Lithium supplementation materials and their preparation methods, positive electrode sheets and secondary batteries
By combining lithium-rich materials with carbon nanomaterials, a core-shell structured lithium-replenishing material is formed, which solves the problem of poor conductivity of existing materials and improves the energy density and coulombic efficiency of batteries.
Patent Information
- Application Number
- CN202310413165.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Existing lithium replenishment materials have poor conductivity, which leads to a decrease in the coulombic efficiency of lithium-ion secondary batteries, affecting cycle life and energy density.
By combining lithium-rich materials with carbon nanomaterials, the carbon nanomaterials are embedded in the inner or outer surface of the lithium-rich materials to form a core-shell structure, thereby improving conductivity and lithium-ion utilization.
The conductivity and stability of the lithium replenishment material are enhanced, effectively improving the energy density and coulombic efficiency of the battery.
Smart Images

Figure CN116454423B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a lithium replenishment material and its preparation method, a positive electrode sheet, and a secondary battery. Background Technology
[0002] During the initial charge and discharge cycle of batteries such as lithium-ion rechargeable batteries, a large amount of solid electrolyte interphase (SEI) film forms on the surface of the negative electrode. This film consumes the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss and reducing the coulombic efficiency of the lithium-ion rechargeable battery. This directly affects the cycle life and energy density of the battery. Currently, this irreversible capacity loss can be eliminated by lithium replenishment at the positive electrode, thereby improving the battery's energy density and other electrical properties. However, existing lithium replenishment materials suffer from poor conductivity, which hinders their industrial production. Summary of the Invention
[0003] This application provides a lithium supplement material and its preparation method, a positive electrode sheet, and a secondary battery.
[0004] In a first aspect, this application provides a lithium replenishment material, which includes a lithium-rich material and a carbon nanomaterial, wherein the lithium-rich material is embedded with the carbon nanomaterial.
[0005] In this application, carbon nanomaterials exhibit excellent electrical conductivity, thereby enhancing the conductivity of the lithium-rich material. Furthermore, the carbon nanomaterials are embedded in the lithium-rich material, exhibiting strong bonding between the carbon nanomaterials and the lithium-rich material. The carbon nanomaterials can be stably fixed within the lithium-rich material, and during use, they are less prone to being stripped away, thus better enhancing the conductivity of the lithium-rich material and effectively increasing the battery's energy density.
[0006] In one embodiment, the lithium-rich material is deposited on the outer surface of the carbon nanomaterial.
[0007] In one embodiment, the carbon nanomaterial surrounds an accommodating space, with a portion of the lithium-rich material deposited on the outer surface of the carbon nanomaterial and a portion of the lithium-rich material embedded within the accommodating space.
[0008] In one embodiment, the lithium-rich material forms a coating layer that covers at least a portion of the outer surface of the carbon nanomaterial.
[0009] In one embodiment, the thickness of the coating layer ranges from 4 μm to 20 μm; and / or, the thickness of the coating layer is greater than the diameter or length of the carbon nanomaterial.
[0010] In one embodiment, each particle of the lithium-rich material includes a plurality of the carbon nanomaterials, which are dispersed within the lithium-rich material.
[0011] In one embodiment, a portion of the carbon nanomaterial is located on the outer surface of the lithium replenishing material particles; and / or, at least a portion of the carbon nanomaterial extends from within the lithium replenishing material to the outside of the lithium replenishing material.
[0012] In one embodiment, the mass ratio of the lithium-rich material to the lithium-replenishing material is 80%-99%.
[0013] In one embodiment, the mass ratio of the carbon nanomaterial to the lithium-rich material is 1% to 25%.
[0014] In one embodiment, the carbon nanomaterial is a carbon nanotube, and the aspect ratio of the carbon nanotube is 10-100.
[0015] In one embodiment, the carbon nanotubes have a diameter of 20 nm to 80 nm.
[0016] In one embodiment, the length of the carbon nanotube is 0.2 μm-2 μm.
[0017] In one embodiment, the lithium-rich material is obtained by lithiation of an intermediate, which is formed by depositing a lithium-rich material precursor on the framework of the carbon nanomaterial, and the lithium-rich material is obtained by lithiation of the lithium-rich material precursor.
[0018] In one embodiment, the lithium-rich material has the general structural formula Li. 1+x A y O z Where 0 < x < 10, 0 < y < 6, 0 < z < 13, and A is one or more of Ni, Co, Fe, Cu, Mg, Mn, Cr, Zn, Ti, Zr, Nb, and Mo.
[0019] In one embodiment, the carbon nanomaterial includes at least one of carbon nanotubes, carbon nanofibers, carbon nanospheres, and graphene.
[0020] In one embodiment, the particle size of the lithium replenishment material satisfies: 4μm≤D50≤20μm.
[0021] In one embodiment, the specific surface area of the lithium replenishing material is 0.5 m². 2 / g-30m 2 / g.
[0022] Secondly, this application provides a method for preparing a lithium-supplementing material, the method comprising:
[0023] A carbon nanomaterial solution and a metal solution are added to a reactor, and the pH of the solution in the reactor is adjusted to be alkaline to obtain an intermediate.
[0024] The intermediate is mixed with a lithium source and sintered under an inert atmosphere to obtain a lithium-replenishing material.
[0025] Thirdly, this application provides a positive electrode sheet, which includes the lithium replenishing material as described above, or the lithium replenishing material prepared by the method described above.
[0026] Fourthly, this application provides a secondary battery, which includes a negative electrode, a separator, and a positive electrode as described above. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the embodiments of this application will be described below.
[0028] Figure 1 A schematic diagram of a lithium replenishment material provided in one embodiment of this application;
[0029] Figure 2 A schematic diagram of a lithium replenishment material provided in one embodiment of this application;
[0030] Figure 3 This is a schematic diagram of a lithium replenishment material provided in one embodiment of this application. Detailed Implementation
[0031] The technical solutions of the embodiments of this application will be described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments.
[0032] In this document, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, unless otherwise stated, "multiple" means two or more.
[0033] Furthermore, in this article, directional terms such as "upper" and "lower" are defined relative to the orientation of the structure as shown in the attached drawings. It should be understood that these directional terms are relative concepts, used for relative description and clarification, and can change accordingly depending on the orientation of the structure.
[0034] For ease of understanding, the English abbreviations and related technical terms used in the embodiments of this application will be explained and described below.
[0035] SEI membrane: refers to Solid Electrolyte Interphase, i.e., solid electrolyte interface membrane.
[0036] During the first charge and discharge cycle of batteries such as lithium-ion rechargeable batteries, a large amount of solid electrolyte interphase (SEI) film forms on the surface of the negative electrode. This film consumes the limited lithium ions and electrolyte in the battery, resulting in a significant reduction in lithium-ion capacity and causing irreversible capacity loss. During the first discharge, the number of lithium ions extracted from the negative electrode is much smaller than the number extracted from the positive electrode during charging, leading to a decrease in the coulombic efficiency of the lithium-ion rechargeable battery and directly affecting its cycle life and energy density. This problem can usually be addressed by replenishing lithium at the positive electrode to eliminate this irreversible capacity loss and improve the battery's energy density and other electrical properties. However, existing lithium replenishment materials suffer from poor conductivity, hindering their widespread application and limiting the improvement of lithium-ion rechargeable battery performance.
[0037] This application provides a lithium replenishing material 1, which is applied to the positive electrode of a battery to pre-lithiate the positive electrode, adding lithium to the battery interior to replenish lithium ions before the battery operates. In one embodiment, the lithium replenishing material 1 can be coated onto the outer surface of the battery positive electrode sheet, or it can be embedded into the outer surface of the battery positive electrode sheet. In other embodiments, the lithium replenishing material 1 can be added during the preparation of the battery positive electrode sheet, dispersing it to both the outer surface and interior of the positive electrode sheet.
[0038] Please see Figure 1 , Figure 1 This is a schematic diagram of a lithium replenishment material 1 provided in one embodiment of this application. This application provides a lithium replenishment material 1, which includes a lithium-rich material 10 and a carbon nanomaterial 11, wherein the lithium-rich material 10 is embedded with the carbon nanomaterial 11.
[0039] Lithium supplement material 1 includes multiple particles. Figure 1 The diagram shows one of the particles in the lithium replenishment material 1. In one embodiment, the particles of the lithium replenishment material 1 are spherical or nearly spherical. The lithium-rich material 10 is also granular. In one embodiment, a particle of the lithium replenishment material 1 includes a lithium-rich material 10 particle and one or more carbon nanomaterials 11.
[0040] The lithium-rich material 10 has a high lithium content. During the first charge, the lithium (Li) in the lithium-rich material 10 can be released and migrate to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby improving the total capacity and energy density of the battery.
[0041] The carbon nanomaterial 11 is conductive, which can improve the conductivity of the lithium replenishment material 1, thereby effectively increasing the energy density of the battery. The lithium-rich material 10 is embedded within the carbon nanomaterial 11, resulting in a strong bond between the lithium-rich material 10 and the carbon nanomaterial 11. In one embodiment, the lithium-rich material 10 is grown on the carbon nanomaterial 11, which can be stably fixed to the lithium-rich material 10. During use, the carbon nanomaterial 11 is not easily peeled off, thus better enhancing the conductivity of the lithium replenishment material 1.
[0042] In one embodiment, the surface of the carbon nanomaterial 11 is uneven, and the surface of the carbon nanomaterial 11 has grooves, in which the lithium-rich material 10 is embedded. In another embodiment, the surface of the carbon nanomaterial 11 has pores, in which the lithium-rich material 10 is embedded.
[0043] The lithium replenishment material 1 provided in this application has good conductivity and a relatively stable overall structure. The lithium replenishment material 1 contains enough lithium to replenish the irreversible lithium loss caused by the formation of the SEI film, thereby effectively improving the energy density of the battery.
[0044] In one embodiment, a lithium-rich material is deposited on the outer surface of a carbon nanomaterial. In another embodiment, the carbon nanomaterial includes solid nanomaterials such as carbon nanofibers and carbon nanospheres. The lithium-rich material is deposited on the outer surface of the carbon nanomaterial, meaning it coats or partially coats the outer surface of the carbon nanomaterial. Simultaneously, the lithium-rich material and the carbon nanomaterial are tightly intercalated, which can better improve the conductivity of the lithium-replenishing material, thereby enhancing its lithium-replenishing effect.
[0045] In one embodiment, the carbon nanomaterial 11 surrounds a accommodating space, with a portion of the lithium-rich material 10 deposited on the outer surface of the carbon nanomaterial 11 and a portion of the lithium-rich material 10 embedded within the accommodating space. In another embodiment, the carbon nanomaterial 11 is a carbon nanotube, and the accommodating space is the internal space of the carbon nanotube. A portion of the lithium-rich material 10 is deposited on the outer surface of the carbon nanotube, and a portion of the lithium-rich material 10 is embedded within the carbon nanotube. The lithium-rich material 10 is located both inside and on the outer surface of the carbon nanomaterial 11, improving the bonding force between the lithium-rich material 10 and the carbon nanomaterial 11. The carbon nanomaterial 11 is less prone to peeling off, allowing it to better enhance the conductivity of the lithium-rich material 1.
[0046] In one embodiment, the lithium-rich material 10 forms a coating layer covering at least a portion of the outer surface of the carbon nanomaterial 11. In one embodiment, the lithium-rich material 10 completely covers the outer surface of the carbon nanomaterial 11. In one embodiment, the lithium-rich material 10 partially covers the outer surface of the carbon nanomaterial 11.
[0047] The lithium replenishment material 1 has a core-shell structure, with carbon nanomaterial 11 as the core and lithium-rich material 10 forming a coating layer as the outer shell. Combining lithium-rich material 10 with carbon nanomaterial 11 improves the conductivity of the composite material, i.e., lithium replenishment material 1, thereby improving the utilization rate of lithium ions in lithium replenishment material 1 and significantly improving the electrochemical performance of the battery.
[0048] In one embodiment, the coating layer formed by the lithium-rich material 10 is a uniform coating layer, meaning the thickness of the coating layer is uniform. The distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10 is equidistant everywhere. In this case, if the carbon nanomaterial 11 is spherical, then the lithium-supplementing material 1 after coating the lithium-rich material 10 is also spherical. If the carbon nanomaterial 11 is elongated, then the lithium-supplementing material 1 after coating the lithium-rich material 10 is also elongated.
[0049] In one embodiment, the coating layer formed by the lithium-rich material 10 is a non-uniform coating layer, that is, the thickness of the coating layer is uneven. For example, if the carbon nanomaterial 11 is elongated and the lithium-supplementing material 1 is spherical, then the thickness of the coating layer formed corresponding to the long side and the short side of the carbon nanomaterial 11 is different.
[0050] In one embodiment, the thickness of the coating layer ranges from 4 μm to 20 μm. The thickness of the coating layer refers to the distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10. In one embodiment, the thickness of the coating layer refers to the minimum or maximum distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10. In another embodiment, the thickness of the coating layer refers to the average distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10. Setting the thickness of the coating layer within the range of 4 μm to 20 μm not only improves the conductivity of the lithium-supplementing material 1 but also enables the lithium-supplementing material 1 to provide sufficient lithium ions.
[0051] In one embodiment, the thickness of the coating layer can be in the range of 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 20μm.
[0052] In one embodiment, a lithium supplement material 1 particle includes a carbon nanomaterial 11 (such as... Figure 2 As shown in the figure, the thickness of the coating layer refers to the maximum distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10. In one embodiment, a lithium-supplementing material 1 particle includes a plurality of carbon nanomaterials 11, and the maximum distance between the outer surface of each carbon nanomaterial 11 and the outer surface of the lithium-rich material 10 satisfies 4μm-20μm.
[0053] In one embodiment, the thickness of the coating layer is greater than the diameter or length of the carbon nanomaterial 11. A larger coating layer results in a larger content of lithium-rich material 10, which can provide more lithium ions to compensate for the lithium loss caused by the formation of the SEI film.
[0054] In one embodiment, when the carbon nanomaterial 11 is spherical, the thickness of the coating layer is greater than the diameter of the spherical carbon nanomaterial 11. For example, the carbon nanomaterial 11 is a carbon nanosphere, and the thickness of the coating layer is greater than the diameter of the carbon nanosphere.
[0055] In one embodiment, when the carbon nanomaterial 11 is elongated, the thickness of the coating layer is greater than the length of the carbon nanomaterial 11. In this case, the thickness of the coating layer refers to the maximum distance between the outer surface of the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10. For example, the carbon nanomaterial 11 is a carbon nanotube, and the thickness of the coating layer is greater than the length of the carbon nanotube.
[0056] In one embodiment, each lithium-rich material 1 particle includes a plurality of carbon nanomaterials 11, and the plurality of carbon nanomaterials 11 are dispersed within the first lithium-rich material 10 (e.g., Figure 1 (As shown).
[0057] Carbon nanomaterial 11 is located within lithium-rich material 10. The bonding force between carbon nanomaterial 11 and lithium-rich material 10 is strong, and carbon nanomaterial 11 can be stably fixed within lithium-rich material 10. During the use of lithium supplement material 1, carbon nanomaterial 11 is not easily peeled off, and can better play the role of improving the conductivity of lithium supplement material 1.
[0058] In this application, the carbon nanomaterial 11 is dispersed, rather than concentrated within the lithium-rich material 10. This dispersed arrangement of the carbon nanomaterial 11 facilitates the construction of a conductive network within the lithium-rich material 1, thereby improving its conductivity.
[0059] In one embodiment, a particle of lithium supplementation material 1 comprises only one carbon nanomaterial 11 (e.g., Figure 2 As shown, a carbon nanomaterial 11 can be located at any position within the lithium-rich material 10. For example, the carbon nanomaterial 11 is a carbon nanotube, and a particle of the lithium-rich material 1 consists of only one carbon nanotube, which is located at the center of the lithium-rich material 1.
[0060] In one embodiment, a lithium replenishment material 1 particle comprises a plurality of carbon nanomaterials 11, which are dispersed at different positions within the lithium-rich material 10. For example, the carbon nanomaterials 11 are carbon nanotubes, and a lithium replenishment material 1 particle comprises three carbon nanotubes spaced apart and located at different positions within the lithium replenishment material 1.
[0061] In one embodiment, a lithium supplement material 1 particle includes a plurality of carbon nanomaterials 11, some of which are dispersed within the lithium-rich material 10, and some of which extend from within the lithium-rich material 10 toward the outside of the lithium-rich material 10 and outward to the outside of the lithium-rich material 10.
[0062] In one embodiment, the carbon nanomaterials 11 contained in the particles of different lithium replenishing materials 1 are different. The different carbon nanomaterials 11 can mean that the types of carbon nanomaterials 11 are different, or that the number of carbon nanomaterials 11 is different, or that both the types and the number of carbon nanomaterials 11 are different. In one embodiment, the carbon nanomaterials 11 in some lithium replenishing material 1 particles are carbon nanotubes, and the carbon nanomaterials 11 in some lithium replenishing material 1 particles are carbon nanospheres. In another embodiment, all carbon nanomaterials 11 in the lithium replenishing material 1 particles are carbon nanotubes; some lithium replenishing material 1 particles contain one carbon nanotube, and some lithium replenishing material 1 particles contain three carbon nanotubes.
[0063] In one embodiment, each lithium replenishment material 1 particle contains the same carbon nanomaterial 11.
[0064] In one implementation, the maximum distance between the outer surfaces of the carbon nanomaterial 11 and the lithium-rich material 10 is greater than or equal to the radius of the lithium replenishment material 1. The fact that the maximum distance between the outer surfaces of the carbon nanomaterial 11 and the lithium-rich material 10 along the radial direction of the lithium replenishment material 1 is greater than or equal to the radius of the lithium replenishment material 1 indicates that the volume of the carbon nanomaterial 11 is relatively smaller than that of the lithium-rich material 10. The lithium-rich material 10 occupies the majority of the internal space of the lithium replenishment material 1, allowing the lithium replenishment material 1 to provide more lithium ions to compensate for the lithium loss caused by the formation of the SEI film. Therefore, the lithium replenishment material 1 has good lithium replenishment capability and can effectively improve the energy density of the battery.
[0065] In one embodiment, the minimum distance between the carbon nanomaterial 11 and the outer surface of the lithium-rich material 10 can be 0.
[0066] In one implementation, the ratio of the diameter of the carbon nanomaterial 11 to the diameter of the lithium-rich material 10 is less than or equal to 0.1. When the carbon nanomaterial 11 is a carbon nanotube, its diameter is the same as that of the carbon nanotube. When the carbon nanomaterial 11 is a carbon nanosphere, its diameter is the same as that of the carbon nanosphere. When the carbon nanomaterial 11 is a carbon nanofiber, its diameter is the same as that of the carbon nanofiber.
[0067] In this application, the ratio of the diameter of carbon nanomaterial 11 to the diameter of lithium-rich material 10 is relatively small, and the volume of carbon nanomaterial 11 is relatively small compared to lithium-rich material 10. Lithium-rich material 10 occupies most of the internal space of lithium replenishment material 1, which allows lithium replenishment material 1 to provide more lithium ions to replenish the lithium loss caused by the formation of SEI film. Lithium replenishment material 1 has good lithium replenishment capability and can effectively improve the energy density of battery.
[0068] In one embodiment, the ratio of the diameter of the carbon nanomaterial 11 to the diameter of the lithium-rich material 10 can be 0.1, 0.095, 0.09, 0.085, 0.08, 0.075, 0.07, 0.065, 0.06, 0.055, 0.05, 0.045, 0.04, 0.035, 0.03, 0.025, 0.02, 0.015, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, or 0.001.
[0069] In one implementation, each lithium-rich material 1 particle includes 1-20 carbon nanomaterials 11, which are dispersed within the lithium-rich material 10.
[0070] In one implementation, the carbon nanomaterial 11 is a carbon nanotube, and each particle of the lithium-rich material 1 includes 1-20 carbon nanotubes, which are dispersed within the lithium-rich material 10 (e.g., ...). Figure 1 (As shown). Carbon nanotubes possess excellent electrical conductivity, and their elongated shape allows for better construction of the conductive network in the lithium replenishment material 1, thus improving its conductivity. Furthermore, while enhancing conductivity, carbon nanotubes occupy a relatively small volume, with most of the volume of the lithium-rich material 10 occupying the space between the lithium nanotubes and the SEI film. This allows the lithium replenishment material 1 to provide more lithium ions to compensate for lithium loss during SEI film formation, effectively increasing the battery's energy density. Additionally, the elongated shape of the carbon nanotubes allows for better integration into the lithium replenishment material 1, improving its stability.
[0071] In one implementation, a portion of the carbon nanomaterial 11 is located on the outer surface of the lithium-supplementing material 1 particle. For example... Figure 3 The carbon nanomaterial 11b is located on the outer surface of the lithium supplement material 1 particles. The diverse positions of the carbon nanomaterial 11b are more conducive to constructing a conductive network to improve the conductivity of the lithium supplement material 1.
[0072] In one implementation, at least a portion of the carbon nanomaterial 11 extends from within the lithium-replenishing material 1 to the outside of the lithium-replenishing material 1. For example... Figure 3The carbon nanomaterial 11a is located partly inside the lithium supplement material 1 particle and partly outside the lithium supplement material 1. The diverse positions of the carbon nanomaterial 11a are more conducive to constructing a conductive network to improve the conductivity of the lithium supplement material 1.
[0073] In one implementation, the mass ratio of lithium-rich material 10 to lithium replenishment material 1 is 80%-99%. This mass ratio refers to the content of lithium-rich material 10 in lithium replenishment material 1. It is understandable that a higher content of lithium-rich material 10 in lithium replenishment material 1 allows it to provide more lithium ions to offset the irreversible lithium loss caused by the formation of the SEI film. However, an excessively high content of lithium-rich material 10 may also lead to poor conductivity in lithium replenishment material 1.
[0074] In this embodiment, by setting the mass percentage of lithium-rich material 10 to lithium-replenishing material 1 in the range of 80%-99%, not only is lithium-replenishing material 1 given better lithium replenishment capability, but other properties such as conductivity of lithium-replenishing material 1 can also be comprehensively improved.
[0075] In one embodiment, the mass ratio of lithium-rich material 10 to lithium-replenishing material 1 can be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 97%, or 99%.
[0076] In one implementation, the mass ratio of carbon nanomaterial 11 to lithium-rich material 10 is 1% to 25%. The relative content of carbon nanomaterial 11 and lithium-rich material 10 affects the performance of lithium replenishment material 1. If the content of carbon nanomaterial 11 is too high, although it can enhance the conductivity of lithium replenishment material 1, the amount of lithium ions that lithium replenishment material 1 can provide is reduced, affecting the lithium replenishment capacity of lithium replenishment material 1. If the content of lithium-rich material 10 is too high, although it can provide more lithium ions, the conductivity of lithium replenishment material 1 is poor, reducing the energy density of the battery.
[0077] In this embodiment, the mass ratio of carbon nanomaterial 11 to lithium-rich material 10 is set in the range of 1% to 25%. This not only ensures that the lithium replenishment material 1 can provide enough lithium ions to compensate for the irreversible lithium loss caused by the formation of the SEI film, but also improves the conductivity of the lithium replenishment material 1.
[0078] In one embodiment, the mass ratio of carbon nanomaterial 11 to lithium-rich material 10 can be 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 21%, 22%, 23%, 24%, or 25%.
[0079] In one implementation, the carbon nanomaterial 11 is a carbon nanotube. Carbon nanotubes possess excellent electrical conductivity, thereby improving the conductivity of the lithium replenishment material 1. Simultaneously, due to their elongated shape, carbon nanotubes can be well integrated into the lithium replenishment material 1, enhancing its stability.
[0080] In one implementation, the aspect ratio of the carbon nanotubes is 7-70. The aspect ratio of carbon nanotubes refers to the ratio of the length to the diameter of the carbon nanotube. If the aspect ratio of the carbon nanotubes is too small, it is not conducive to forming a conductive network inside the lithium-rich material 1, which is not conducive to improving the conductivity of the lithium-rich material 1. If the aspect ratio of the carbon nanotubes is too large, the carbon nanotubes are too long, and it is not easy for the carbon nanotubes to be encapsulated within the lithium-rich material 10, which increases the difficulty of preparing the lithium-rich material 1.
[0081] In this application, the aspect ratio of carbon nanotubes is set in the range of 10-100. On the one hand, a suitable aspect ratio can improve the conductivity of carbon nanotubes, thereby improving the conductivity of lithium replenishment material 1. On the other hand, a suitable aspect ratio makes it easier for carbon nanotubes to be encapsulated in lithium replenishment material 1, making the preparation process simpler and facilitating the industrial production of lithium replenishment material 1.
[0082] In one embodiment, the aspect ratio of the carbon nanotubes is 10, 20, 30, 40, 50, 60, 70, 80, 90 or 100.
[0083] In one implementation, the diameter of the carbon nanotubes is 20 nm to 80 nm. The conductivity of carbon nanotubes is related to their diameter; carbon nanotubes with a suitable diameter have better conductivity, which is more conducive to improving the conductivity of lithium-supplementing material 1.
[0084] In one embodiment, the diameter of the carbon nanotubes is 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, or 80 nm.
[0085] In one implementation, the carbon nanotubes have a length of 0.2 μm to 2 μm. A length within this range facilitates the formation of a conductive network, thereby improving the conductivity of the lithium-supplementing material 1. Simultaneously, the suitable length of the carbon nanotubes makes the preparation of the lithium-supplementing material 1 easier.
[0086] In one implementation, the length of the carbon nanotubes is 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, or 2 μm.
[0087] In one implementation, the lithium-supplementing material 1 is obtained by lithiation of an intermediate, which is formed by depositing a lithium-rich material precursor on the framework of carbon nanomaterial 11. Lithiation of the lithium-rich material precursor yields the lithium-rich material 10. The metal precursor can be a metal hydroxide. The intermediate is a composite material formed by the deposition of the metal precursor on the carbon nanomaterial 11. Lithiation of the intermediate refers to the reaction of the metal hydroxide in the intermediate with a lithium source to generate the lithium-rich material 10, at which point the lithium-rich material 10 encapsulates the carbon nanomaterial 11 to form the lithium-supplementing material 1.
[0088] In this application, the metal precursor grows and deposits continuously with carbon nanomaterial 11 as the core, eventually attaching to the carbon nanomaterial 11 and coating it to form a particulate intermediate. The intermediate is then lithiated to obtain the lithium supplement material 1. This formation method results in a high bonding force between the carbon nanomaterial 11 and the lithium-rich material 10, making it less likely for the carbon nanomaterial 11 to fall off, and thus improving the conductivity of the lithium supplement material 1.
[0089] In one implementation, the general structural formula of the lithium-rich material 10 is Li. 1+x A y O z Where 0 < x < 10, 0 < y < 6, 0 < z < 13, and A is one or more of Ni, Co, Fe, Cu, Mg, Mn, Cr, Zn, Ti, Zr, Nb, and Mo. This type of lithium-rich material 10 can be better matched with the structure of the lithium-supplementing material 1 and the carbon nanomaterial 11 in this application, so that the lithium-supplementing material 1 has better performance.
[0090] In one embodiment, the lithium-rich material 10 is selected from Li8ZrO6, Li5FeO4, Li6MnO4, Li6CoO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, and Li2Ni 0.5 Mn 1.5 One or more of O4 and Li6ZnO4.
[0091] In one implementation, the carbon nanomaterial 11 includes at least one of carbon nanotubes, carbon nanofibers, carbon nanospheres, and graphene. These types of carbon nanomaterials 11 have stable structures and are not easily exfoliated, which can better improve the stability of the lithium supplement material 1.
[0092] In one implementation, the particle size of the lithium replenishment material satisfies: 4μm ≤ D50 ≤ 20μm. D50 refers to the particle size corresponding to a cumulative particle size distribution percentage of 50% in the lithium replenishment material 1. If the particle size of the lithium replenishment material 1 is too small, it is prone to agglomeration, making it difficult for lithium inside the lithium replenishment material 1 to be extracted when replenishing active lithium to the negative electrode, thus reducing the lithium replenishment effect of the lithium replenishment material 1; while if the particle size of the lithium replenishment material 1 is too large, its dispersibility is poor, which is not conducive to the preparation of the positive electrode sheet.
[0093] In this embodiment, the particle size D50 of the lithium replenishment material 1 is controlled between 4 micrometers and 20 micrometers. This ensures the rapid extraction of lithium ions while also improving the dispersibility of the lithium replenishment material 1, making it easier to use.
[0094] In one embodiment, the particle size D50 of the lithium replenishment material 1 can be 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14μm, 14.5μm, 15μm, 16μm, 17μm, 18μm, 19μm, or 20μm.
[0095] In one implementation, the specific surface area of the lithium-supplementing material is 0.5 m². 2 / g-30m 2 / g. In one embodiment, the specific surface area is tested using the BET (Brunauer-Emmett-Teller) specific surface area test method, and the specific surface area is the BET specific surface area. If the specific surface area of the lithium replenishment material 1 is too small, it is not conducive to improving the conductivity and lithium ion extraction and insertion capabilities of the lithium replenishment material 1; if the specific surface area of the lithium replenishment material 1 is too large, the density of the lithium replenishment material 1 is usually low, and the volumetric energy density is low.
[0096] In this embodiment, the specific surface area of the lithium replenishment material 1 is controlled to be 0.5 m². 2 / g-30m 2 Within the range of / g, it can not only improve the conductivity and lithium ion extraction and insertion capabilities of the lithium replenishment material, but also improve the volumetric energy density of lithium replenishment material 1.
[0097] In one embodiment, the specific surface area of the lithium replenishing material 1 is 1 m². 2 / g-10m 2 / g.
[0098] In one embodiment, the specific surface area of the lithium replenishing material 1 is 1 m². 2 / g-4m 2 / g.
[0099] In one embodiment, the specific surface area of the lithium replenishment material can be 0.5 m². 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g、1m 2 / g、2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g、9m 2 / g, 10m 2 / g、11m 2 / g、12m 2 / g、13m 2 / g、14m 2 / g, 15m 2 / g, 16m 2 / g、17m 2 / g、18m 2 / g、19m 2 / g、20m 2 / g、21m 2 / g、22m 2 / g、23m 2 / g、24m 2 / g、25m 2 / g、26m 2 / g、27m 2 / g、28m 2 / g、29m 2 / g or 30m 2 / g.
[0100] This application provides a method for preparing a lithium-supplementing material 1. The method for preparing the lithium-supplementing material includes steps S1 and S2, as detailed below:
[0101] Step S1: Add the carbon nanomaterial 11 solution and the metal solution to the reactor, and adjust the pH of the solution in the reactor to alkaline to obtain the intermediate.
[0102] Step S2: Mix the intermediate with the lithium source and sinter under an inert atmosphere to obtain lithium supplement material 1.
[0103] In step S1, the metal solution can be a metal salt solution, which can be converted into a metal hydroxide under alkaline conditions and deposited on the carbon nanomaterial 11 in the form of metal hydroxide. The intermediate is the carbon nanomaterial 11 with the metal hydroxide deposited on it. In step S2, the intermediate is lithiated, that is, the metal hydroxide in the intermediate reacts with the lithium source to generate a lithium-rich material 10, thereby obtaining the lithium-replenishing material 1.
[0104] In this embodiment, the concentration of the metal solution and the concentration of the carbon nanomaterial 11 solution are adjusted to regulate the content of lithium-rich material 10 in the lithium-replenishing material 1. In this application, metal hydroxide is deposited on carbon nanomaterial 11 by co-precipitation, and then the metal hydroxide is lithiated to obtain lithium-replenishing material 1. This formation method results in a high bonding force between carbon nanomaterial 11 and lithium-rich material 10, making it less likely for carbon nanomaterial 11 to detach, and thus improving the conductivity of lithium-replenishing material 1.
[0105] In one embodiment, the pH of the solution in the reactor is 9-12.
[0106] In one embodiment, the reactor is a ternary reactor.
[0107] In one embodiment, the concentration of the metal solution is 1-4 mol / L.
[0108] In one embodiment, the carbon nanomaterial 11 solution is added to the reactor at a rate of 5-50 ml / min, and the metal solution is added to the reactor at a rate of 0.2-1 ml / min.
[0109] In one embodiment, the preparation method of lithium supplement material 1 further includes the synthesis of carbon nanomaterial 11 solution: carbon nanomaterial 11, water and dispersant are mixed in a mass ratio of (2-11):(1000):(0.4-2.2) to obtain a carbon nanomaterial 11 solution with a concentration of 2-11 g / L.
[0110] In one embodiment, the sintering temperature of the intermediate and the lithium source is 700-900°C, and the sintering time is 4-20h.
[0111] In one embodiment, the metal solution can be at least one of a metal sulfate, carbonate, or chloride.
[0112] In one embodiment, the pH adjusting agent for the solution in the reactor is at least one of ammonia, sodium hydroxide, and potassium hydroxide.
[0113] In one embodiment, the lithium source includes at least one of lithium hydroxide, lithium oxide, lithium oxalate, and lithium carbonate.
[0114] In one embodiment, the inert atmosphere includes one or more of nitrogen, argon, and helium.
[0115] This application provides a positive electrode sheet, which includes the lithium replenishing material 1 as described above, or the lithium replenishing material 1 prepared by the preparation method of the lithium replenishing material 1 as described above.
[0116] This application provides a secondary battery, which includes a negative electrode, a separator, and a positive electrode as described above.
[0117] In one embodiment, the secondary battery is a lithium-ion secondary battery.
[0118] To illustrate the beneficial effects of the method of this application, the following embodiments and comparative examples are also provided.
[0119] Example 1
[0120] This embodiment provides a lithium replenishment material 1, which includes a lithium-rich material and a carbon nanomaterial. The lithium-rich material 10 is Li2NiO2, and the carbon nanomaterial 11 is carbon nanotube. The mass ratio of carbon nanotube to Li2NiO2 is 1%, and the mass ratio of Li2NiO2 to lithium replenishment material 1 is 99%. Ten carbon nanotubes are dispersed in the particles of lithium replenishment material 1.
[0121] The preparation method of lithium supplement material 1 in this embodiment includes the following steps:
[0122] Step 1: Synthesize carbon nanotube solution: Mix carbon nanotubes, water, and sodium dodecyl sulfate at a mass ratio of 5:1000:1 to obtain a high-concentration carbon nanotube solution (i.e., carbon nanomaterial 11 solution) of 8 g / L.
[0123] Step 2: Prepare nickel hydroxide deposited on carbon nanotubes using a co-precipitation method. The high-concentration carbon nanotube solution synthesized in Step 1 is pumped into a ternary reactor at a rate of 5-20 ml / min. Then, a 2 mol / L high-concentration nickel sulfate solution is pumped into the ternary reactor at a rate of 0.2-1 ml / min. Simultaneously, the pH of the solution is adjusted to 11, and high-speed stirring is maintained for a period of time to synthesize the material with nickel hydroxide deposited on carbon nanotubes.
[0124] Step 3: Add lithium source to the material prepared in step 2 by molar ratio, and sinter at 780℃ for 10h under an inert atmosphere to obtain Li2NiO2 deposited on carbon nanotubes as positive electrode lithium replenishment material 1.
[0125] Testing revealed that in lithium replenishment material 1, the D50 particle size was 3.35 μm and the BET specific surface area was 3.5 m². 2 / g.
[0126] Example 2
[0127] The difference from lithium supplement material 1 in Example 1 is that the mass ratio of carbon nanotubes to Li2NiO2 is 15%.
[0128] Example 3
[0129] The difference from lithium supplement material 1 in Example 1 is that the mass ratio of Li2NiO2 to lithium supplement material 1 is 50%.
[0130] Example 4
[0131] The difference between lithium replenishing material 1 and lithium replenishing material 1 in Example 1 is that lithium replenishing material 1 particles include 5 carbon nanotubes.
[0132] Example 5
[0133] The difference between this material and the lithium-supplementing material 1 in Example 1 is that the carbon nanomaterial 11 is a carbon nanosphere.
[0134] Comparative Example 1
[0135] The difference from Example 1 is that in Comparative Example 1, the carbon nanomaterials 11 are concentrated within the lithium-rich material 10, that is, the lithium-replenishing material 1 has a core-shell structure, the core is composed of carbon nanomaterials 11, and the lithium-rich material 10 covers the outside of the core.
[0136] Comparative Example 2
[0137] The difference from Example 1 is that the lithium supplement material 1 in Comparative Example 2 has a core-shell structure, with the core composed of lithium-rich material 10 and carbon nanomaterial 11 covering the outside of the core, and the mass ratio of carbon nanotubes to Li2NiO2 is 15%.
[0138] The lithium replenishment materials provided in Examples 1-5 and the lithium replenishment materials provided in Comparative Examples 1 and 2 were assembled into positive electrode electrodes and lithium-ion batteries respectively according to the following methods:
[0139] Positive electrode sheet: The positive electrode lithium supplement material is mixed with lithium manganese iron phosphate at a mass ratio of 5:95 to obtain a mixture. The mixture is then mixed with polyvinylidene fluoride and SP-Li at a mass ratio of 95:3:2 and ball-milled to obtain a positive electrode slurry. The positive electrode slurry is coated on the surface of aluminum foil, rolled, and then vacuum dried at 110°C overnight to obtain the positive electrode sheet.
[0140] Negative electrode: Lithium metal sheet;
[0141] Electrolyte: Ethyl carbonate and ethyl methyl carbonate are mixed in a volume ratio of 3:7, and LiPF6 is added to form an electrolyte with a concentration of 1 mol / L.
[0142] Diaphragm: Polypropylene microporous diaphragm;
[0143] Lithium-ion battery assembly: Lithium-ion batteries are assembled in an inert atmosphere glove box according to the assembly sequence of lithium metal sheet-separator-electrolyte-positive electrode.
[0144] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery examples was tested as shown in Table 1, and the test conditions were as follows:
[0145] Constant current and constant voltage charging, first charge / discharge voltage 2.5-4.3V, current 0.1C, cut-off current 0.01C.
[0146] The relevant performance test results are shown in Table 1 below:
[0147] Table 1 Performance Test Results
[0148]
[0149]
[0150] As can be seen from Table 1, Examples 1-5 and Comparative Examples 1-2, the proportion of lithium-rich material Li2NiO2 in the lithium replenishment material, the number of carbon nanotubes in the lithium replenishment material, and the type of carbon nanomaterial all affect the performance of the composite cathode (specific capacity of the first charge, initial coulombic efficiency, capacity retention rate, and specific capacity of the lithium replenishment). This is because carbon nanomaterials can improve the conductivity and structural stability of Li2NiO2, and a high proportion of Li2NiO2 can improve the lithium replenishment performance after composite.
[0151] Comparing Examples 1-3 and Comparative Example 2, it can be seen that when the proportion of Li2NiO2 in the lithium replenishment material is high, both the initial charging specific capacity and the lithium replenishment specific capacity are improved. This is because the high proportion of Li2NiO2 in the lithium replenishment material can provide more Li + This is to compensate for the lithium loss during the initial charging of the positive electrode. Furthermore, as can be seen from Example 2 and Comparative Example 2, compared to Comparative Example 2 where the carbon nanomaterials are only located on the surface of the lithium-rich material, in Example 2, the carbon nanomaterials are dispersed on the surface of the lithium-rich material, which can better improve the conductivity of the lithium-replenishing material, thereby achieving a higher initial coulombic efficiency.
[0152] Comparing Example 1 and Comparative Example 1, it can be seen that when carbon nanomaterials are partially coated by lithium-rich materials or located on the surface of lithium-rich materials, their initial coulombic efficiency and capacity retention are improved. This is because the surface carbon nanomaterials further enhance the conductivity of Li₂NiO₂ and Li₂. + Transmission rate. However, compared to Comparative Example 1, Example 1 exhibits superior first coulombic efficiency and capacity retention, indicating that carbon nanomaterials embedded in lithium-rich materials in a dispersed form (Example 1) are more effective in improving the electrochemical performance of the battery than carbon nanomaterials concentrated within lithium-rich materials (Comparative Example 1).
[0153] Comparing Examples 1, 4, and 5, it can be seen that the number of carbon nanotubes and the type of carbon nanomaterial in the lithium replenishment material also affect the subcoulombic efficiency and capacity retention. Within a certain range, increasing the number of carbon nanomaterials and selecting a suitable type of carbon nanomaterial can improve electrochemical performance. Compared to Examples 4 and 5, Example 1 selects carbon nanotubes as the carbon nanomaterial and increases the number of carbon nanotubes, which can better construct the conductive network of the lithium replenishment material, thereby better improving the electrochemical performance of the battery.
[0154] The lithium replenishment materials, their preparation methods, positive electrode sheets, and secondary batteries provided in the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and embodiments of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the methods and core ideas of this application. At the same time, for those skilled in the art, there will be changes in specific embodiments and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A lithium supplementation material, characterized in that, The lithium supplementation material includes: A lithium-rich material, a structural general formula of the lithium-rich material is Li 1+x A y O z Wherein, 0 < x < 10, 0 < y < 6, 0 < z < 13, A is one or more of Ni, Co, Fe, Cu, Mg, Mn, Cr, Zn, Ti, Zr, Nb, Mo; A carbon nanomaterial, wherein the carbon nanomaterial is embedded within a lithium-rich material, the carbon nanomaterial is dispersed, the carbon nanomaterial surrounds an accommodating space, a portion of the lithium-rich material is deposited on the outer surface of the carbon nanomaterial, a portion of the lithium-rich material is embedded within the accommodating space; a portion of the carbon nanomaterial is located on the outer surface of the lithium-rich material; and / or, at least a portion of the carbon nanomaterial extends from within the lithium-rich material to the outside of the lithium-rich material; The carbon nanomaterial includes carbon nanotubes, and the accommodating space is the internal space of the carbon nanotubes; The lithium-rich material forms a coating layer that coats at least a portion of the outer surface of the carbon nanomaterial. The thickness of the coating layer refers to the minimum, maximum, or average distance between the outer surface of the carbon nanomaterial and the outer surface of the lithium-rich material. The thickness of the coating layer ranges from 4 μm to 20 μm. And / or, the thickness of the coating layer is greater than the diameter or length of the carbon nanomaterial. The lithium replenishing material is obtained by lithiation of an intermediate, comprising: mixing the intermediate with a lithium source and sintering it under an inert atmosphere to obtain the lithium replenishing material; the intermediate is formed by depositing a lithium-rich material precursor on the framework of the carbon nanomaterial.
2. The lithium replenishment material according to claim 1, characterized in that, Each of the lithium-rich material particles includes a plurality of the carbon nanomaterials, which are dispersed within the lithium-rich material.
3. The lithium replenishment material according to claim 1, characterized in that, The mass ratio of the lithium-rich material to the lithium-replenishing material is 80%-99%; and / or, the mass ratio of the carbon nanomaterial to the lithium-rich material is 1%-25%.
4. The lithium replenishment material according to claim 1, characterized in that, The particle size of the lithium supplementation material satisfies: 4μm≤D50≤20μm; and / or The specific surface area of the lithium supplementing material is 0.5m 2 / g-30m 2 / g.
5. The lithium replenishment material according to claim 1, characterized in that, The carbon nanotubes have an aspect ratio of 10-100; and / or The carbon nanotubes have a diameter of 20 nm to 80 nm; and / or The length of the carbon nanotubes is 0.2μm-2μm.
6. The lithium replenishment material according to claim 1, characterized in that, The lithium-rich material is obtained by lithiation of the lithium-rich material precursor.
7. A method for preparing a lithium-supplementing material, characterized in that, The method for preparing the lithium supplementation material includes: A carbon nanomaterial solution and a metal solution are added to a reactor, and the pH of the solution in the reactor is adjusted to be alkaline to obtain an intermediate. The intermediate is mixed with a lithium source and sintered under an inert atmosphere to obtain the lithium replenishment material. The lithium supplementing material comprises a lithium-rich material and a carbon nanomaterial, the lithium-rich material has a general structure of Li 1+x A y O z wherein, 0 The carbon nanomaterial is in a dispersed state, the carbon nanomaterial is surrounded by a containing space, part of the lithium-rich material is deposited on the outer surface of the carbon nanomaterial, and part of the lithium-rich material is embedded in the containing space; part of the carbon nanomaterial is located on the outer surface of the lithium-rich material; and / or, at least part of the carbon nanomaterial extends from the lithium-rich material to the outside of the lithium-rich material; the carbon nanomaterial comprises carbon nanotubes, and the containing space is the inner space of the carbon nanotubes. The lithium-rich material forms a coating layer that coats at least a portion of the outer surface of the carbon nanomaterial. The thickness of the coating layer refers to the minimum, maximum, or average distance between the outer surface of the carbon nanomaterial and the outer surface of the lithium-rich material. The thickness of the coating layer ranges from 4 μm to 20 μm. And / or, the thickness of the coating layer is greater than the diameter or length of the carbon nanomaterial.
8. A positive electrode sheet, characterized in that, The positive electrode sheet includes the lithium replenishing material as described in any one of claims 1-6, or the lithium replenishing material prepared by the method for preparing the lithium replenishing material as described in claim 7.
9. A secondary battery, characterized in that, The secondary battery includes a negative electrode, a separator, and a positive electrode as described in claim 8.
Citation Information
Patent Citations
Nickel hydroxide / multi-walled carbon nanotube composite material and preparation method thereof
CN103943372A
Lithium-supplementing additive as well as preparation method and application thereof
CN107819113A
Lithium-supplementing material Li2NiO2 as well as preparation method and application thereof
CN110218078A
Lithium supplementing material and preparation method thereof, negative electrode and lithium ion battery
CN112993251A
Preparation method and application of precursor of aluminum and zirconium doped lithium nickelate positive electrode material
CN113809321A