A method for preparing perovskite thin film and application of solar cell device
By generating 2D perovskite seeds in situ during the preparation process of perovskite films, the problems of multi-phase structure and synthesis difficulty in traditional methods are solved, and the photoelectric conversion efficiency of efficient perovskite solar cells is improved, reaching 25.17%. efficiency.
Patent Information
- Application Number
- CN202310505963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-06
AI Technical Summary
The traditional 2D perovskite seed crystal induction method results in the formation of a messy multi-phase 2D perovskite structure in perovskite solar cells, which hinders the improvement of 3D perovskite crystallization and photoelectric conversion efficiency. At the same time, the 2D perovskite seed crystal The synthesis is difficult, which limits its large-scale application.
During the preparation process of the perovskite film, organic ligand materials are spin-coated on the surface of the lead iodide film and annealed to generate 2D perovskite seeds in situ, avoiding the formation of multi-phase structures and directly inducing perovskite. The crystallization of the light-absorbing layer improves the film quality and photoelectric conversion efficiency.
The formation of a high-quality, high-crystallinity perovskite light-absorbing layer has been achieved, improving the photoelectric conversion efficiency of perovskite solar cells to 25.17%, which is much higher than traditional methods. It is suitable for different types of organic ligands and has good performance. of universality.
Smart Images

Figure CN116600615B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of perovskite photovoltaic technology, and particularly proposes a method for in-situ generation of two-dimensional perovskite seeds and induction of three-dimensional perovskite crystallization; a method for preparing a perovskite film and an application of solar cell devices are proposed. Background Art
[0002] As a third-generation new solar cell technology, perovskite solar cells are widely studied because of their low cost, simple preparation process and high photoelectric conversion efficiency (PCE). At present, in the field of perovskite solar cells, the main ways to improve the photoelectric conversion efficiency of the battery include seed induction, interface passivation, optimization of carrier transport layer and other means. Among them, seed induction is a key means to improve the quality and PCE of perovskite films. At present, the mainstream seed additives mainly include inorganic substances (for example, KCl, KI, RbCl, etc.), two-dimensional (2D) organic ligand materials (for example, phenylethylamine iodide, thiophenemethylamine iodide, etc.), other organic compounds and polymer additives. Among them, organic ligand materials as additives can form a 2D phase perovskite structure at the 3D perovskite grain boundary. This 2D structure acts as a seed to induce 3D perovskite crystallization to form a 2D / 3D hybrid structure. In the field of 2D / 3D hybrid perovskites, the traditional strategy is to directly add organic ligand materials or 2D perovskite seeds into the perovskite precursor solution to prepare 2D / 3D hybrid perovskite films. This method can form 2D perovskite seeds in the 3D perovskite grain boundary or in the precursor solution, improving the quality of the perovskite film and device performance. The traditional two-step perovskite film preparation process of 2D seed-induced crystallization is as follows:
[0003] Step 1: Deposit or spin-coat an electron transport layer on the cleaned ITO or FTO conductive glass. Specifically, before preparing the electron transport layer on ITO or FTO, it needs to be cleaned, including cleaning the ITO or FTO conductive glass with detergent, deionized water, acetone and isopropanol for 15 minutes each. Treat the cleaned ITO or FTO conductive glass with UV-ozone, that is, ultraviolet-ozone treatment, and then spin-coat a layer of tin dioxide nanoparticle solution on the treated ITO or FTO, the thickness of which can be selected from 20-100nm, and anneal it, the annealing temperature can be selected from 140-180℃, and the annealing time can be selected from 15-30 minutes; the solvent of the tin dioxide nanoparticle solution is water.
[0004] Step 2: Spin-coat a layer of lead iodide solution on the electron transport layer, the lead iodide concentration can be 1.1mol / L-1.7mol / L, the solvent can be N,N-dimethylformamide and dimethyl sulfoxide, and anneal, the annealing temperature is 50-80°C, and the annealing time is 0.5 minutes to 5 minutes. The previously synthesized 2D perovskite seed or organic ligand material is added to the lead iodide solution.
[0005] Step 3: spin coating a mixed solution of formamidine iodide and methylamine chloride on the lead iodide film, wherein the concentration of formamidine iodide can be 60-120 mg / ml, the concentration of methylamine chloride can be 6-20 mg / ml, and the solvent can be isopropanol and ethanol; annealing the film at 100-180° C. for 10-30 minutes to obtain a seed-induced crystallized three-dimensional perovskite film;
[0006] Step 4: Spin coating a hole transport layer; the hole transport layer comprises spin coating a 2,2′,7,7′-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene (Spiro-oMeTAD) solution on the surface of the perovskite to obtain a hole transport layer, wherein the solvent in the Spiro-oMeTAD solution comprises chlorobenzene.
[0007] Step 5: Vacuum evaporation is used to deposit a layer of molybdenum trioxide and a metal electrode on the hole transport layer.
[0008] However, the quality of the 2D / 3D hybrid perovskite active layer prepared using this traditional strategy is still poor, and its photoelectric conversion efficiency (PCE) is still low. The photoelectric conversion efficiency of 2D / 3D hybrid perovskite solar cells (PSCs) reported in the literature does not exceed 25%. The main reason is that adding organic ligand materials or 2D perovskite seeds into the perovskite precursor solution can form a disordered multiphase 2D perovskite seed (n = 1, 2, 3, 4...), and this disordered multiphase structure is not conducive to the crystallization of 3D perovskite. At the same time, this disordered multiphase 2D perovskite seed formed in the precursor solution or during the crystallization process will eventually remain at the grain boundary of the 3D perovskite, further hindering the charge transfer of the perovskite light-absorbing layer. On the other hand, this method of adding 2D perovskite seeds into the 3D perovskite precursor solution is not conducive to the large-scale generation of perovskite solar cells, so this traditional solution is not suitable for industrialization. The main reason is that the synthesis of 2D perovskite seeds is difficult. In the laboratory, the synthesis of 2D perovskite seeds often requires high temperature heating and stirring at 120℃-150℃, and then slowly cooling at a cooling rate of 1℃ / hour to obtain 2D perovskite seeds. This method of synthesizing 2D perovskite seeds is very susceptible to interference from the external environment, such as the vibration of the sample stage, the room temperature of the laboratory and other factors. The most important thing is that this method is often only suitable for milligram-level synthesis. Once the sample volume is expanded, it is difficult to obtain high-quality 2D perovskite seeds. At the same time, for different types of 2D perovskite seeds, the difficulty of synthesis is also different. For most 2D perovskite seeds, researchers cannot even obtain them in the laboratory. Therefore, this traditional method of adding 2D perovskite seeds into 3D perovskite precursor solution greatly hinders the photoelectric conversion efficiency and performance of 2D / 3D hybrid PSCs, and also limits the scope of use of 2D perovskite seeds. Summary of the invention
[0009] In view of the above research background, this technology can form 2D perovskite seeds in situ during the two-step perovskite film preparation process to induce the crystallization of the perovskite film. This method of forming 2D seeds in situ without the need for additional seed synthesis steps expands the scope of use of 2D perovskite seeds.
[0010] The specific technical solutions are as follows:
[0011] The perovskite light-absorbing layer is the core part of the perovskite solar cell, and its quality determines the overall performance of the perovskite solar cell. For the perovskite light-absorbing layer, the degree of crystallinity and quality determine the overall quality of the layer. Adding 2D perovskite seeds or organic ligand materials to the perovskite precursor is a general method for adjusting the quality of the perovskite light-absorbing layer. However, if an organic ligand is added as a seed, the seed material may further react with MACl or FAI to form a disordered multiphase 2D perovskite (n≥1); if a pure phase 2D perovskite (whose n value is usually 1) is added as a seed, it is necessary to synthesize 2D perovskite seeds in advance, and the synthesis of 2D perovskite seeds is often difficult. In order to obtain a high-quality perovskite light-absorbing layer, the present invention invents a method for generating 2D perovskite seeds in situ without prior synthesis and inducing the crystallization of the perovskite light-absorbing layer. The invention overcomes the above defects at the same time, avoids the formation of disordered multiphase 2D perovskite at the 3D perovskite grain boundary, and improves the charge transfer of the active layer. At the same time, the invention can form 2D perovskite seeds in situ without the need to synthesize 2D perovskite seeds in advance. The invention can be simply stated as follows: in the process of preparing the perovskite light-absorbing layer by a two-step method, an organic ligand is spin-coated on the surface of the lead iodide film, and 2D perovskite seeds are generated in situ by annealing and further induce the crystallization of the perovskite light-absorbing layer to obtain a high-quality, high-crystallinity perovskite light-absorbing layer.
[0012] The technical solution of the present invention is as follows:
[0013] A method for preparing a perovskite film; an organic ligand is spin-coated on the surface of a lead iodide film, 2D perovskite seeds are generated in situ through annealing, and the crystallization of a perovskite light-absorbing layer is further induced to obtain a perovskite light-absorbing layer with high crystallinity.
[0014] The method for preparing a perovskite film comprises: spin coating a layer of lead iodide solution on an electron transport layer, and after annealing, spin coating a layer of organic ligand material on the surface of the lead iodide film to form a two-dimensional perovskite seed dispersed on the surface of the lead iodide film; spin coating a mixed solution of formamidine iodide salt and methylamine chloride salt on the lead iodide film, and performing annealing to obtain a three-dimensional perovskite film induced by seed crystallization.
[0015] The above-mentioned organic ligand materials include 2-thiophenemethylamine iodide ThMAI, 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide ThPyI, tetrahydroisoquinoline hydroiodide THIQI, and thiophenemethylamine iodide TTMAI, butylamine iodide BAI, phenylethylamine iodide PEAI, and the like.
[0016] Preferably, the organic ligand material 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide ThPyI is spin-coated to form (ThPy) in situ with lead iodide 2 PbI 4 Seed crystal.
[0017] The preferred spin-coated organic ligand material tetrahydroisoquinoline iodide salt THIQI forms (THIQ) in situ with lead iodide 2 PbI 4 Seed crystal.
[0018] The preferred spin coating organic ligand material phenylethylamine iodide PEAI is in situ formed with lead iodide (PEA) 2 PbI 4 Seed crystal.
[0019] Preferably, the organic ligand material 2-thiophenemethylamine iodide ThMAI is spin-coated to form (ThMA) in situ with lead iodide 2 PbI 4 .
[0020] Preferably, the organic ligand material butylamine iodide BAI is spin-coated to form (BA) with lead iodide. 2 PbI 4 .
[0021] Preferably, the organic ligand material is spin-coated and thiophenemethylamine iodide TTMAI is formed with lead iodide (TTMAI). 2 PbI 4 .
[0022] The chemical structure of the preferred spin-coated organic ligand material is as follows:
[0023]
[0024] The perovskite film preparation method of the present invention is used for the preparation method of solar cell devices, comprising the following steps:
[0025] Step 1) depositing or spin coating an electron transport layer on the cleaned ITO or FTO conductive glass; spin coating a layer of lead iodide solution on the surface of the tin dioxide film, and annealing;
[0026] Step 2) Spin-coat a layer of organic ligand material, such as phenylethylamine iodide, thiophene methylamine iodide, butylamine iodide, etc., on the surface of the lead iodide film in step 1, wherein the solvent may be isopropanol or ethanol, and the concentration may be 0.5mg / ml-10mg / ml; and anneal the film, the annealing temperature is 50-100°C, and the annealing time is 0 minutes-10 minutes; during the annealing process, the organic ligand material will interact with the lead iodide to form a layer of 2D perovskite seeds in situ dispersed on the surface of the lead iodide film. Among them, the n value of the 2D perovskite seeds is 1; and the 2D perovskite seeds are distributed on the surface of the lead iodide film in an island shape, rather than completely covering the surface of the lead iodide film. This distribution pattern will not hinder the penetration of the subsequent FAI / MACl solution, and will be conducive to the formation of the perovskite film.
[0027] Step 3: spin coating a mixed solution of formamidine iodide salt and methylamine chloride salt on the lead iodide film and annealing the mixed solution to obtain a seed-induced crystallized three-dimensional perovskite film;
[0028] Step 4: Spin-coat a hole transport layer on the surface of the perovskite film; and sequentially evaporate a layer of molybdenum trioxide and a metal electrode on the hole transport layer using a vacuum evaporation method.
[0029] The method for preparing a solar cell device is characterized in that a layer of organic ligand material is spin-coated on the surface of the lead iodide film and annealed to form two-dimensional perovskite seeds dispersed on the surface of the lead iodide film. The annealing temperature is 50-100°C, and the annealing time can be selected from 0-10 minutes. During the annealing process, the organic ligand material will interact with the lead iodide to form 2D perovskite seeds in situ, and the 2D perovskite seeds are distributed on the surface of the lead iodide film in an island shape, rather than completely covering the lead iodide film. This distribution pattern will not hinder the penetration of the FAI / MACl solution, and will be conducive to the formation of the perovskite film.
[0030] In the two-step process of preparing perovskite thin films, organic ligands or other organic, inorganic, polymer and other materials are spin-coated onto the surface of the lead iodide film. After annealing, 2D perovskite seeds or other types of seeds are formed in situ on the surface of the lead iodide film, and 3D perovskite crystals are induced to crystallize, thereby obtaining higher film quality. Figure 1 The X-ray diffraction pattern of can indicate the formation of 2D perovskite seeds. Figure 1 As shown in the figure, after a layer of organic ligand cations is spin-coated on the surface of lead iodide and annealed, a diffraction peak appears at 6.3°. Compared with the XRD diffraction peak of 2D perovskite (n=1), it can be found that the diffraction peak at 6.3° can be attributed to the peak of 2D perovskite formed in situ by the organic ligand material on the surface of the lead iodide film. In addition, as a comparison, the X-ray diffraction spectrum without spin-coating of 2D spacer cations does not have a peak of 2D perovskite at 6.3°. Figure 1 It is very clear that spin coating the organic ligand material on the surface of the lead iodide film can in situ generate 2D perovskite seeds, which will act as seeds in the subsequent perovskite growth process to induce perovskite crystallization. Figure 2 The X-ray diffraction patterns of 3D perovskite films with and without spin-coated organic ligand materials on the surface of the lead iodide film. Comparing the X-ray diffraction patterns of 3D perovskites with and without spin-coated organic ligand materials, it can be found that the diffraction peak of the perovskite film with spin-coated organic ligand materials at around 14.2° is significantly stronger than that of the perovskite film without spin-coated organic ligand materials. This shows that the 2D perovskite seeds generated in situ by spin-coating organic ligand materials on the surface of the lead iodide film can induce the crystallization of the 3D perovskite film and form a higher quality perovskite active layer. Figure 3 and Figure 4From the scanning electron microscopy (SEM) images, it can be observed that 2D seeds are generated on the surface of the lead iodide film after spin coating of the organic ligand. Figure 4 This is a lead iodide film spin-coated with organic ligand materials. The bright small particles circled are clearly different from other darker parts. We attribute this small round particle that is clearly different from other parts to the in-situ generated 2D perovskite seed. Figure 3 Lead iodide film without spin-coated organic ligand material. Figure 4 In sharp contrast, Figure 3 We did not find any similar 2D perovskite seeds in Figure 1 The conclusion is consistent with that of the study, that is, spin coating of organic ligand materials on the surface of lead iodide film can form 2D perovskite seeds in situ. After the lead iodide film and the organic ligand material are spin coated, the mixed solution of FAI and MACl is then spin coated, and the perovskite film is formed by annealing. The lead iodide spin coated with organic ligand material (i.e., the sample with organic ligand material spin coated on the lead iodide film) can still be observed after spin coating of FAI and MACl solution and annealing to form a perovskite film (such as Figure 2 This indicates that the originally generated 2D perovskite seeds were not destroyed during the spin coating of FAI and MACl solutions. Figure 5 The figure shows the efficiency comparison of devices with and without in-situ seeding to induce perovskite crystallization. It also compares the efficiency of devices using the traditional method to induce perovskite crystallization (adding organic ligand materials directly into the lead iodide solution instead of spin coating on the surface of the lead iodide film). Figure 5 It can be seen from the JV curve in the figure and the efficiency and corresponding parameters stated in the table that the perovskite solar cell prepared by this patent has a higher opening voltage and fill factor, as well as a higher photoelectric conversion efficiency, with an efficiency of up to 25.17%, which is much higher than the device prepared by the traditional seed induction method (23.97% efficiency). Moreover, the device efficiency (25.17%) obtained by this patent is currently the highest photoelectric conversion efficiency in this field (2D / 3D hybrid perovskite solar cell). On the other hand, compared with the device without seed induction, the efficiency of the solar cell device prepared by the technical solution in this patent is also higher than that of the device without any seed induction. Figure 6 This is a structural diagram of the device prepared in this patent. Fig.10 Figure 2 is the chemical structure diagram of the organic ligand material used.
[0031] Compared with the traditional method of 2D perovskite seed induced crystallization, the present invention can form 2D seed induced perovskite crystal in situ, without the need for additional synthesis steps, and the 2D seed formed by the present technology is a pure phase (n = 1 phase), does not contain other heterogeneous phase structures, and is more conducive to charge transfer and obtaining high-quality perovskite films. From the device aspect, the photoelectric conversion efficiency of the perovskite solar cell prepared using this technology is the highest efficiency currently based on 2D / 3D hybrid perovskite solar cells, much higher than the traditional method, and has good universality, can be applied to different organic ligands, and in situ form pure phase 2D perovskite seeds of different structures. As a result, the perovskite film prepared by the technical solution in this patent has a higher crystal quality, and the corresponding solar cell device can obtain a higher photoelectric conversion efficiency (25.17%), which is much higher than the photovoltaic efficiency obtained by the traditional method and seed-free induced crystallization. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 , XRD spectra of the lead iodide film with and without organic ligand cations spin-coated on the surface. Among them, the diffraction peak of the 2D perovskite phase appeared in the XRD spectrum of the lead iodide film after spin-coating the organic ligand cations, indicating that this technology can form 2D perovskite seeds in situ.
[0033] Figure 2 , XRD spectra of perovskite films with and without spin-coated organic ligand cations. Among them, the XRD spectrum of the perovskite film with spin-coated organic ligand cations on the surface of the lead iodide film still retains the diffraction peak of the 2D perovskite seed, indicating that the 2D perovskite seed formed in situ was not destroyed in the subsequent FAI solution spin coating step and annealing.
[0034] Figure 3 , SEM image of lead iodide film without 2D seeds. This image shows that there is no formation of 2D seeds in lead iodide.
[0035] Figure 4 , SEM image of the lead iodide film after spin coating with organic ligand cations. The brighter dots in the circle are 2D perovskite seeds formed in situ. The seeds are distributed in large quantities on the surface of the lead iodide film and can induce perovskite crystallization. The SEM corresponds to the XRD data.
[0036] Figure 5 , the photoelectric conversion efficiency diagram (JV curve diagram) of the traditional 2D seed induced and in-situ seed induced 2D / 3D perovskite solar cells prepared with 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide as an example. Among them, the in-situ seed induced 2D seed induced perovskite film showed significantly improved PCE and open circuit voltage (Voc).
[0037] Figure 6, device structure of the prepared 2D / 3D hybrid perovskite solar cell.
[0038] Figure 7 , the photoelectric conversion efficiency diagram (JV curve diagram) of the solar cell device prepared using phenylethylamine iodide as an example.
[0039] Figure 8 , the photoelectric conversion efficiency diagram (JV curve diagram) of the solar cell device prepared using thiophenemethylamine iodide as an example.
[0040] Fig. 9 , the photoelectric conversion efficiency diagram (JV curve diagram) of the solar cell device prepared using butylamine iodide as an example.
[0041] Fig.10 , the photoelectric conversion efficiency diagram (JV curve diagram) of the solar cell device prepared using tetrahydroisoquinoline iodide salt as an example.
[0042] Fig.11 , the photoelectric conversion efficiency diagram (JV curve diagram) of the solar cell device prepared using thiophenemethylamine iodide as an example. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0044] The perovskite film preparation method of the present invention is used for the preparation method of solar cell devices, comprising the following steps:
[0045] Step 1) depositing or spin coating an electron transport layer on the cleaned ITO or FTO conductive glass;
[0046] Step 2) Spin-coating a layer of lead iodide solution on the electron transport layer and annealing it;
[0047] Step 3) spin coating a layer of organic ligand material on the surface of the lead iodide film, and annealing the layer to form two-dimensional perovskite seeds or other types of seeds dispersed on the surface of the lead iodide film;
[0048] Step 4: Spin-coating a mixed solution of formamidine iodide salt and methylamine chloride salt on the surface of the lead iodide film; annealing the film at 100-180° C. to obtain a seed-induced crystallized three-dimensional perovskite film;
[0049] Step 5: Spin coating a hole transport layer to obtain a hole transport layer;
[0050] Step 6: Vacuum evaporation is used to deposit a layer of molybdenum trioxide and a metal electrode on the hole transport layer.
[0051] The step 1) deposits or spin-coats a layer of electron transport layer on the cleaned ITO or FTO conductive glass; specifically, before preparing the electron transport layer on the ITO or FTO, it needs to be cleaned, including cleaning the ITO or FTO conductive glass with detergent, deionized water, acetone and isopropyl alcohol for 15 minutes each. Treat the cleaned ITO or FTO conductive glass with UV-ozone (ultraviolet-ozone treatment), then spin-coat a layer of tin dioxide nanoparticle solution (thickness can be selected from 20-100nm) on the treated ITO or FTO, and anneal it (annealing temperature can be selected from 140-180°C, annealing time can be selected from 15-30 minutes); wherein the solvent of the tin dioxide nanoparticle solution is water;
[0052] In the step 2), a layer of lead iodide solution is spin-coated on the electron transport layer (the lead iodide concentration can be 1.1 mol / L-1.7 mol / L, and the solvent can be N,N-dimethylformamide and dichlorothionyl), and annealed (annealing temperature is 50-80° C., and annealing time is 0.5 min-5 min);
[0053] In the step 3), a layer of organic ligand material (such as phenylethylamine iodide, thiophenemethylamine iodide, butylamine iodide, etc., the solvent can be isopropanol and ethanol, and the concentration can be 0.5 mg / ml-10 mg / ml) is spin-coated on the surface of the lead iodide film, and annealed (annealing temperature is 50-100° C., annealing time is 0 min-10 min) to form two-dimensional perovskite seeds or other types of seeds dispersed on the surface of the lead iodide film;
[0054] The step 4: spin coating a mixed solution of formamidine iodide and methylamine chloride on the lead iodide film (wherein the concentration of formamidine iodide can be selected from 60-120 mg / ml, the concentration of methylamine chloride can be selected from 6-20 mg / ml, and the solvent can be selected from isopropanol and ethanol); annealing the film at 100-180° C. (annealing time can be selected from 10-30 minutes) to obtain a seed-induced crystallized three-dimensional perovskite film;
[0055] The step 5: spin coating a hole transport layer; the hole transport layer comprises spin coating a 2,2′,7,7′-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene (Spiro-oMeTAD) solution onto the surface of the passivation layer to obtain a hole transport layer, wherein the solvent in the Spiro-oMeTAD solution comprises chlorobenzene.
[0056] The step 6: using vacuum evaporation to deposit a layer of molybdenum trioxide and a metal electrode on the hole transport layer.
[0057] The present invention spin-coats a layer of lead iodide solution on the electron transport layer, and after annealing, spin-coats a layer of organic ligand material on the surface of the lead iodide film, and anneals, to form a two-dimensional perovskite seed dispersed on the surface of the lead iodide film; spin-coats a mixed solution of formamidine iodide salt and methylamine chloride salt on the lead iodide film, and anneals, to obtain a three-dimensional perovskite film induced by seed crystallization. Spin-coating the organic ligand on the surface of the lead iodide film, anneals, and generates 2D perovskite seed in situ, and further induces the crystallization of the perovskite light-absorbing layer, so as to obtain a perovskite light-absorbing layer with high crystallinity.
[0058] Preferably, 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide ThPyI is spin-coated on the surface of the lead iodide film to form (ThPy) in situ with the lead iodide. 2 PbI 4 Seed; Spin-coat phenylethylamine iodide salt PEAI on the surface of the lead iodide film to form (PEA) in situ with lead iodide 2 PbI 4 Seed; spin-coat thiophenemethylamine iodide salt ThMAI on the surface of the lead iodide film to form (ThMA) in situ with lead iodide 2 PbI 4 ; Spin-coat butylamine iodide salt BAI on the surface of lead iodide film to form (BA) with lead iodide 2 PbI 4 .
[0059] Embodiment 1:
[0060] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0061] 2. A layer of organic ligand material 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide is spin-coated on the surface of the lead iodide film in step 1, and annealed to form a 2D perovskite seed crystal, wherein the concentration of the 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide solution is 2 mg / ml, the solvent is isopropanol, the annealing temperature is 70° C., and the annealing time is 2 minutes.
[0062] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0063] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0064] The above is an implementation case of in-situ seed-induced crystallization using 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide as an organic ligand material. The conventional seed-induced crystallization scheme is: in step 3 above, 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide seeds are added to the lead iodide solution, and the solution is spin-coated on the electron transport layer. The comparison chart of the photovoltaic conversion efficiency of the device obtained in this implementation case 1 is Figure 5 , the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 23.97%, which is significantly lower than the 25.17% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has a higher crystal quality! The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
[0065] Embodiment 2:
[0066] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0067] 2. A layer of organic ligand material phenylethylamine iodide salt is spin-coated on the surface of the lead iodide film in step 1, and annealed to form 2D perovskite seeds, wherein the concentration of the phenylethylamine iodide salt solution is 5 mg / ml, the solvent is ethanol, the annealing temperature is 50° C., and the annealing time is 10 minutes.
[0068] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0069] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0070] The above is an implementation case of in-situ seed crystallization induced by using phenylethylamine iodide salt as the organic ligand material. The conventional seed crystallization scheme is: in step 3 above, phenylethylamine salt seed crystals are added into the lead iodide solution, and the solution is spin-coated on the electron transport layer. The comparison chart of the photovoltaic conversion efficiency of the device obtained in the implementation case 1 is Figure 7 , the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 23.07%, which is significantly lower than the 24.11% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has a higher crystal quality! The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
[0071] Embodiment 3:
[0072] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0073] 2. A layer of organic ligand material thiophenemethylamine iodide is spin-coated on the surface of the lead iodide film in step 1, and annealed to form 2D perovskite seeds, wherein the concentration of the thiophenemethylamine iodide solution is 10 mg / ml, the solvent is isopropanol, the annealing temperature is 100° C., and the annealing time is 0.5 min.
[0074] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0075] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0076] The above is an implementation case of in-situ seed-induced crystallization using thiophene methylamine iodide salt as a 2D organic coordination material. The conventional seed-induced crystallization scheme is: in step 3 above, thiophene methylamine salt seeds are added to the lead iodide solution, and the solution is spin-coated on the electron transport layer. The remaining steps are the same. The comparison chart of the photovoltaic conversion efficiency of the device obtained in the implementation case 2 is Figure 8, the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 23.05%, which is significantly lower than the 24.05% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has a higher crystal quality! . The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
[0077] Embodiment 4:
[0078] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0079] 2. A layer of organic ligand material butylamine iodide is spin-coated on the surface of the lead iodide film in step 1, and annealed to form 2D perovskite seeds, wherein the concentration of the butylamine iodide solution is 0.5 mg / ml, the solvent is isopropanol, the annealing temperature is 70° C., and the annealing time is 0 min.
[0080] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0081] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0082] The above is an implementation case of in-situ seed crystallization induced by using butylamine iodide as an organic ligand material. The conventional seed crystallization scheme is: in step 3 above, butylamine salt seeds are added into the lead iodide solution, and the solution is spin-coated on the electron transport layer. The remaining steps are the same. The comparison chart of the photovoltaic conversion efficiency of the device obtained in this implementation case 1 is Fig. 9 , the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 22.96%, which is significantly lower than the 24.01% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has higher quality! . The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
[0083] The technical solutions disclosed and proposed by the present invention can be realized by those skilled in the art by referring to the contents of this article and appropriately changing the conditions, routes and other links. Although the methods and preparation techniques of the present invention have been described through preferred embodiments, relevant technicians can obviously modify or re-combine the methods and technical routes described herein without departing from the content, spirit and scope of the present invention to realize the final preparation technology. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.
[0084] Embodiment 5:
[0085] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0086] 2. A layer of organic ligand material tetrahydroisoquinoline iodide is spin-coated on the surface of the lead iodide film in step 1, and annealed to form 2D perovskite seeds, wherein the concentration of the tetrahydroisoquinoline iodide solution is 6 mg / ml, the solvent is isopropanol, the annealing temperature is 70° C., and the annealing time is 1 minute.
[0087] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0088] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0089] The above is an implementation case of in-situ seed-induced crystallization using tetrahydroisoquinoline iodide salt as an organic ligand material. The conventional seed-induced crystallization scheme is: in step 3 above, tetrahydroisoquinoline iodide salt seeds are added into the lead iodide solution, and the solution is spin-coated on the electron transport layer. The comparison chart of the photovoltaic conversion efficiency of the device obtained in this implementation case is as follows: Fig.10 , the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 23.44%, which is significantly lower than the 25.05% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has a higher crystal quality! The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
[0090] Embodiment 6:
[0091] 1. Using the existing technical solution, a layer of tin dioxide nanoparticle solution is spin-coated on the cleaned ITO or FTO conductive glass; a layer of lead iodide film is spin-coated on the surface of the tin dioxide film, and then annealed.
[0092] 2. A layer of organic ligand material and thiophenemethylamine iodide salt is spin-coated on the surface of the lead iodide film in step 1, and annealed to form 2D perovskite seeds, wherein the concentration of the thiophenemethylamine iodide salt solution is 5 mg / ml, the solvent is isopropanol, the annealing temperature is 60° C., and the annealing time is 3 minutes.
[0093] 3. Using the existing technical solution, a mixed organic salt solution of formamidine iodine (FAI) and methylamine chloride (MACl) is spin-coated on the lead iodide film that generates the seed crystal, and annealed to form a perovskite film.
[0094] 4. Using the existing technical solution, a hole transport layer of 2,2′,7,7′-tetra[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene is spin-coated on the surface of the perovskite film. A layer of molybdenum trioxide and a layer of silver electrode are evaporated on the hole transport layer; the thickness of the molybdenum trioxide is 12 nanometers, and the thickness of the silver electrode is 100 nanometers.
[0095] The above is an implementation case of in-situ seed crystallization induced by using thiophene methylamine iodide as an organic ligand material. The conventional seed crystallization scheme is: in step 3 above, thiophene methylamine iodide seed crystals are added into the lead iodide solution, and the solution is spin-coated on the electron transport layer. The comparison chart of the photovoltaic conversion efficiency of the device obtained in this implementation case is as follows: Fig.11 , the traditional seed-induced crystallization scheme only achieved a photoelectric conversion efficiency of 22.74%, which is significantly lower than the 24.43% photoelectric conversion efficiency obtained by the in-situ seed-induced crystallization scheme. This shows that the perovskite active layer induced by in-situ seed crystallization has a higher crystal quality! The result is a device efficiency diagram showing that the device efficiency obtained by the in-situ seed-induced scheme of this patent is higher than that of the traditional seed-induced scheme.
Claims
1. A method for preparing a perovskite film; characterized in that: An organic ligand is spin-coated on the surface of a lead iodide film, and two-dimensional perovskite seeds are generated in situ after annealing, and the crystallization of the perovskite light-absorbing layer is further induced to obtain a perovskite light-absorbing layer with high crystallinity. Specifically, a layer of lead iodide solution is spin-coated on the electron transport layer, and after annealing, a layer of organic ligand material is spin-coated on the surface of the lead iodide film, and after annealing, a two-dimensional perovskite seed is formed and dispersed on the surface of the lead iodide film. A mixed solution of formamidine iodide salt and methylamine chloride salt is spin-coated on the above-mentioned lead iodide film, and annealing is performed to obtain a three-dimensional perovskite film induced by seed crystallization; the two-dimensional perovskite seed is pure phase.
2. The method for preparing a perovskite thin film according to claim 1, characterized in that: 4,5,6,7-tetrahydrothieno[2,3-C]pyridine hydroiodide ThPyI is spin-coated on the surface of the lead iodide film to form (ThPy)2PbI4 seed crystals in situ with lead iodide.
3. The method for preparing a perovskite thin film according to claim 1, characterized in that: Tetrahydroisoquinoline iodide salt THIQI is spin-coated on the surface of the lead iodide film to form (THIQ)2PbI4 seed crystals in situ with the lead iodide.
4. The method for preparing a perovskite thin film according to claim 1, characterized in that: Phenylethylamine iodide salt PEAI is spin-coated on the surface of the lead iodide film to form (PEA)2PbI4 seed crystals in situ with the lead iodide.
5. The method for preparing a perovskite thin film according to claim 1, characterized in that: Thiophenemethylamine iodide salt ThMAI is spin-coated on the surface of the lead iodide film to in-situ form (ThMA)2PbI4 with lead iodide.
6. The method for preparing a perovskite thin film according to claim 1, characterized in that: Butylamine iodide salt BAI is spin-coated on the surface of the lead iodide film to form (BA)2PbI4 with lead iodide.
7. The method for preparing a perovskite thin film according to claim 1, characterized in that: Thiophenemethylamine iodide TTMAI is spin-coated on the surface of the lead iodide film to form (TTMA)2PbI4 with lead iodide.
8. The method for preparing a perovskite film according to claim 1 is used in a method for preparing a solar cell device, characterized in that: The steps include: Step 1) depositing or spin coating an electron transport layer on the cleaned ITO or FTO conductive glass; Step 2) Spin-coating a layer of lead iodide solution on the electron transport layer and annealing it; Step 3) Spin-coating a layer of organic ligand material on the surface of the lead iodide film, and annealing the layer to form two-dimensional perovskite seeds dispersed on the surface of the lead iodide film; Step 4: Spin-coating a mixed solution of formamidine iodide salt and methylamine chloride salt on the surface of the lead iodide film; annealing the film at 100-180° C. to obtain a seed-induced crystallized three-dimensional perovskite film; Step 5: Spin-coating a hole transport layer to obtain a hole transport layer; Step 6: Vacuum evaporation is used to deposit a layer of molybdenum trioxide and a metal electrode on the hole transport layer.
9. The method for preparing a perovskite film according to claim 8 is used in a method for preparing a solar cell device, characterized in that: Step 3) Spin-coating a layer of organic ligand material on the surface of the lead iodide film, including phenylethylamine iodide, thiophenemethylamine iodide or butylamine iodide; the solvent is isopropanol and ethanol, the concentration is 0.5-10 mg / ml material, and annealing treatment is performed, the annealing temperature is 50-100°C, the annealing time is 0 minutes to 10 minutes, and two-dimensional perovskite seeds are dispersed on the surface of the lead iodide film.
Citation Information
Patent Citations
Perovskite layer preparation method, solar cell and assembly
CN114447232A
Cited By
Two-dimensional single crystal redissolution modified cesium-containing perovskite cell and preparation method thereof