4.2eV to 4.7eV, prepared by magnetron sputtering, with a film thickness of 60nm to 140nm and a square resistance of 50Ω / □ to 200Ω / □.

[0091] The battery performance data of Example 1, Example 2 and Comparative Example 1 are shown in Table 1. As can be seen from Table 1, the use of a multi-layer film structure in the interjunction transparent conductive layer has a slight effect on light transmission, resulting in a slightly smaller current, but the FF of the battery is greatly improved, so the battery efficiency is improved. This shows that the intermediate transparent conductive layer plays a role in regulating the contact between the two batteries.

[0092] Table 1

[0093] Voc(mV) <![CDATA[Jsc(mA / cm 2 )]]> FF(%) Eff(%) Comparative Example 1 1760.2 21.23 81.20 30.34 Example 1 1760.9 21.26 83.00 31.07 Example 2 1759.6 21.35 81.28 30.53

[0094] In summary, compared with the prior art, the present invention provides a transparent conductive film precursor solution / slurry, which can be used to prepare a highly conductive, highly transmittance, multi-layer interjunction conductive layer 3 by a solution method, so that the work function of the interjunction conductive layer 3 can be adjusted, which can well match the battery energy levels on both sides, and make the transition of the energy band from the bottom battery 2 to the top battery 4 more continuous, thereby reducing the contact resistance with the batteries on both sides, helping to improve carrier transport, enhance battery FF, and effectively improve battery conversion efficiency, which is of great significance to the development of stacked batteries and the photovoltaic industry.

[0095] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0096] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a stacked solar cell, characterized in that: The steps include: preparing a bottom battery; A transparent conductive film precursor slurry is used to prepare an interjunction conductive layer by spin coating, spraying, coating, roll-to-roll printing or screen printing, wherein the transparent conductive film precursor slurry comprises 1 wt%~30wt% of a first conductive material, 0.1 wt%~30wt% of a second conductive material, 0~3wt% of a coupling agent, 0~10wt% of a thickener, and 20 wt%~90wt% of a solvent, and the total weight percentage of the above components is 100%, the first conductive material comprises a conductive polymer, micro-nano conductive particles, graphene, graphene oxide, carbon nanotubes, C60 and its derivatives, C70 and its derivatives, or a combination of one or more thereof, and the second conductive material is a metal nano conductive material; preparing a top cell; Preparation of metal electrodes; Wherein, preparing the interjunction conductive layer comprises: Using the first precursor slurry to prepare a lower transparent conductive film; Using the second precursor slurry to prepare an upper transparent conductive film; The work functions of the first conductive material in the first precursor slurry and the first conductive material in the second precursor slurry are different, and the work functions of the upper transparent conductive film and the lower transparent conductive film are different, which can well match the battery energy levels on both sides and make the transition of the energy band from the bottom battery to the top battery more continuous.

2. The method for preparing a stacked solar cell according to claim 1, characterized in that: The first conductive material in the first precursor slurry has a lower work function than the first conductive material in the second precursor slurry.

3. The method for preparing a stacked solar cell according to claim 1, characterized in that: In the first precursor slurry, the first conductive material is magnesium-doped zinc oxide ZnO:Mg, and its proportion is 5wt%; the second conductive material is silver nanowires, and its proportion is 0.5wt%; the coupling agent is a silane coupling agent, and its proportion is 0.1%; the proportion of the thickener is 0; and the balance is a solvent; In the second precursor slurry, the first conductive material is PEDOT:PSS, and its ratio is 8wt%; the second conductive material is silver nanowire, and its ratio is 0.3wt%; the coupling agent is silane coupling agent, and its ratio is 0.1%; the thickener ratio is 0; and the remainder is solvent.

4. The method for preparing a stacked solar cell according to claim 3, characterized in that: The solvent of the first precursor slurry is a mixture of deionized water and isopropanol, with deionized water accounting for 95wt% of the solvent and isopropanol accounting for 5wt% of the solvent; the solvent of the second precursor slurry is a mixture of deionized water and isopropanol, with deionized water accounting for 97wt% of the solvent and isopropanol accounting for 3wt% of the solvent.

5. The method for preparing a stacked solar cell according to claim 1, characterized in that: The conductive polymer includes one or more combinations of polyacetylene, poly(p-phenylene sulfide), poly(p-phenylene), polypyrrole, polythiophene, and PEDOT:PSS; And / or, the micro-nano conductive particles include one or more combinations of zinc oxide, molybdenum oxide, tungsten oxide, and titanium oxide.

6. The method for preparing a stacked solar cell according to claim 1, characterized in that: The second conductive material is one or more of silver nanowires, silver nanoparticles, silver nanosheets, copper nanowires, and gold nanoparticles.

7. The method for preparing a stacked solar cell according to claim 1, characterized in that: The coupling agent is one or more of a silane coupling agent, an epoxy resin coupling agent, and a titanate coupling agent; And / or, the thickener is one or more of xanthan gum, guar gum, cationic guar gum, hydroxypropyl guar gum, magnesium aluminum silicate, silicon dioxide, sodium magnesium silicate, hydrated silicon dioxide, montmorillonite, sodium lithium magnesium silicate, and hectorite; And / or, the solvent is one or more of water, methanol, ethanol, isopropanol, formic acid, acetic acid, and ether.

8. The method for preparing a stacked solar cell according to claim 1, characterized in that: The method for preparing the transparent conductive film precursor slurry comprises the following steps: S1: According to the components and contents of the transparent conductive film precursor slurry as claimed in claim 1, other components are added to the solvent in sequence and at intervals during heating and stirring, and the order of adding the other components is the first conductive substance, the second conductive substance, the coupling agent, and the thickener, or the order of adding the other components is the second conductive substance, the first conductive substance, the coupling agent, and the thickener; S2 sieves the slurry, and the sieve aperture size is 1μm ~150μm.

9. The method for preparing a stacked solar cell according to claim 8, characterized in that: In step S1, the heating temperature is 30-80°C, the stirring speed is 10 rpm ~ 1000 rpm, and the stirring time is 1 min ~ 360 min.

10. A stacked solar cell, characterized in that: The solar cell is prepared by the method for preparing the stacked solar cell according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Transparent conductive film for solar cell, composition for said transparent conductive film, and multi-junction solar cell

    CN102197492A

  • Spray transparent and conductive ink as well as preparation method and application thereof

    CN107384025A

  • Efficient and stable perovskite / silicon two-end laminated solar cell

    CN111554764A

  • Intermediate series connection layer, laminated photovoltaic device and production method

    CN113224176A