A cathode electrode and a battery thereof

By setting up a composite active coating in the cathode plate to balance the working voltage of the phosphate material and layered oxide, the problem of the structure and cycle stability of the cathode plate under high voltage is solved, and the synergistic advantages of the materials are fully utilized and Improvement of electrochemical performance.

CN116864616BActive Publication Date: 2024-10-08EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310860963.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2024-10-08
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

It is difficult for existing cathode plates to achieve the synergistic advantages of phosphate materials and layered oxides at high voltages, and is prone to excessive delithiation, resulting in poor structure and cycle stability.

Method used

A composite active coating is installed in the cathode plate, including a layered oxide active coating, a protective layer and a phosphate active coating. The working voltage of the two is balanced through the protective layer, and the thickness and area density are reasonably set to ensure voltage matching. and material synergy.

Benefits of technology

The structural stability and cycle stability of the cathode plate under high voltage are achieved, excessive delithiation is avoided, and the electrochemical performance and energy density are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116864616B_ABST
    Figure CN116864616B_ABST
Patent Text Reader

Abstract

The present invention provides a cathode electrode sheet, comprising a current collector and a composite active coating arranged on the surface of the current collector; in the thickness direction of the composite active coating, the composite active coating comprises a layered oxide active coating, a protective layer and a phosphate active coating which are composited in sequence, the phosphate active coating comprises a first phosphate material, the protective layer comprises a second phosphate material, and the layered oxide active coating comprises a layered oxide; and the working voltage of the first phosphate material is lower than the working voltage of the second phosphate material; the thickness ratio of the protective layer to the thickness of the layered oxide active coating is 2-50:5-200; the surface density of the protective layer is 1-50 g / m 2 The surface density of the layered oxide active coating is 10 to 200 g / m 2 The cathode electrode provided by the present invention fully utilizes the synergistic advantages of phosphate materials and layered oxides, and ensures that the cathode electrode as a whole has excellent structural stability and cycle stability under high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular, relates to a cathode electrode sheet and a battery thereof. Background Art

[0002] Phosphate materials have good cycle performance and safety performance, and layered oxides have high capacity and compaction density; using phosphate materials and layered oxides simultaneously in the cathode pole piece can achieve a cathode pole piece with better comprehensive performance in cycle performance, safety performance, capacity, and compaction density. At present, there are co-doped pole pieces on the market that directly mix and coat the above two materials. This design is easy to manufacture, but the particle size and density of the above two materials are very different, and it is difficult to achieve uniform mixing, so that the phosphate material and the layered oxide cannot give full play to the synergistic advantages of the two; there are also patents that point out that phosphate materials and layered oxides can be layered and coated to obtain composite pole pieces, but no matter whether the phosphate material is located in the upper or lower layer, the composite pole piece produced cannot match the application of high voltage, which easily leads to excessive lithium removal of the pole piece. This is mainly due to the low working voltage of the phosphate material and the high working voltage of the layered oxide. Separate coating cannot achieve stable dynamic performance under high voltage. Based on this, how to give full play to the synergistic advantages of phosphate materials and layered oxides in the same cathode pole piece and ensure the structural stability and cycle stability of the cathode pole piece under high voltage is a technical problem that technicians in this field urgently need to solve in their research. Summary of the invention

[0003] The object of the present invention is to provide a cathode electrode sheet in which the synergistic advantages of phosphate materials and layered oxides can be fully utilized, and the cathode electrode sheet as a whole can be ensured to have excellent structural stability and cycle stability under high voltage.

[0004] According to one aspect of the present invention, a cathode electrode sheet is provided, comprising a current collector and a composite active coating arranged on the surface of the current collector; in the thickness direction of the composite active coating, the composite active coating comprises a layered oxide active coating, a protective layer and a phosphate active coating which are composited in sequence, the phosphate active coating comprises a first phosphate material, the protective layer comprises a second phosphate material, and the layered oxide active coating comprises a layered oxide; and the working voltage of the first phosphate material is lower than the working voltage of the second phosphate material; the thickness ratio of the protective layer to the layered oxide active coating is 2-50:5-200; the surface density of the protective layer is 1-50 g / m 2 The surface density of the layered oxide active coating is 10 to 200 g / m 2For example, the ratio of the thickness of the protective layer to the thickness of the layered oxide active coating is 2:5, 2:50, 2:100, 2:150, 2:200, 25:5, 25:50, 25:100, 25:150, 25:200, 50:5, 50:50, 50:100, 50:150 or 50:200, etc.; the surface density of the protective layer is 1 g / m 2 , 10g / m 2 , 20g / m 2 , 30g / m 2 , 40g / m 2 or 50g / m 2 ; The surface density of the layered oxide active coating is 10g / m 2 , 50g / m 2 , 100g / m 2 , 150g / m 2 or 200g / m 2 Since the working voltage of phosphate materials is low, it does not match the working voltage of layered oxides. The cathode electrode that integrates the above two materials is prone to degradation of electrode performance due to structural instability under high voltage. The cathode electrode provided by the present invention separates the layered oxide and the first phosphate material with different working voltages by setting a protective layer between the layered oxide active coating and the phosphate active coating; moreover, on the one hand, by using a second phosphate material with a working voltage higher than that of the first phosphate material to form the protective layer, the voltage between the first phosphate material and the layered oxide is balanced, so that the second phosphate material with a higher voltage protects the first phosphate material with a lower voltage; on the other hand, by reasonably setting the thickness ratio and surface density of the protective layer and the layered oxide active coating, the content of the second phosphate material in the protective layer and the layered oxide in the layered oxide active coating is controlled within a suitable range, and on the basis of ensuring that the protective layer effectively plays its voltage balancing role, the composite effect of the layered oxide active coating and the protective layer is improved, the high capacity characteristics of the layered oxide active coating are brought into play, and the long cycle advantages and high safety advantages of the first phosphate material are also brought into play, so as to avoid the interface impedance caused by the mismatch between the working voltages of the protective layer and the layered oxide active coating, and effectively promote the continuous lithium insertion and extraction of the protective layer and the phosphate active coating. This is conducive to forming a continuous and stable discharge platform, preventing the problem of excessive lithium deintercalation caused by the voltage drop between the layered oxide and the phosphate material, and achieving stable lithium deintercalation between the layered oxide and the phosphate material; thereby fully leveraging the synergistic advantages of the phosphate material and the layered oxide in the same cathode electrode, and ensuring that the cathode electrode as a whole has excellent structural stability and cycle stability under high voltage.

[0005] Specifically, the chemical formula of the first phosphate material and the second phosphate material is LiMn xFe y A (1-x-y) PO 4 , where 0≤x≤1, 0≤y≤1, element A refers to one or two of Mg, Al, Ni, Co, V, Nb, Ca, Ti, Zn, Cu, Zr, Sr, Sn, Y, W, B, Si, Na, and K, and the general chemical formula of the layered oxide is Li a Ni b Co c M (1-b-c) O 2 , where 0.8≤a≤1.4, 0.2≤b≤1, 0≤c≤0.3, and the M element refers to one or two of Mn, Mg, Al, Zr, Ti, V, W, B, Nb, Ca, Zn, Cu, Sr, Sn, Y, Si, Na, and K.

[0006] Preferably, on the same side of the current collector of the cathode electrode sheet, the layered oxide active coating, the protective layer, and the phosphate active coating are sequentially arranged in a direction away from the surface of the current collector.

[0007] Preferably, the thickness ratio of the protective layer to the thickness of the layered oxide active coating is 2-50:30-150; the surface density of the protective layer is 1-50 g / m 2 The surface density of the layered oxide active coating is 30 to 150 g / m 2 .

[0008] Preferably, the thickness of the protective layer is 2 to 50 μm; the thickness of the layered oxide active coating is 30 to 150 μm. For example, the thickness of the protective layer is 2 μm, 10 μm, 20 μm, 30 μm, 40 μm or 50 μm; the thickness of the layered oxide active coating is 30 μm, 60 μm, 90 μm, 120 μm or 150 μm, etc. On the one hand, if the thickness of the protective layer is too small and the surface density is too small, the content of the second phosphate material in the protective layer is too small, and it cannot play a good role in balancing the discharge voltage; if the thickness of the protective layer is too large and the surface density is too large, the second phosphate material with a higher working voltage has a higher impedance, which deteriorates the cycle performance of the electrode. Therefore, the cathode electrode provided by the present invention can effectively balance the working voltage of the protective layer and the layered oxide active coating while ensuring that the impedance of the battery is at a low level by reasonably setting the thickness and surface density of the protective layer, thereby improving the electrochemical performance of the cathode electrode. On the other hand, if the layered oxide active coating is too thin, the content of layered oxide in the layered oxide active coating is too small, which will reduce the capacity and energy density of the electrode; if the layered oxide active coating is too thick, the transmission path of lithium ions will become longer, which will increase the impedance of the electrode and reduce the cycle performance.

[0009] Preferably, the thickness of the phosphate active coating is 50 to 150 μm and the surface density is 15 to 280 g / m 2 For example, the thickness of the phosphate active coating is 50 μm, 100 μm or 150 μm; the surface density is 15 g / m 2 , 80g / m 2 , 140g / m 2 , 200g / m 2 or 280g / m 2 On the one hand, the thinner the phosphate active coating is, the less the content of the first phosphate material is, and thus the capacity of the cathode electrode is lower, and its energy density is lower; the thicker the phosphate layer is, the thicker the electrode is as a whole, the longer the lithium ion transmission path is, and thus the electrode impedance is higher, and the cycle performance is lower; the present invention further improves the energy density and cycle performance of the battery by reasonably setting the thickness and surface density of the phosphate active coating.

[0010] Preferably, D represents the sum of the thicknesses of the layered oxide active coating, the protective layer and the phosphate active coating that are compounded in sequence, and D satisfies: 50μm≤D≤300μm. If the thickness of the cathode pole piece is too thin, the content of the three cathode active materials contained is too small, the pole piece is difficult to process, and the capacity and energy density are low; if the thickness of the pole piece is too thick, the electrolyte infiltration is difficult, resulting in increased impedance of the pole piece and reduced cycle performance. In the present invention, by controlling the thickness of the cathode pole piece within the above range, the cycle performance and energy density of the pole piece can be further improved while ensuring the processing performance of the pole piece.

[0011] Preferably, the second phosphate material includes one of lithium iron manganese phosphate, lithium vanadium phosphate, nickel manganese phosphate, lithium manganese vanadium phosphate, and lithium nickel iron phosphate. The chemical formula of lithium iron manganese phosphate is LiMn m Fe (1-m) PO 4 (0<m<1), the chemical formula of lithium vanadium phosphate is Li 3 V 2 (PO 4 ) 3 , the chemical formula of lithium nickel manganese phosphate is LiNi n Mn (1-n) PO 4 (0<n<1), the chemical formula of lithium manganese vanadium phosphate is LiMn p V (1-p) PO 4 (0<p<1), the chemical formula of lithium nickel iron phosphate is LiFe q Ni (1-q) PO 4 (0<q<1).

[0012] Preferably, the second phosphate material is a carbon-coated phosphate material, and the carbon content of the carbon-coated phosphate material is 0.5-3wt% calculated by mass percentage. The present invention provides a carbon coating layer on the surface of the second phosphate material, and reasonably sets the carbon content in the carbon coating layer, so that the working voltage and conductivity of the second phosphate material constituting the protective layer are improved, thereby making the cathode electrode sheet have better compaction density and structural stability, and giving the battery excellent electrochemical performance and cycle performance. If the carbon content in the carbon coating layer of the second phosphate material is too low, the conductivity of the phosphate material will decrease, thereby causing the electrode sheet surface resistance to increase; if the carbon content in the carbon coating layer of the phosphate material is too high, it is necessary to increase the thickness of the carbon coating layer to a certain extent, deteriorating the compaction density of the cathode sheet, and also increasing the difficulty of making the cathode electrode sheet, reducing the peeling force of the cathode electrode sheet, thereby causing the electrochemical performance and cycle performance of the battery to decrease.

[0013] Preferably, the particle size of the carbon-coated phosphate material is 0.1 to 5 μm, and the specific surface area is 10 to 30 g / m 2 The present invention controls the particle size and specific surface area of ​​the carbon-coated phosphate material within the above range, which can improve the compaction density and structural stability of the cathode electrode while ensuring the processing performance of the cathode electrode, thereby improving the electrochemical performance and cycle performance of the battery.

[0014] Preferably, the intensity of the D peak in the Raman spectrum corresponding to the carbon-coated phosphate material is 1 d The intensity of the G peak in the Raman spectrum corresponding to the carbon-coated phosphate material is I g , carbon-coated phosphate materials meet: 0.7≤I d / I g ≤1.2. The present invention is to coat the phosphate material with carbon d with I g The ratio of is controlled within the range of 0.7 to 1.2, which is conducive to controlling the graphitization degree and thickness of the carbon coating layer on its surface within a reasonable range, thereby improving the structural stability and conductivity of the phosphate material. d / I g <0.7, the graphitization degree of the carbon coating is low, the structure of the carbon coating is unstable, and the conductivity is reduced; if the I of the phosphate material d / I g >1.2, the thickness of the carbon coating layer is thick and the lithium ion transmission path is long, which leads to a decrease in the electrochemical performance and cycle performance of the battery.

[0015] Specifically, I d Refers to the D peak in the Raman spectrum corresponding to the carbon-coated phosphate material (the D peak is located at 1580cm in the Raman spectrum -1The intensity of the absorption peak near g Refers to the G peak in the Raman spectrum corresponding to the carbon-coated phosphate material (the G peak is located at 1360cm in the Raman spectrum -1 The intensity of the absorption peak near .

[0016] According to another aspect of the present invention, a battery is provided, the battery comprising the above-mentioned cathode electrode plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of the structure of the cathode electrode piece prepared in Examples 1 to 9;

[0018] Figure 2 This is a schematic diagram of the structure of the cathode electrode obtained in Example 10;

[0019] Figure 3 Schematic diagram of the structure of the cathode electrode sheet prepared in Comparative Examples 1 to 4;

[0020] Figure 4 The schematic diagram of the structure of the cathode electrode piece prepared in Comparative Examples 5 to 6;

[0021] Figure 5 This is a schematic diagram of the structure of the cathode electrode prepared in Comparative Example 7.

[0022] Reference numerals: 1 layered oxide active coating, 2 protective layer, 3 phosphate active coating, 4 current collector. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides a battery, and the preparation method thereof comprises the following steps:

[0026] 1. Preparation of cathode electrode

[0027] The first phosphate material LiFePO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; the second phosphate material LiMn 0.6 Fe 0.4 PO 4(Particle size of the second phosphate material = 0.9 μm, specific surface area = 30 g / m 2 , and the second phosphate material has a carbon layer on its surface), a conductive agent acetylene black, and a binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a second cathode slurry; the layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the third cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then coated with a second cathode slurry on the surface of the layered oxide active coating 1 and dried to form a layered oxide active coating with a thickness of 5 μm and a surface density of 10 g / m 2 The protective layer 2 is then coated with the first cathode slurry on the surface of the protective layer 2 and dried to form a layer with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then rolled and sliced ​​to obtain a cathode electrode sheet, in which D represents the sum of the thicknesses of the layered oxide active coating 1, the protective layer 2 and the phosphate active coating 3, which are compounded in sequence, and D = 105 μm; the schematic diagram of the structure of the cathode electrode sheet obtained above is shown in Figure 1 shown.

[0028] 2. Anode plate preparation

[0029] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0030] 3. Preparation of electrolyte

[0031] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0032] 4. Preparation of diaphragm

[0033] The diaphragm is made of polyethylene diaphragm;

[0034] 5. Battery cell assembly

[0035] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, the battery of this embodiment is obtained.

[0036] Example 2

[0037] This embodiment is used to prepare a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the first phosphate material is LiMn 0.1 Fe 0.9 PO 4 , the second phosphate material is LiMn 0.7 Fe 0.3 PO 4 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0038] Example 3

[0039] This embodiment is used to prepare a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the first phosphate material is LiMn 0.6 Fe 0.4 PO 4 , the second phosphate material is Li 3 V 2 (PO 4 ) 3 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0040] Example 4

[0041] This embodiment prepares a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the first phosphate material is LiFePO 4 , the second phosphate material is Li 3 V 2 (PO 4 ) 3 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0042] Example 5

[0043] This embodiment prepares a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the thickness of the protective layer is 0.4 μm and the surface density is 1 g / m 2 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0044] Example 6

[0045] This embodiment prepares a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the thickness of the protective layer is 2 μm and the surface density is 2 g / m 2 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0046] Example 7

[0047] This embodiment prepares a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the thickness of the protective layer is 20 μm and the surface density is 25 g / m 2 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0048] Example 8

[0049] This embodiment prepares a battery with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the thickness of the protective layer is 50 μm and the surface density is 45 g / m 2 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0050] Example 9

[0051] The present embodiment is to prepare a battery with reference to the embodiment 1. The difference between the present embodiment and the embodiment 1 is that the thickness of the protective layer is 400 μm and the surface density is 50 g / m 2 Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.

[0052] Example 10

[0053] This embodiment provides a battery, and the preparation method thereof comprises the following steps:

[0054] 1. Preparation of cathode electrode

[0055] The first phosphate material LiFePO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; the second phosphate material LiMn 0.6 Fe 0.4 PO 4 (The particle size D50 of the second phosphate material = 0.8 μm, specific surface area = 30 g / m 2, and the second phosphate material has a carbon layer on its surface), a conductive agent acetylene black, and a binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a second cathode slurry; the layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the first cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then coated with a second cathode slurry on the surface of the phosphate active coating 3 and dried to form a phosphate active coating with a thickness of 5 μm and a surface density of 10 g / m 2 The protective layer 2 is then coated with the third cathode slurry on the surface of the protective layer 2 and dried to form a layer with a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then rolled and sliced ​​to obtain a cathode electrode sheet; the schematic diagram of the structure of the cathode electrode sheet obtained above is as shown in Figure 2 shown.

[0056] 2. Anode plate preparation

[0057] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0058] 3. Preparation of electrolyte

[0059] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0060] 4. Preparation of diaphragm

[0061] The diaphragm is made of polyethylene diaphragm;

[0062] 5. Battery cell assembly

[0063] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, the battery of this embodiment is obtained.

[0064] Embodiment 11

[0065] This embodiment provides a battery, and the preparation method thereof comprises the following steps:

[0066] 1. Preparation of cathode electrode

[0067] The first phosphate material LiMn 0.6 Fe 0.4 PO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; the second phosphate material LiMn 0.6 Fe 0.4 PO 4 (Particle size of the second phosphate material = 0.1 μm, specific surface area = 30 g / m 2 , and the second phosphate material has a carbon layer on its surface), a conductive agent acetylene black, and a binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a second cathode slurry; the layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the first cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then coated with a second cathode slurry on the surface of the phosphate active coating 3 and dried to form a phosphate active coating with a thickness of 5 μm and a surface density of 10 g / m 2 The protective layer 2 is then coated with the third cathode slurry on the surface of the protective layer 2 and dried to form a layer with a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then rolled and sliced ​​to obtain a cathode electrode sheet; the schematic diagram of the structure of the cathode electrode sheet obtained above is as shown in Figure 2 shown.

[0068] 2. Anode plate preparation

[0069] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0070] 3. Preparation of electrolyte

[0071] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0072] 4. Preparation of diaphragm

[0073] The diaphragm is made of polyethylene diaphragm;

[0074] 5. Battery cell assembly

[0075] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, the battery of this embodiment is obtained.

[0076] Comparative Example 1

[0077] This comparative example provides a battery, and its preparation method comprises the following steps:

[0078] 1. Preparation of cathode electrode

[0079] The first phosphate material LiFePO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the third cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then coated with the first cathode slurry on the surface of the layered oxide active coating 1 and dried to form a layered oxide active coating with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then rolled and sliced ​​to obtain a cathode electrode sheet; the schematic diagram of the structure of the cathode electrode sheet obtained above is as shown in Figure 3 shown.

[0080] 2. Anode plate preparation

[0081] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0082] 3. Preparation of electrolyte

[0083] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0084] 4. Preparation of diaphragm

[0085] The diaphragm is made of polyethylene diaphragm;

[0086] 5. Battery cell assembly

[0087] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and the battery of this comparative example is obtained through vacuum packaging, standing, forming, shaping and other processes.

[0088] Comparative Example 2

[0089] This comparative example is used to prepare a battery with reference to comparative example 1. The difference between this comparative example and comparative example 1 is that the first phosphate material is LiMn 0.6 Fe 0.4 PO 4 Except for the above differences, the materials and process operations used in this comparative example are strictly consistent with those of comparative example 1.

[0090] Comparative Example 3

[0091] This comparative example is used to prepare a battery with reference to Example 1. The difference between this comparative example and Example 1 is that the thickness of the protective layer is 0.2 μm and the surface density is 0.5 g / m 2 Except for the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.

[0092] Comparative Example 4

[0093] This comparative example is used to prepare a battery with reference to Example 1. The difference between this comparative example and Example 1 is that the thickness of the protective layer is 420 μm and the surface density is 80 g / m 2Except for the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.

[0094] Comparative Example 5

[0095] This comparative example provides a battery, and its preparation method comprises the following steps:

[0096] 1. Preparation of cathode electrode

[0097] The first phosphate material LiFePO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the first cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then coated with a third cathode slurry on the surface of the phosphate active coating 3 and dried to form a phosphate active coating having a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then rolled and sliced ​​to obtain a cathode electrode sheet; the schematic diagram of the structure of the cathode electrode sheet obtained above is as shown in Figure 3 shown.

[0098] 2. Anode plate preparation

[0099] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0100] 3. Preparation of electrolyte

[0101] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0102] 4. Preparation of diaphragm

[0103] The diaphragm is made of polyethylene diaphragm;

[0104] 5. Battery cell assembly

[0105] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and the battery of this comparative example is obtained through vacuum packaging, standing, forming, shaping and other processes.

[0106] Comparative Example 6

[0107] This comparative example is used to prepare a battery with reference to comparative example 3. The difference between this comparative example and comparative example 3 is that the first phosphate material is LiMn 0.6 Fe 0.4 PO 4 Except for the above differences, the materials and process operations used in this comparative example are strictly consistent with those of comparative example 3.

[0108] Comparative Example 7

[0109] This comparative example provides a battery, and its preparation method comprises the following steps:

[0110] 1. Preparation of cathode electrode

[0111] The first phosphate material LiFePO 4 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then solvent NMP is added to prepare a first cathode slurry; the second phosphate material LiMn 0.6 Fe 0.4 PO 4 (Particle size of the second phosphate material = 0.9 μm, specific surface area = 30 g / m 2 , and the second phosphate material has a carbon layer on its surface), a conductive agent acetylene black, and a binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a second cathode slurry; the layered oxide LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then a solvent NMP is added to prepare a third cathode slurry; the third cathode slurry is coated on the surface of the current collector 4 and dried to form a slurry with a thickness of 40 μm and a surface density of 130 g / m 2 The layered oxide active coating 1 is then coated with the first cathode slurry on the surface of the layered oxide active coating 1 and dried to form a layered oxide active coating with a thickness of 60 μm and a surface density of 125 g / m 2 The phosphate active coating 3 is then coated with a second cathode slurry on the surface of the phosphate active coating 3 and dried to form a phosphate active coating with a thickness of 5 μm and a surface density of 5 g / m2 The protective layer 2 is then rolled and sliced ​​to obtain a cathode electrode sheet; the schematic diagram of the structure of the cathode electrode sheet obtained above is as shown in Figure 3 shown.

[0112] 2. Anode electrode preparation

[0113] The anode active material graphite, the conductive agent acetylene black, the binder carboxymethyl cellulose (CMC), and SBR (styrene butadiene rubber) are mixed in a mass ratio of 94:1:2:3, and then deionized water is added as a solvent and stirred evenly to obtain an anode slurry; the anode slurry is evenly coated on the surface of the copper foil, and then dried, rolled, and sliced ​​to obtain an anode sheet.

[0114] 3. Preparation of electrolyte

[0115] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0116] 4. Preparation of diaphragm

[0117] The diaphragm is made of polyethylene diaphragm;

[0118] 5. Battery cell assembly

[0119] The cathode electrode sheet, the isolation film, and the anode electrode sheet are stacked in order, the isolation film is placed between the cathode electrode sheet and the anode electrode sheet to play an isolation role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, the battery of this embodiment is obtained.

[0120] Test Case

[0121] 1. Participants

[0122] In this test example, the cathode plates and batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 7 were used as test objects to conduct relevant performance tests.

[0123] 2. Test content

[0124] (1) Surface resistance

[0125] The diaphragm resistance test equipment TT-ACCF-G2 was used to test and record the resistance of the cathode electrode under a pressure of 0.4T, and the surface resistance of the cathode electrode was calculated according to the following formula: surface resistance = resistance / area of ​​the electrode.

[0126] (2) Cycle performance

[0127] The tested batteries were placed in a 45°C constant temperature box, charged at 1C constant current and constant voltage, cut off at 0.02C, and then discharged at 1C to 80% SOH, and the number of cycles was recorded.

[0128] (3) Energy density

[0129] The test battery was charged to 4.25V at 0.33C constant current and constant voltage, cut off at 0.02C, and then discharged to 2.8V at 0.33C. The capacity, average voltage and cell mass were recorded. The energy density of the battery was calculated according to the following formula: Energy density = capacity * average voltage / battery mass.

[0130] 3. Test results

[0131] Table 1. Performance test results of the batteries of Examples 1 to 11 and Comparative Examples 1 to 7

[0132]

[0133] The relevant performance test results of the batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 7 are shown in Table 1.

[0134] The performance test results of Examples 1 and 10 are compared with those of Comparative Examples 1 and 5. As shown in Table 1, under the same conditions for preparing the first phosphate material and other materials of the battery, compared with Examples 1 and 10, the cathode pole pieces prepared in Comparative Examples 1 and 5 are only provided with a phosphate active coating and a layered oxide active coating, but no protective layer. Since the working voltage of the first phosphate material is relatively low, it does not match the working voltage of the layered oxide. The cathode pole piece integrating the above two materials is prone to structural instability under high voltage. The cycle performance of the battery obtained is significantly lower than that of the battery obtained in Examples 1 and 10, and the energy density of the battery obtained is lower than that of the battery obtained in Examples 1 and 10; the performance test results of Examples 3 and 11 are compared with those of Comparative Examples 2 and 6. It can be seen from Table 1 that under the same conditions for preparing the first phosphate active material and other materials of the battery, compared with Examples 3 and 11, the cathode pole pieces prepared in Comparative Examples 2 and 6 are only provided with a phosphate active coating and a layered oxide active coating, but no protective layer is provided. Since the working voltage of the first phosphate material is relatively low, it does not match the working voltage of the layered oxide. The cathode pole piece integrating the above two materials is prone to structural instability under high voltage. The cycle performance of the battery obtained thereby is significantly lower than that of the battery prepared in Examples 3 and 11, and the energy density is lower than that of the battery prepared in Examples 3 and 11. This shows that, relative to Comparative Examples 1-2, 5-6, the cathode pole pieces provided in Examples 1, 3, 10-11 balance the voltage between the layered oxide and the first phosphate material with a lower voltage by introducing a protective layer, thereby protecting the first phosphate material with a lower voltage, reducing the problem of excessive lithium desorption caused by the voltage drop between the layered oxide and the phosphate material with a lower voltage, achieving stable lithium desorption between the layered oxide and the phosphate material, and thereby giving full play to the synergistic advantages of the phosphate material and the layered oxide in the same cathode pole piece, and improving the electrochemical performance and cycle performance of the cathode pole piece at high voltage.

[0135] The performance test results of Examples 1, 5-9 and Comparative Examples 3-4 are compared. It can be seen from Table 1 that under the same conditions of other materials and operations for preparing the battery, the thickness ratio of the protective layer to the layered oxide active coating in the cathode electrode sheets prepared in Comparative Examples 3-4 does not meet the requirement of 2-50:5-200, and the surface density of the protective layer is less than 1 g / m 2, the cycle performance of the battery obtained thereby is significantly lower than that of the battery obtained in Example 1, and the energy density is lower than that of the battery obtained in Example 1. This shows that, relative to Comparative Examples 3 to 4, the cathode plates provided in Examples 1, 5 to 9 reasonably set the thickness ratio and surface density of the protective layer to the layered oxide active coating, so that the content of the second phosphate material in the protective layer and the layered oxide in the layered oxide active coating is controlled within a suitable range, and on the basis of ensuring that the protective layer effectively plays its voltage balancing role, the composite effect of the layered oxide active coating and the protective layer is improved, and the problems such as interface impedance caused by the mismatch of the working voltage between the protective layer and the layered oxide active coating are further prevented, thereby improving the electrochemical performance and cycle performance of the obtained cathode plates at high voltage.

[0136] Comparing the performance test results corresponding to Example 1 and Comparative Example 7, it can be seen from Table 1 that under the same conditions of preparing other materials and operations for the battery, the cathode electrode plate prepared in Comparative Example 7 has a phosphate active coating of a first phosphate material with a lower voltage disposed between the layered oxide active coating and the protective layer, and the cycle performance of the battery obtained is significantly lower than that of the battery prepared in Example 1, and the energy density is lower than that of the battery prepared in Example 1. This shows that, relative to Comparative Example 7, the cathode electrode plate provided in Example 1 separates the layered oxide and the first phosphate material with different working voltages by disposing a protective layer between the phosphate active coating and the layered oxide active coating; and the working voltage of the second phosphate material constituting the protective layer is higher than that of the first phosphate material, balancing the voltage between the first phosphate material and the layered oxide, realizing the protective effect of the second phosphate material with a higher voltage on the first phosphate material with a lower voltage, thereby improving the electrochemical performance and cycle performance of the prepared cathode electrode plate at high voltage.

[0137] The performance test results of Example 1 are compared with those of Examples 5 to 9. As shown in Table 1, under the same conditions of other materials and operation for preparing the battery, the thickness of the protective layer set in Example 5 is less than 2 μm, and the surface density is less than 1 g / m 2 The content of the second phosphate material in the protective layer is relatively small, and it is difficult to play a good role in balancing the discharge voltage. The energy density and cycle performance of the battery obtained are lower than those of the battery prepared in Example 1. The thickness of the protective layer set in Example 9 is greater than 50 μm, and the surface density is greater than 50 g / m 2The second phosphate material with a higher voltage has a higher impedance, which deteriorates the cycle performance of the electrode sheet, and the energy density and cycle performance of the battery obtained are lower than those of the battery prepared in Example 1. This shows that, compared with Examples 5 and 9, the cathode electrode sheets provided in Examples 1, 6 to 8 can effectively balance the voltage of the protective layer and the layered oxide active coating while ensuring that the impedance of the battery is at a low level by reasonably setting the thickness and surface density of the protective layer, so that the prepared battery has excellent electrochemical performance and cycle performance.

[0138] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A cathode electrode, characterized in that: The invention comprises a current collector and a composite active coating disposed on the surface of the current collector; in the thickness direction of the composite active coating, the composite active coating comprises a layered oxide active coating, a protective layer and a phosphate active coating which are composited in sequence, the phosphate active coating comprises a first phosphate material, the protective layer comprises a second phosphate material, and the layered oxide active coating comprises a layered oxide; and the operating voltage of the first phosphate material is lower than the operating voltage of the second phosphate material; The ratio of the thickness of the protective layer to the thickness of the layered oxide active coating is 2-50:5-200; The surface density of the protective layer is 1 to 50 g / m 2 The surface density of the layered oxide active coating is 10 to 200 g / m 2 .

2. The cathode electrode according to claim 1, characterized in that: The ratio of the thickness of the protective layer to the thickness of the layered oxide active coating is 2-50:30-150; The surface density of the protective layer is 1 to 50 g / m 2 The surface density of the layered oxide active coating is 30 to 150 g / m 2 .

3. The cathode electrode according to claim 1, characterized in that: The thickness of the protective layer is 2-50 μm; the thickness of the layered oxide active coating is 30-150 μm.

4. The cathode electrode according to claim 3, characterized in that: The thickness of the phosphate active coating is 50 to 150 μm; the surface density is 15 to 280 g / m 2 .

5. The cathode electrode according to any one of claims 1 to 4, characterized in that: D represents the sum of the thicknesses of the layered oxide active coating, the protective layer and the phosphate active coating which are composited in sequence, and D satisfies: 50 μm≤D≤300 μm.

6. The cathode electrode according to claim 1, characterized in that: The second phosphate material includes one of lithium manganese iron phosphate, lithium vanadium phosphate, lithium nickel manganese phosphate, lithium manganese vanadium phosphate, and lithium nickel iron phosphate.

7. The cathode electrode according to claim 1, characterized in that: The second phosphate material is a carbon-coated phosphate material. Calculated by mass percentage, the carbon content of the carbon-coated phosphate material is 0.5-3wt%.

8. The cathode electrode according to claim 7, characterized in that: The carbon-coated phosphate material has a particle size of 0.1 to 5 μm and a specific surface area of ​​10 to 30 g / m 2 .

9. The cathode electrode according to claim 7, characterized in that: The intensity of the D peak in the Raman spectrum corresponding to the carbon-coated phosphate material is taken as I d The intensity of the peak G in the Raman spectrum corresponding to the carbon-coated phosphate material is taken as I g , the carbon-coated phosphate material satisfies: 0.7≤I d / I g ≤1.

2.

10. A battery, characterized in that: It comprises the cathode electrode piece as claimed in any one of claims 1 to 9.