A kind of polyamide resin and its polymerization method and application
By using monomer polymerized polyamide resins such as 1,4-cyclohexanedicarboxylic acid, 1,10-decyldiamine and 1,12-dodecyldiamine, the trans structure ratio is controlled, and the traditional materials are solved at high temperatures. The problem of loss of transparency after SMT packaging achieves high light transmittance and stability of polyamide resin in the field of translucent LEDs.
Patent Information
- Application Number
- CN202310479493.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-28
AI Technical Summary
It is difficult for existing materials to maintain the transparency of translucent LED lamp beads after high temperature and SMT packaging. Traditional PPA materials lose their transparency characteristics in recrystallization and cannot meet the needs of the translucent LED field.
Polyamide resins polymerized from monomers such as 1,4-cyclohexanedicarboxylic acid, 1,10-decyldiamine and 1,12-dodecyldiamine were developed by controlling the trans structure ratio and polymerization conditions. A polyamide resin that is resistant to high temperature, has high initial light transmittance and does not recrystallize.
The polyamide resin has achieved a high light transmittance after SMT treatment, meeting the needs of the translucent LED field, and destroying the molecular chain regularity by controlling the trans structure ratio, ensuring the stability and transparency of the material.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, in particular to a polyamide resin and a polymerization method and application thereof. Background Art
[0002] Compared with the semi-aromatic heat-resistant polyamide polymerized from terephthalic acid or isophthalic acid, the heat-resistant polyamide polymerized from 1,4-cyclohexanedicarboxylic acid monomer does not contain benzene rings in its molecular structure and has a weaker electron-withdrawing effect. Therefore, the heat-resistant polyamide polymerized from 1,4-cyclohexanedicarboxylic acid monomer is less likely to obtain electrons when subjected to long-term ultraviolet aging, and its molecular structure is more stable, and its resistance to ultraviolet aging is better.
[0003] As people's living standards improve, the demand for LED lamp beads increases, and translucent LED lamp beads are gradually derived. They can be used in high-end fields such as outdoor transparent display screens, shopping malls, and counter display screens, and have high added value. This type of product not only requires the material to have high temperature resistance, but also has good light transmittance after SMT (infrared reflow soldering) packaging. However, traditional PPA materials are difficult to make transparent; even if the resin is transparent in the initial state through structural adjustment, recrystallization will occur during subsequent SMT packaging, the molecular chain will be rearranged, the regularity of the molecular chain will increase, the crystallinity will increase, and the transparent property will be lost, which is similar to the situation of PCT materials. At present, there is no suitable material on the market to meet the needs of the translucent LED field.
[0004] Therefore, it is necessary to develop a polyamide resin matrix with high temperature resistance and still maintain high transparency after SMT to meet the needs of the translucent LED field. Summary of the invention
[0005] The object of the present invention is to provide a polyamide resin which is resistant to high temperatures, has high initial light transmittance, and will not undergo recrystallization after SMT treatment, as well as a polymerization method and application thereof.
[0006] The present invention is achieved through the following technical solutions:
[0007] A polyamide resin, characterized in that, measured by mole percentage, it comprises the following repeating units:
[0008] Diacid unit: 1,4-cyclohexanedicarboxylic acid;
[0009] Diamine units: 1,10-decanediamine and 1,12-dodecanediamine, wherein the molar fraction of 1,10-decanediamine in the diamines is 76-82%.
[0010] Preferably, the amount of 1,10-decanediamine in the diamine is 78-80%.
[0011] In the polyamide resin, the trans structure accounts for 81-85% of the amount of the polyamide resin. The test method is: take 5 mg of polyamide resin, dissolve it in 10 mg of deuterated trifluoroacetic acid, and use Bruker's DPX400 nuclear magnetic resonance instrument to perform nuclear magnetic hydrogen spectrum test on the sample. In the nuclear magnetic hydrogen spectrum, the cis structure peaks at 1.96 ppm and the trans structure peaks at 1.83 ppm. The two peaks are integrated by nuclear magnetic field to obtain the trans structure ratio of the resin.
[0012] The melting point range of the polyamide resin is 321-334°C. Referring to ASTM D3418-2003, Standard Test Method for Transition Temperatures of Polymers By Differential Scanning Calorimetry; the specific test method is: using a Perkin Elmer Dimond DSC analyzer to test the melting point of the sample; nitrogen atmosphere, flow rate of 50mL / min; during the test, first heating to 350°C at 20°C / min, maintaining at 350°C for 2min, removing the thermal history of the resin, then cooling to 50°C at 20°C / min, maintaining at 50°C for 2min, and then heating to 350°C at 20°C / min, and setting the endothermic peak temperature at this time as the T melting point.
[0013] The relative viscosity of the polyamide resin is in the range of 1.8-2.8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
[0014] The polymerization method of the polyamide resin of the present invention comprises the following steps: adding reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave; the amount of benzoic acid substance is 1.5-3.0% of the amount of reaction monomer substance, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other feed materials except deionized water, and the weight of deionized water is 25-35% of the total feed weight; vacuuming and filling inert gas (which may be high-purity nitrogen) as protective gas, heating to 215-225° C. within 1.5-2.5 hours, and then reacting at the temperature range for 0.5-1.5 hours; then continuing to react at 225-235° C. and 2.0-2.4 MPa pressure for 1-3 hours, removing the water formed during the reaction process, discharging after the reaction is completed, and vacuum drying the prepolymer to obtain a prepolymer product, and solid phase viscosity enhancement of the prepolymer product for 8-12 hours under the conditions of 240-260° C. and 45-55 Pa pressure to obtain a polyamide resin.
[0015] The polyamide resin of the present invention is used for preparing translucent LED related parts, such as LED lamp bracket.
[0016] The present invention has the following beneficial effects
[0017] Through experiments, it was found that the cis / trans structure of the polyamide resin is derived from 1,4-cyclohexanedicarboxylic acid. 1,4-cyclohexanedicarboxylic acid constitutes the diacid unit of the polyamide resin of the present invention. By controlling the molar content of each unit in the polyamide, it was unexpectedly found that a specific trans structure ratio can be obtained (research has found that the trans structure ratio of the polyamide resin in which 1,4-cyclohexanedicarboxylic acid constitutes the diacid unit is related to the structure and ratio of the diamine monomer. The possible reason is that the longer the molecular chain of the diamine monomer, the higher the stability of the trans structure, and therefore the higher the ratio of the trans structure), which destroys the regularity of the molecular chain. It not only has a high initial transmittance, but also will not undergo recrystallization after SMT treatment, and can still maintain a high transmittance. Implementation
[0018] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0019] 1,4-Cyclohexanedicarboxylic acid: purity 98%, SKY CHDA, purchased from SK Chemicals;
[0020] 1,10-Decanediamine: purity 97%, D100615, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0021] 1,12-Dodecanediamine: purity 98%, D106441, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0022] 1,6-Hexanediamine: purity 99%, H103910, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0023] 1,14-Tetradecanediamine: purity 95%, SY250668, purchased from Shanghai Shaoyuan Reagent Co., Ltd.;
[0024] Benzoic acid: purity 99.5%, 242381, purchased from Sigma-Aldrich;
[0025] Sodium hypophosphite: purity 98%, S475696, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0026] The preparation method of polyamide resin of the embodiment and comparative example is as follows: adding reaction monomer, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave; the amount of benzoic acid substance is 1.5% of the amount of reaction monomer substance, the weight of sodium hypophosphite is 0.10% of the weight of other feed materials except deionized water, and the weight of deionized water is 30% of the total feed weight; vacuumizing and filling with high-purity nitrogen as a protective gas, heating to 220° C. within about 2 hours, and then reacting at this temperature range for 1 hour; then continuing to react at 230° C. and a pressure of 2.2 MPa for 2 hours, removing the water formed during the reaction, discharging the material after the reaction is completed, and obtaining a prepolymer product after vacuum drying the prepolymer, and the prepolymer product is solid-phase thickened for 8-12 hours under the conditions of 250° C. and a pressure of 50 Pa to obtain a polyamide resin.
[0027] Various test methods:
[0028] (1) Polyamide relative viscosity test method: refer to GB12006.1-89, polyamide viscosity determination method; the specific test method is: measure the relative viscosity of polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01℃.
[0029] (2) Polyamide resin melting point test method: refer to ASTM D3418-2003, Standard Test Method for Transition Temperatures of Polymers By Differential Scanning Calorimetry; the specific test method is: use Perkin Elmer Dimond DSC analyzer to test the melting point of the sample; nitrogen atmosphere, flow rate is 50mL / min; during the test, first increase the temperature to 350℃ at 20℃ / min, keep at 350℃ for 2min to remove the thermal history of the resin, then cool to 50℃ at 20℃ / min, keep at 50℃ for 2min, and then increase the temperature to 350℃ at 20℃ / min, and set the endothermic peak temperature at this time as T melting point.
[0030] (3) Test method for the cis-trans ratio of polyamide: Take 5 mg of polyamide resin, dissolve it in 10 mg of deuterated trifluoroacetic acid, and use Bruker's DPX400 nuclear magnetic resonance instrument to perform nuclear magnetic resonance hydrogen spectrum test on the sample. In the nuclear magnetic hydrogen spectrum, the cis structure peak is at 1.96 ppm, and the trans structure peak is at 1.83 ppm. Perform nuclear magnetic integration of the two peaks to obtain the trans structure ratio of the resin.
[0031] (4) SMT test: The polyamide composition was injection molded into a 60 mm*60 mm*0.8 mm thin plate, and the thin plate was placed in the SMT instrument for testing. Infrared reflow soldering conditions: The SMT infrared reflow soldering device was set up with the following conditions:
[0032] a Preheating stage: raise the temperature from room temperature to 150°C within 120 seconds;
[0033] b Heating stage: raising the temperature from 150°C to 190°C within 90 seconds;
[0034] c Reflow stage: Raise the temperature to 217°C at a heating rate of 2.5°C per second, then raise the temperature from 217°C to 260°C and then lower it to 217°C within 80 seconds;
[0035] d Cooling stage: lower the temperature to room temperature at a cooling rate of more than 2°C per second.
[0036] (5) Polyamide transmittance test method: Referring to ISO13468-1-2019, the polyamide resin is injection molded into a 2 mm thick smooth panel, and the initial and post-SMT transmittance tests of the material are performed using a spectrophotometer.
[0037] Table 1: Amount fraction and test results of each unit substance of polyamide resin in Examples and Comparative Examples 1-2
[0038] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 1,4-Cyclohexanedicarboxylic acid 50 50 50 50 50 50 50 1,10-Decanediamine 38 39 39.5 40 41 37 42 1,12-Dodecanediamine 12 11 10.5 10 9 13 8 Relative viscosity 2.237 2.264 2.208 2.246 2.249 2.210 2.224 Trans structure ratio, mol% 81.3 82.4 82.9 83.7 84.9 80.3 85.5 Melting point, °C 321 325 327 329 334 316 341 Initial transmittance, % 72 74 76 77 73 68 66 Transmittance after SMT, % 71 72 73 75 71 57 55
[0039] It can be seen from Examples 1-5 that when 1,10-decanediamine accounts for 78-80% of the molar fraction of the diamine substance, the molar fraction of the trans structure in the polyamide resin is 82-84%, and both the initial transmittance and the transmittance after SMT are relatively high.
[0040] It can be seen from Comparative Example 1 that when the molar fraction of 1,10-decanediamine in the diamine substance is less than 78%, the molar fraction of the trans structure in the polyamide resin is less than 81%, the resin molecular chain has relatively good regularity, and the initial transmittance is reduced; and after SMT, the molecular chain has good regularity and is easy to recrystallize again, resulting in a significant decrease in transmittance.
[0041] It can be seen from Comparative Example 2 that in Comparative Example 2, the melting point of the resin is higher than 340° C., and the injection molding temperature is close to the resin decomposition temperature, which makes it difficult to perform injection molding, resulting in low initial light transmittance and light transmittance after SMT.
[0042] Table 2: Molecular fraction content and test results of each unit substance of polyamide resin in comparative examples 3-5
[0043] Comparative Example 3 Comparative Example 4 Comparative Example 5 1,4-Cyclohexanedicarboxylic acid 50 50 50 1,10-Decanediamine 40 40 50 1,6-Hexanediamine 10 1,14-Tetradecanediamine 10 Relative viscosity 2.289 2.266 2.204 Trans structure ratio, mol% 87.5 79.2 76.2 Melting point, °C 338 322 351 Initial transmittance, % 62 65 60 Transmittance after SMT, % 49 53 46
[0044] It can be seen from Comparative Examples 3-5 that it is difficult for other types of monomers to achieve a trans-structure ratio within the scope of the present invention, achieve high light transmittance, and ensure light transmittance after SMT.
[0045] The initial light transmittance of the polyamide resin of the present application is ≥72%, and the light transmittance after SMT is ≥71%.
Claims
1. A polyamide resin, characterized in that In terms of mole percentage, it comprises the following repeating units: Diacid unit: 1,4-cyclohexanedicarboxylic acid; Diamine units: 1,10-decanediamine and 1,12-dodecanediamine, wherein the molar fraction of 1,10-decanediamine in the diamines is 76-79%; In the polyamide resin, the trans structure accounts for 81.3-82.9% of the molar fraction of the polyamide resin.
2. The polyamide resin according to claim 1, characterized in that The melting point of the polyamide resin is in the range of 321-334°C.
3. The polyamide resin according to claim 1, characterized in that The relative viscosity of the polyamide resin is in the range of 1.8-2.
8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
4. The polymerization method of the polyamide resin according to any one of claims 1 to 3, characterized in that: The following steps are involved: Add reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave; the amount of benzoic acid is 1.5-3.0% of the total amount of reaction monomers, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other materials except deionized water, and the weight of deionized water is 25-35% of the total weight of materials; evacuate and fill with inert gas as protective gas, raise the temperature to 215-225° C. within 1.5-2.5 hours, and then react at this temperature range for 0.5-1.5 hours; then continue to react at 225-235° C. and 2.0-2.4 MPa for 1-3 hours, remove the water formed during the reaction, discharge the material after the reaction is completed, and obtain a prepolymer product after vacuum drying the prepolymer, and solid phase thicken the prepolymer product for 8-12 hours under the conditions of 240-260° C. and 45-55 Pa pressure to obtain a polyamide resin.
5. The use of the polyamide resin according to any one of claims 1 to 3, characterized in that: Used to prepare translucent LED related components.
6. Application of the polyamide resin obtained by the preparation method of claim 4, characterized in that: Used to prepare translucent LED related components.