A HCPDI-CdSe NPs film and its preparation method and application

By combining highly conjugated PDI with CdSe nanoparticles to prepare HCPDI-CdSe NPs films, the problem of narrow photoresponse range of inorganic semiconductor materials and high photogenerated charge recombination rate of organic semiconductor materials is solved, achieving efficient photocatalytic full water splitting ability. and stability, suitable for commercial applications.

CN116459868BActive Publication Date: 2024-10-15TAIYUAN UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310215341.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-08
Publication Date
2024-10-15
Estimated Expiration
2043-03-08

AI Technical Summary

Technical Problem

Existing inorganic semiconductor materials have a narrow photoresponse range and cannot effectively utilize visible light. In addition, organic semiconductor materials have problems such as high photogenerated charge recombination rate, poor transfer and separation ability, and complex synthesis processes, which hinder the improvement of photocatalytic performance.

Method used

By combining highly conjugated PDI with CdSe nanoparticles, HCPDI-CdSe NPs films are prepared, and self-assembled HCPDI is used to form hydrogen bonds with CdSe nanoparticles to improve its stability at the interface and photocatalytic performance.

Benefits of technology

It achieves good photocatalytic total water splitting ability without the need for a cocatalyst, improves photocatalytic performance and stability, has a simple process and low cost, and is suitable for large-area applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116459868B_ABST
    Figure CN116459868B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of photocatalytic materials, and specifically relates to a HCPDI-CdSe NPs film and a preparation method and application thereof. The preparation method of the HCPDI-CdSe NPs film of the present invention comprises the following steps: (1) CdSe nanoparticles are uniformly mixed with self-assembled HCPDI and a solvent to obtain a mixture I; (2) the mixture I obtained by the treatment of step (1) is applied to the surface of a glass slide, dried, and annealed in a rare gas atmosphere to obtain the HCPDI-CdSe NPs film. The HCPDI-CdSe NPs prepared by the method of the present invention have very good film-forming properties and a smooth surface. If synthesized according to the steps of the present invention, the formed film can only be wiped off and the sample can be damaged by contacting an organic solvent or applying mechanical force, which is very convenient for the recovery of the catalyst. It has a good photocatalytic ability to completely split water without adding a co-catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a HCPDI-CdSe NPs film and a preparation method and application thereof. Background Art

[0002] Faced with increasingly severe environmental problems, we urgently need to transform our energy. How to achieve efficient conversion of clean, renewable solar energy has become a research hotspot for many scholars. Semiconductor photocatalysis is a technology that uses semiconductors to convert and store solar energy into chemical energy. Semiconductor photocatalysis technology is limited by three aspects: absorption of sunlight, separation and transfer of charges, and interfacial reactions of catalysts. Traditional semiconductor materials cannot optimize these issues at the same time, which severely limits their application. Therefore, a lot of work is used to explore their modification. In this process, a semiconductor material with an organic-inorganic structure gradually came into our view.

[0003] Inorganic semiconductor materials have always been a research hotspot in this field, but most of them have a narrow light response range and only show photocatalytic effects in the ultraviolet region; and ultraviolet light only accounts for about 5% of the sunlight spectrum, which hinders their commercial promotion. Organic semiconductor materials have gradually attracted attention because of their good visible light response, but they still have problems such as high photogenerated charge recombination rate, poor photogenerated carrier transfer and separation ability, and complex synthesis process. If the superior charge transfer and separation ability of inorganic semiconductor materials and the superior light absorption ability of organic semiconductors can be combined to form a new type of photocatalytic semiconductor material, it will provide a new possibility for the formation of commercial photocatalytic materials. However, this material still has the problems of mismatched energy band relationship, difficult and unstable connection of organic-inorganic interface, which will hinder the rapid migration of photogenerated carriers at the interface and seriously affect its photocatalytic performance.

[0004] In addition, in general, the synthesis of organic semiconductors has problems such as complex process, high cost and toxic synthesis environment; the synthesis of CdSe nanoparticles has problems such as many steps and unstable structure; after mixing, the finished product performance is low and CdSe photocorrosion is serious.

[0005] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention

[0006] The purpose of the present invention is to provide a HCPDI-CdSe NPs film and a preparation method and application thereof, so as to solve or improve the problem in the prior art that the photocatalytic performance of organic-inorganic semiconductor materials needs to be improved. The HCPDI-CdSe nanoparticles (NPs) of the present invention are obtained by compounding highly conjugated PDI (3,4,9,10-perylenetetracarboxylic acid diimide) with CdSe.

[0007] In order to achieve the above-mentioned object, the present invention provides the following technical scheme: a method for preparing a HCPDI-CdSe NPs film, comprising the following steps: (1) uniformly mixing CdSe nanoparticles, self-assembled HCPDI and a solvent to obtain a mixture I; (2) applying the mixture I obtained by the treatment in step (1) on the surface of a glass slide, drying it, and annealing it in a rare gas atmosphere to obtain the HCPDI-CdSe NPs film.

[0008] Preferably, the self-assembled HCPDI is obtained by self-assembly of 3,4,9,10-perylenetetracarboxamide diimide under acidic conditions; and the mass ratio of the CdSe nanoparticles to HCPDI is (0.9-1.1):1.

[0009] Preferably, in step (2), the annealing temperature is 240-260° C., and the annealing time is 1.9-2.1 h.

[0010] Preferably, the CdSe nanoparticles are prepared by a method comprising the following steps: A1. mixing and grinding sodium sulfite, selenium powder and sodium hydroxide to obtain a first mixture; A2. mixing and grinding the first mixture and cadmium acetate to obtain a second mixture in a blocky brown color; A3. washing the second mixture to obtain a CdSe paste; A4. drying and grinding the CdSe paste to obtain a CdSe powder; A5. annealing the CdSe powder to obtain the CdSe nanoparticles.

[0011] Preferably, the molar ratio of the sodium sulfite, selenium powder and sodium hydroxide is 1:(1.81-1.83):(3.63-3.65); the molar ratio of cadmium acetate to selenium powder is (0.9-5.1):1.

[0012] Preferably, in step A3, the second mixture is washed with water and then with alcohol; in step A4, the drying is carried out in a rare gas atmosphere, the drying temperature is 85-95°C, and the drying time is 9.9-10.1h; in step A5, the annealing temperature is 245-255°C, and the annealing time is 1.9-2.1h.

[0013] Preferably, the self-assembled HCPDI is prepared according to a method comprising the following steps: B1. 3,4,9,10-perylenetetracarboxylic acid diimide is mixed with concentrated sulfuric acid, and after ultrasonication, a red mixed solution is obtained; B2. The red mixed solution obtained by the treatment in step B1 is mixed evenly with an ethylene glycol aqueous solution, and after standing, a purple-red suspension is obtained; B3. The purple-red suspension is centrifuged and washed to obtain the self-assembled HCPDI.

[0014] Preferably, in step B1, the mass volume ratio of 3,4,9,10-perylenetetracarboxylic acid diimide to concentrated sulfuric acid is 1:(195-205); in step B2, the volume ratio of concentrated sulfuric acid to ethylene glycol aqueous solution is 1:(9.9-10.1), and the standing time is 44-46 min.

[0015] The present invention also proposes a HCPDI-CdSe NPs film, which adopts the following technical solution: a HCPDI-CdSe NPs film, wherein the HCPDI-CdSe NPs film is prepared by the method as described above.

[0016] The present invention also proposes an application of a HCPDI-CdSe NPs film, which adopts the following technical solution: application of the HCPDI-CdSe NPs film as described above in photocatalytic water splitting.

[0017] Beneficial effects:

[0018] (1) The HCPDI-CdSe NPs prepared by the method of the present invention have very good film-forming properties and a smooth surface. If synthesized according to the steps of the present invention, the formed film can only be wiped off and the sample damaged by contact with an organic solvent or mechanical force. It has good photocatalytic water splitting ability without adding a promoter. Due to its good film-forming property, it can be used on a large area and has a good application prospect.

[0019] (2) The CdSe nanoparticles used in the preparation method of the HCPDI-CdSe NPs film of the present invention are obtained by grinding a CdSe powder in an air atmosphere, so that the CdSe powder is partially oxidized to CdO during the grinding process, thereby introducing O atoms, which can form hydrogen bonds between the CdSe nanoparticles and the HCPDI. Because of their saturation and directionality, the CdSe nanoparticles can be evenly dispersed and stably bound on the surface of the HCPDI, can exist in a solid form at room temperature, and can still exist stably after the hydrolysis reaction.

[0020] (3) The equipment and raw materials used in the present invention are cheap, the experimental steps are simple and easy to operate, the product yield and yield are high, the obtained product has good performance and high stability, and is easy to use and recycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings constituting a part of the specification of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their description are used to explain the present invention and do not constitute improper limitations on the present invention.

[0022] in:

[0023] Figure 1A state diagram of a tube furnace used in an embodiment of the present invention (used for annealing to generate HCPDI-CdSeNPs thin film);

[0024] Figure 2 This is a microscopic morphology of the HCPDI-CdSe NPs film prepared in Example 1 of the present invention;

[0025] Figure 3 This is a state diagram of the HCPDI-CdSe NPs film of an embodiment of the present invention performing complete water splitting in a photocatalytic quartz reactor;

[0026] Figure 4 This is a picture of the HCPDI-CdSe NPs film of an embodiment of the present invention in a photocatalytic water splitting experiment;

[0027] Figure 5 This is a graph showing the test results of the hydrogen and oxygen production performance of the photocatalytic water splitting of the HCPDI-CdSe NPs film in an embodiment of the present invention;

[0028] Figure 6 This is a physical picture of the HCPDI-CdSe NPs film prepared in an example of the present invention. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0030] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0031] In view of the problem that the photocatalytic performance of current organic-inorganic semiconductor materials needs to be improved, the present invention provides a method for preparing an HCPDI-CdSe NPs film, comprising the following steps: (1) uniformly mixing CdSe nanoparticles, self-assembled HCPDI and a solvent to obtain a mixture I; (2) applying the mixture I obtained by the step (1) on the surface of a glass slide, drying it, and then annealing it in a rare gas atmosphere to obtain the HCPDI-CdSe NPs film.

[0032] Wherein, the "drying" in step (2) refers to the process in which the film changes from wet to dry after the mixture I is applied to the surface of the glass slide, when the mixture I is golden (i.e., golden after the solvent evaporates); the solvent mainly dissolves the HCPDI; preferably, the solvent is a mixed solvent of n-hexane and anhydrous ethanol; preferably, the rare gas is argon; in the present invention, the rare gas cannot be replaced by nitrogen to avoid the introduction of nitrogen into the 3,4,9,10-perylenetetracarboxylic acid diimide molecule; the annealing treatment mainly serves to make the product more crystalline, reduce defects and facilitate electron-hole transport.

[0033] The present invention mixes CdSe nanoparticles with self-assembled HCPDI, and the resulting paste mixture is applied to the surface of a glass slide, so that a film firmly bonded to the glass slide can be obtained, and then annealing treatment can be performed to prepare an HCPDI-CdSe NPs film with good photocatalytic performance. The HCPDI-CdSe NPs film preparation method of the present invention is simple and efficient, and the prepared HCPDI-CdSe NPs film can not only effectively combine inorganic and organic semiconductor materials, but also has a strong full water decomposition ability when it is applied to photocatalytic water decomposition without adding any sacrificial agent.

[0034] In addition, the mixture I has good film-forming property, and the surface is flat after film formation, and can be used in a large area, which has good application prospects. The HCPDI-CdSe NPs film prepared according to the method of the present invention can only be wiped off or damaged when it contacts an organic solvent or applies a large mechanical force, and has good binding property with a glass slide. When the HCPDI-CdSe NPs film needs to be recycled, the HCPDI-CdSe NPs film can be separated from the glass slide by applying an organic solvent or a large mechanical force to it, so as to achieve the recycling of the HCPDI-CdSe NPs film.

[0035] In a preferred embodiment of the present invention, the self-assembled HCPDI is prepared by self-assembly of 3,4,9,10-perylenetetracarboxylic acid diimide under acidic conditions; the mass ratio of CdSe nanoparticles to HCPDI is (0.9-1.1):1 (for example, 0.9:1, 1:1 or 1.1:1). Among them, too many CdSe nanoparticles will lead to aggravated photocorrosion, and the corrosion will stop when it reaches a certain level. Too much HCPDI will lead to an increase in photogenerated holes, a decrease in hydrogen production sites, and a decrease in hydrogen production efficiency.

[0036] In a preferred embodiment of the present invention, in step (2), the annealing temperature is 240-260°C.

[0037] (For example, 240°C, 245°C, 250°C, 255°C or 260°C), and the annealing time is 1.9-2.1h (for example, 1.9h, 2.0h or 2.1h). Among them, too high annealing temperature will lead to carbonization of the product, too low annealing temperature will lead to low crystallinity, too short annealing time will lead to incomplete crystallization, too long annealing time will lead to high cost, which is not worth the cost.

[0038] In a preferred embodiment of the present invention, CdSe nanoparticles are prepared by a method comprising the following steps: A1. Mixing and grinding sodium sulfite, selenium powder and sodium hydroxide to obtain a first mixture; A2. Mixing and grinding the first mixture and cadmium acetate to obtain a second mixture in a brown block form; A3. Washing the second mixture to obtain a CdSe paste; A4. Drying and grinding the CdSe paste to obtain a CdSe powder; A5. Annealing the CdSe powder to obtain CdSe nanoparticles. Among them, the function of step A1 is to convert selenium atoms into selenium ions; step A2 allows the selenium ions obtained in A1 to form cadmium selenide with cadmium ions; step A3 can remove unreacted and generated impurities; step A4 grinds to obtain nano-scale particles; and step A5 performs annealing and crystallization treatment. Preferably, the grinding in step A4 is carried out in an air atmosphere so that during the grinding process, part of the CdSe powder material is oxidized to CdO, thereby introducing O atoms, so that hydrogen bonds can be formed between CdSe NPs and HCPDI. Because of their saturation and directionality, the CdSe nanoparticles can be evenly dispersed and stably bound on the surface of HCPDI, can exist in a solid form at room temperature, and can still exist stably after the hydrolysis reaction.

[0039] In a preferred embodiment of the present invention, the molar ratio of sodium sulfite, selenium powder and sodium hydroxide is 1: (1.81-1.83): (3.63-3.65) (for example, 1: 1.81: 3.63, 1: 1.82: 3.63, 1: 1.83: 3.63, 1: 1.82: 3.64, 1: 1.82: 3.65, 1: 1.83: 3.64 or 1: 1.83: 3.65); the molar ratio of cadmium acetate to selenium powder is (0.9-5.1): 1 (for example, 0.9: 1, 1.5: 1, 2.3: 1, 3.4: 1, 4.2: 1 or 5.1: 1). The ratio of cadmium acetate to selenium powder is changed to change the relative content of Cd and Se. The change of composition can cause the CdSe and HCPDI energy band positions to shift, eventually resulting in a sharp decline in performance. Preferably, the molar ratio of cadmium acetate to selenium powder is (0.9-3):1 (eg, 0.9:1, 1.5:1, 2.1:1, 2.6:1 or 3:1).

[0040] In a preferred embodiment of the present invention, in step A3, the second mixture is washed with water and alcohol successively; in step A4, drying is carried out in a rare gas (e.g., argon) atmosphere, the drying temperature is 85-95°C (e.g., 85°C, 90°C, or 95°C), and the drying time is 9.9-10.1h (e.g., 9.9h, 10.0h, or 10.1h); in step A5, the annealing temperature is 245-255°C (e.g., 245°C, 250°C, or 255°C), and the annealing time is 1.9-2.1h (e.g., 1.9h, 2.0h, or 2.1h). Among them, too low a temperature will lead to insufficient crystallinity; it can be seen from the phase diagram of CdSe that too high a temperature will change the crystal phase and cause CdSe to volatilize, seriously reducing the performance of CdSe. If the time is too short, the crystallinity is insufficient, and if it is too long, the cost will increase.

[0041] In a preferred embodiment of the present invention, the self-assembled HCPDI is prepared according to a method comprising the following steps: B1. 3,4,9,10-perylenetetracarboxylic acid diimide is mixed with concentrated sulfuric acid, and after ultrasonication, a red mixed solution is obtained; B2. The red mixed solution obtained by the treatment of step B1 is mixed evenly with an ethylene glycol aqueous solution, and after standing, a purple-red suspension is obtained; B3. The purple-red suspension is centrifuged and washed to obtain the self-assembled HCPDI. Among them, the ethylene glycol molecules in the ethylene glycol aqueous solution can play a role in connecting and assembling 3,4,9,10-perylenetetracarboxylic acid diimide molecules, and it can form hydrogen bonds with 3,4,9,10-perylenetetracarboxylic acid diimide molecules, so that the 3,4,9,10-perylenetetracarboxylic acid diimide molecules can be assembled into an ordered polymer.

[0042] In a preferred embodiment of the present invention, in step B1, the mass volume ratio of 3,4,9,10-perylenetetracarboxylic acid diimide to concentrated sulfuric acid is 1:(195-205) (for example, 1:195, 1:200 or 1:205; wherein the mass of 3,4,9,10-perylenetetracarboxylic acid diimide is in g, and the volume of concentrated sulfuric acid is in mL); in step B2, the volume ratio of concentrated sulfuric acid to ethylene glycol aqueous solution is 1:(9.9-10.1) (for example, 1:9.9, 1:10 or 1:10.1), and the standing time is 44-46 min (for example, 44 min, 45 min or 46 min). wherein the mass of 3,4,9,10-perylenetetracarboxylic acid diimide is in g, and the volume of concentrated sulfuric acid (95%) is in mL. Among them, in the dosage ratio of 3,4,9,10-perylenetetracarboxylic acid diimide, concentrated sulfuric acid and ethylene glycol aqueous solution, if the ratio of 3,4,9,10-perylenetetracarboxylic acid diimide is too small, the concentrated sulfuric acid raw material will be wasted; if the ratio of 3,4,9,10-perylenetetracarboxylic acid diimide is too large, it will not be completely dissolved; if the ratio of concentrated sulfuric acid is too small, the ethylene glycol solution will be wasted; if the ratio of concentrated sulfuric acid is too large, the solution will boil and the self-assembly will not be complete. If the standing time is too long, there will be no obvious change, and if the standing time is too short, it will lead to incomplete self-assembly.

[0043] The present invention further provides a HCPDI-CdSe NPs film. The HCPDI-CdSe NPs film in the embodiment of the present invention is prepared by the method as described above.

[0044] The HCPDI-CdSe NPs film of the present invention uses self-assembled HCPDI as a substrate, CdSe NPs are uniformly distributed on the self-assembled HCPDI, the structure of the HCPDI is conducive to the adsorption of water molecules and the dissociation of O2; the dispersed CdSe NPs are conducive to enhancing light absorption, improving the utilization rate of sunlight, and generating more photogenerated electron-hole pairs; a small amount of CdO is contained in the CdSe NPs, which can not only better combine CdSe with HCPDI, but also better adsorb water molecules, thereby improving the photocatalytic reaction rate.

[0045] The present invention also proposes the application of the HCPDI-CdSe NPs film as described above. The application of the embodiment of the present invention is: application of the HCPDI-CdSe NPs film in photocatalytic water splitting; wherein the products of the photocatalytic water splitting are hydrogen and oxygen.

[0046] The HCPDI-CdSe NPs film and its preparation method and application of the present invention are described in detail below through specific embodiments.

[0047] The raw materials used in the following examples are shown in Table 1:

[0048] Table 1

[0049]

[0050]

[0051] Example 1

[0052] The preparation method of the HCPDI-CdSe NPs film of this embodiment comprises the following steps:

[0053] (1) Preparation of CdSe nanoparticles, comprising the following steps:

[0054] A1. Weigh 0.5237 g of sodium sulfite, 0.5993 g of selenium powder and 0.6052 g of granular sodium hydroxide, pour it into a mortar and grind it for 20 min to obtain a first mixture;

[0055] A2. Weigh 5.9978 g of cadmium acetate dihydrate and pour it into the mortar containing the first mixture and continue grinding for 30 min to obtain a blocky brown substance (second mixture);

[0056] A3. Transfer the second mixture to a 100mL beaker, add 80mL of deionized water, stir evenly, pour into three 50mL centrifuge tubes, and centrifuge at 10,000 rpm for 5 minutes. Then pour out the supernatant, add 30mL of deionized water and centrifuge three times. Use the same method to centrifuge three times with anhydrous ethanol to obtain a CdSe paste.

[0057] A4. The CdSe paste was transferred to a tube furnace, dried at 90°C for 10 h under an argon atmosphere, and then taken out and ground into powder to obtain a CdSe powder.

[0058] A5. Anneal the CdSe powder at 250°C for 2 h in an argon atmosphere.

[0059] (2) Preparing a self-assembled HCPDI, comprising the following steps:

[0060] B1. Weigh 0.1 g of 3,4,9,10-perylenetetracarboxylic acid diimide and place it in a 50 mL beaker. Use a 25 mL measuring cylinder to measure 20 mL of concentrated sulfuric acid (95%) and pour it into the beaker containing HCPDI. Stir ultrasonically for 30 min to obtain a red mixed solution.

[0061] B2. Use a 100mL measuring cylinder to measure 50mL of ethylene glycol and 150mL of deionized water, respectively, and pour them into a 500mL beaker to prepare 200mL of ethylene glycol aqueous solution (25vol%). Pour the red mixed solution after ultrasonic stirring into 200mL of ethylene glycol aqueous solution (25vol%), stir with a glass rod for 15min, seal with plastic wrap and let stand for 45min to obtain a purple-red suspension;

[0062] B3. Pour the purple-red suspension into 6 50 mL centrifuge tubes for centrifugation. Then add 35 mL of deionized water to each centrifuge tube and centrifuge five times. Centrifuge once with anhydrous ethanol in the same way to obtain a purple paste-like self-assembled HCPDI.

[0063] (3) Preparation of a mixture of HCPDI and CdSe NPs: Weigh 0.1 g of CdSe NPs obtained in step (1) and place it into 0.1 g of self-assembled HCPDI obtained in step (2). Use a pipette to add 2 mL of n-hexane and 2 mL of anhydrous ethanol to the mixture of HCPDI and CdSe NPs. Stir the mixture with a glass rod for 10 min to mix it evenly, thereby obtaining a mixture of HCPDI and CdSe NPs.

[0064] (4) Preparation of HCPDI-CdSe NPs film: The mixture obtained in step (3) was evenly applied on a 10 mm × 20 mm × 1 mm glass slide. When the mixture on the glass slide turned golden yellow, Figure 1 The furnace tube in the high-temperature tube furnace shown in the figure was wiped with deionized water, then wiped with anhydrous ethanol and dried to ensure the cleanliness of the tube; the glass slide carrying the sample was gently placed flat on a 50mm×20mm×20mm quartz boat, and then gently pushed into the middle of the furnace tube. After sealing the flange, the furnace tube was vacuum-cleaned with argon gas three times, each time to 2×10 -2 Torr, and then argon was introduced to the atmospheric pressure of 6.9×10 -2 Torr, exhaust the air in the tube, put it into a high-temperature tube furnace and anneal it at 250°C for 2h, control the argon flow rate to 20mL / min, and the heating rate to 4°C / min. After cooling naturally to room temperature, take out the quartz boat to obtain the HCPDI-CdSe NPs film of this embodiment (as shown in the actual picture) Figure 6 shown).

[0065] (5) Product storage: The prepared HCPDI-CdSe NPs film was stored in a sealed sample bag to prevent moisture, acid, alkali and salt corrosion, and light. The storage temperature was 20°C and the relative humidity was 10%.

[0066] in, Figure 1The state diagram of the HCPDI-CdSe NPs film generated by tube furnace annealing in the embodiment of the present invention, the position and connection relationship of each component must be correct and the operation must be carried out in sequence. In step (1), the drying and annealing of the CdSe paste material are carried out in a high-temperature tube furnace, and are completed in an argon atmosphere and heated state.

[0067] The morphology and structure of the HCPDI-CdSe NPs film prepared in this example were analyzed: Figure 2 is the microscopic morphology of HCPDI-CdSe NPs film; Figure 2 It can be clearly seen that CdSe nanoparticles are uniformly dispersed on HCPDI. This structure has a strong ability to separate photogenerated charges, which can increase the light absorption range during complete water splitting and promote charge transfer.

[0068] Example 2

[0069] The difference between this embodiment and embodiment 1 is that in step (1), the amount of sodium sulfite is 0.5356 g, the amount of selenium powder is 0.6075 g, the amount of granular sodium hydroxide is 0.6189 g, and the amount of cadmium acetate dihydrate is 2.0723 g.

[0070] Example 3

[0071] The difference between this embodiment and embodiment 1 is that in step (1), the amount of sodium sulfite is 0.5237 g, the amount of selenium powder is 0.5976 g, the amount of granular sodium hydroxide is 0.6051 g, and the amount of cadmium acetate dihydrate is 10.0798 g.

[0072] Comparative Example 1

[0073] The difference between this comparative example and Example 1 is that in step (1), after CdSe is dried at 90° C. for 10 h, the temperature is directly raised to 250° C. for annealing for 2 h, and the annealed CdSe is taken out and ground into powder; the rest is consistent with Example 1.

[0074] Comparative Example 2

[0075] The difference between this comparative example and Example 1 is that in step (1), the step of annealing the CdSe powder at 250° C. for 2 h in an argon atmosphere is omitted; the rest is consistent with Example 1.

[0076] Comparative Example 3

[0077] The difference between this comparative example and Example 2 is that in step (1), after CdSe is dried at 90°C for 10 hours, the temperature is directly raised to 250°C for annealing for 2 hours, and the annealed CdSe is taken out and ground into powder; the rest is consistent with Example 2.

[0078] Comparative Example 4

[0079] The difference between this comparative example and Example 2 is that in step (1), the step of annealing the CdSe powder at 250° C. for 2 h in an argon atmosphere is omitted; the rest is consistent with Example 2.

[0080] Comparative Example 5

[0081] The difference between this comparative example and Example 3 is that in step (1), after CdSe is dried at 90°C for 10 hours, the temperature is directly raised to 250°C for annealing for 2 hours, and the annealed CdSe is taken out and ground into powder; the rest is consistent with Example 3.

[0082] Comparative Example 6

[0083] The difference between this comparative example and Example 3 is that in step (1), the step of annealing the CdSe powder at 250° C. for 2 h in an argon atmosphere is omitted; the rest is consistent with Example 3.

[0084] Experimental example

[0085] The HCPDI-CdSe NPs film prepared above was used for photocatalytic water splitting to produce hydrogen and oxygen. The specific process is as follows:

[0086] (1) Use a 100 mL graduated cylinder to measure 75 mL of deionized water. Figure 3 Pour it on top of the photocatalytic quartz reactor, use tweezers to put the stage into the bottom of the reactor, and then use tweezers to place the annealed sample on top of the stage. Put on the rubber ring and quartz cover, and clamp it with a fixing clamp to make the reactor in a sealed state.

[0087] (2) Argon was introduced into the air inlet at a flow rate of 1 mL / min for 30 min to exhaust all the air in the reactor. The exhaust port was then closed first, and then the air vent was closed to seal the reactor.

[0088] (3) Place the top of the photocatalytic quartz reactor directly under the xenon lamp, turn on the xenon lamp so that the light can shine on the sample, and continue to illuminate for 4 hours to perform a complete water splitting reaction. The reaction process is as follows: Figure 4 shown.

[0089] (4) 5 mL of gas in the photocatalytic quartz reactor after the reaction was extracted using a syringe, and the hydrogen production rate and oxygen production rate were measured using a chromatograph.

[0090] The experimental results are as follows Figure 5 As shown in Table 1 below:

[0091] Table 1

[0092]

[0093] In summary:

[0094] The HCPDI-CdSe NPs film prepared by the present invention can photocatalytically split water without the presence of a sacrificial agent, and the hydrogen and oxygen production rates are both high;

[0095] The HCPDI-CdSe NPs films prepared in Comparative Examples 1, 3, and 5 were tested for the gases after the reaction under photocatalysis, and no product was formed, which did not meet the use standard. The reason is that the oxygen atoms were not introduced, so that no stable connection was formed between HCPDI and cadmium selenide, which hindered the separation and transmission of photogenerated carriers at the heterojunction interface, and therefore did not have the ability to fully decompose water.

[0096] The performance of Comparative Examples 2, 4, and 6 is significantly lower than that of Examples 1, 2, and 3. The reason is that the unannealed cadmium selenide nanoparticles do not have good crystallinity, which is not conducive to the transmission of photogenerated carriers and has a serious recombination phenomenon, so the photocatalytic water splitting performance is not very good.

[0097] Comparing Examples 1, 2 and 3, Example 1 achieves the highest performance because the change in the raw material ratio causes the valence band position to shift, so that Example 1 can form a stronger built-in electric field than Examples 2 and 3, which is more conducive to the separation and transmission of photogenerated carriers and has better overall water splitting performance.

[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing HCPDI-CdSe NPs thin film, It is characterized in that The following steps are involved: (1) mixing CdSe nanoparticles, self-assembled HCPDI and solvent uniformly to obtain a mixture I; (2) applying the mixture I obtained by the treatment in step (1) on the surface of a glass slide, drying it, and then annealing it in a rare gas atmosphere to obtain the HCPDI-CdSe NPs film; The CdSe nanoparticles are prepared by a method comprising the following steps: A1. The sodium sulfite, selenium powder and sodium hydroxide are mixed and ground to obtain a first mixture; the molar ratio of the sodium sulfite, selenium powder and sodium hydroxide is 1: (1.81-1.83): (3.63-3.65); A2. The first mixture and cadmium acetate were mixed and ground to obtain a second brown block mixture; the molar ratio of cadmium acetate to selenium powder was (0.9-5.1): 1; A3. Washing the second mixture to obtain a CdSe paste; A4. The CdSe paste is dried and ground to obtain a CdSe powdery substance; A5. Annealing the CdSe powder to obtain the CdSe nanoparticles; in step A5, the annealing temperature is 245-255 ° C, and the annealing time is 1.9-2.1 h In step (1), the mass ratio of the CdSe nanoparticles to HCPDI is (0.9-1.1):1; In step (2), the annealing temperature is 240-260°C, and the annealing time is 1.9-2.1 h.

2. The method for preparing the HCPDI-CdSe NPs film according to claim 1, It is characterized in that The self-assembled HCPDI is obtained by self-assembly of 3,4,9,10-perylenetetracarboxylic acid diimide under acidic conditions.

3. The method for preparing the HCPDI-CdSe NPs film according to claim 1, It is characterized in that In step A3, the second mixture is washed with water and then with alcohol; In step A4, the drying is performed in a rare gas atmosphere, the drying temperature is 85-95° C., and the drying time is 9.9-10.1 h.

4. The method for preparing the HCPDI-CdSe NPs film according to claim 1, It is characterized in that The self-assembled HCPDI is prepared according to a method comprising the following steps: B1. Mix 3,4,9,10-perylenetetracarboxylic acid diimide with concentrated sulfuric acid and, after ultrasonication, obtain a red mixed solution; B2. The red mixed solution obtained by step B1 was mixed evenly with an aqueous solution of ethylene glycol and allowed to stand to obtain a purple-red suspension; B3. Centrifuge and wash the purple-red suspension to obtain the self-assembled HCPDI.

5. The method for preparing the HCPDI-CdSe NPs film according to claim 4, It is characterized in that In step B1, the mass volume ratio of 3,4,9,10-perylenetetracarboxylic acid diimide to concentrated sulfuric acid is 1:(195-205); wherein the mass of 3,4,9,10-perylenetetracarboxylic acid diimide is measured in g, and the volume of concentrated sulfuric acid is measured in mL; In step B2, the volume ratio of the concentrated sulfuric acid to the ethylene glycol aqueous solution is 1:(9.9-10.1), and the standing time is 44-46 min.

6. A HCPDI-CdSe NPs film, It is characterized in that The HCPDI-CdSe NPs film is prepared by the method according to any one of claims 1 to 5.

7. Use of the HCPDI-CdSe NPs film as claimed in claim 6 in photocatalytic water splitting.