A zeolite imidazole ester framework-ionic liquid composite gel electrolyte and its preparation method
By combining ZIF-90 with ionic liquids, a chemically cross-linked polymer electrolyte was developed, which solved the safety hazards of lithium batteries and the problem of uneven ZIF dispersion, achieving high safety and excellent electrochemical performance.
Patent Information
- Application Number
- CN202310925052.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-26
AI Technical Summary
Existing lithium batteries use flammable and volatile organic liquid electrolytes, posing safety hazards and problems such as lithium dendrite growth. Furthermore, uneven dispersion of ZIFs in the electrolyte affects battery performance.
By combining ZIF-90 with ionic liquids, a chemically cross-linked polymer electrolyte is formed through a click reaction. The large surface area and multi-level nanopores of ZIF-90 are used to fix the ionic liquid, thereby enhancing battery stability. Furthermore, the ZIF-90 particles are bonded to the polymer through the adhesion of polydopamine.
A composite gel electrolyte with high safety, high ionic conductivity, wide electrochemical window and high ion mobility number was achieved, which inhibits lithium dendrite formation and improves battery cycle performance and rate performance.
Smart Images

Figure CN116885273B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of batteries, specifically relating to a zeolite imidazole ester framework-ionic liquid composite gel electrolyte, its preparation method and application, and particularly the use of this electrolyte in solid-state lithium metal batteries. Background Technology
[0002] Faced with environmental pollution and the fossil fuel crisis, there is a need for an efficient, clean, and safe energy storage system. Lithium metal batteries, due to their high theoretical capacity (3860 mAh·g), are a suitable choice. -1 Lithium-ion batteries have attracted significant attention due to their advantages such as low reduction potential (-3.040V vs. standard hydrogen electrode) and are considered strong contenders for next-generation energy storage systems. However, commercial lithium-ion batteries currently use flammable and volatile organic liquid electrolytes, posing challenges such as safety issues and lithium dendrite growth. Therefore, there is an urgent need to develop highly safe lithium metal batteries.
[0003] Solid-state electrolytes have attracted widespread attention and rapid development as a solution due to their thermal stability and lack of liquid leakage risk. Among them, zeolite imidazole ester frameworks (ZIFs), which combine transition metal ions with organic ligands, are considered strong candidates for solid-state electrolytes. ZIFs possess a designable hierarchical pore structure, high porosity, and high stability, and their nanoporous structure enables rapid lithium-ion transport. They can also attract anions, promote lithium salt dissolution, and restrict anion movement, thereby improving ionic conductivity and lithium-ion transfer number. Furthermore, the high porosity of ZIFs facilitates the adsorption of highly reactive small molecules, improving the interfacial stability between the electrolyte and the electrode and extending the electrochemical stability window. Currently, ZIFs are mainly used as fillers incorporated into polymers to prepare composite solid-state electrolytes. However, in practical applications, ZIFs exhibit severe agglomeration, leading to uneven dispersion of the filler in the electrolyte and limited improvement in battery performance.
[0004] Gel polymer electrolytes (GPEs) possess advantages such as high flexibility, ease of manufacture, and good interfacial compatibility. However, commonly used organic electrolytes such as ethers and esters in GPEs pose risks of leakage, combustion, and explosion. Ionic liquids (ILs) exhibit negligible vapor pressure, non-flammability, and electrochemical stability, making them a suitable alternative to currently used organic electrolytes to improve battery safety. Furthermore, the synergistic effect of combining ZIFs with ILs, where the pore structure restricts the migration of larger cations and anions, effectively enhancing the battery's electrochemical performance. Therefore, this invention primarily relates to a composite gel electrolyte with high room-temperature ionic conductivity, a wide electrochemical window, high ion transport number, and good safety, possessing broad application prospects. Summary of the Invention
[0005] The purpose of this invention is to provide a zeolite imidazole ester framework-ionic liquid composite gel electrolyte and its preparation method. This method combines ZIF-90 and an ionic liquid, forming a chemically cross-linked polymer electrolyte through a click reaction, while simultaneously immobilizing the ionic liquid to improve the electrochemical performance and safety of the battery.
[0006] The technical solution of this invention combines ZIF-90, polydopamine, and an ionic liquid. The large surface area and hierarchical nanopores of ZIF-90 serve as a stable framework, immobilizing the ionic liquid within it, while allowing small lithium ions to pass freely. Polydopamine possesses multiple adhesive forces, effectively binding ZIF-90 particles and the polymer together, enhancing battery stability. To achieve a chemically cross-linked polymer electrolyte, a thiol-ene click chemistry reaction is used, which not only avoids side reactions but also enables rapid cross-linking under mild reaction conditions. The prepared zeolite imidazole ester framework-ionic liquid composite gel electrolyte exhibits an ionic conductivity exceeding 10 at room temperature. -4 S·cm -1 .
[0007] A method for preparing a zeolite imidazole ester framework-ionic liquid composite gel electrolyte includes the following steps:
[0008] Preparation of S1.ZIF-90: Zinc salt was dissolved in solvent 1 to obtain solution A; imidazole-2-formaldehyde was dissolved in solvent 2 to obtain solution B; solution A and solution B were mixed, stirred, and the pale yellow precipitate was washed, centrifuged, and vacuum dried to obtain ZIF-90 powder;
[0009] Furthermore, the solvent 2 is at least one of methanol, water, and N,N-dimethylformamide;
[0010] Furthermore, the zinc salt is one of zinc nitrate hexahydrate or zinc acetate dihydrate, preferably zinc nitrate hexahydrate;
[0011] Furthermore, the molar ratio of the zinc salt to imidazole-2-carboxaldehyde is 1:1 to 10, preferably 1:4;
[0012] Furthermore, the stirring time is 0.25 to 24 hours.
[0013] Preparation of S2.ZIF-90@PDA: ZIF-90 powder was dispersed in an alkaline solvent and ultrasonically treated. 1 wt% to 15 wt% of dopamine hydrochloride was added and stirred for 5 to 24 hours. Then, the mixture was washed, centrifuged and dried to obtain the modified nanofiller ZIF-90@PDA.
[0014] Furthermore, the mass concentration of the ZIF-90 solution is 10–50 mg / mL;
[0015] Furthermore, the pH value of the alkaline solvent is 8.0 to 8.6, preferably 8.5.
[0016] S3. Preparation of zeolite imidazole ester framework-ionic liquid composite gel electrolyte: ZIF-90@PDA and polymer were dispersed in an appropriate amount of solvent, stirred evenly, and then coated onto the electrode sheet and vacuum dried to obtain a support layer; in a glove box, lithium salt, ionic liquid, fluoroethylene carbonate, click reaction precursor and initiator were mixed evenly and dropped onto the support layer to assemble the battery; the battery was placed in an oven and allowed to stand to complete the click reaction, thus obtaining the zeolite imidazole ester framework-ionic liquid composite gel electrolyte.
[0017] Furthermore, the polymer is one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, and polyvinyl alcohol;
[0018] Furthermore, the mass ratio of ZIF-90@PDA to polymer is 1:0.1 to 0.25;
[0019] Furthermore, the lithium salt is one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, and lithium bis(trifluoromethanesulfonyl)imide, preferably lithium bis(trifluoromethanesulfonyl)imide;
[0020] Further, the ionic liquid is one or more combinations of N-methylimidazolium bis(trifluoromethanesulfonyl)imine salt, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imine salt, 1-hexylimidazolium trifluoromethanesulfonate, and 1-ethyl-3-methylimidazolium hexafluorophosphate.
[0021] Furthermore, the click reaction precursor is a polyethylene glycol monomer with unsaturated double bonds and a thiol with two or more mercapto groups;
[0022] Furthermore, the concentration of lithium salt in the mixture is 0.5–2.0 mol / L;
[0023] Furthermore, the temperature of the click reaction is 25–80°C;
[0024] Furthermore, the glove box is kept under an argon atmosphere, with water and oxygen concentrations controlled below 0.01 ppm.
[0025] Furthermore, the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared by the method of the present invention has a thickness of 10-200 μm.
[0026] On the other hand, the present invention provides a solid-state lithium battery comprising a positive electrode material, a negative electrode material, and a zeolite imidazole ester framework-ionic liquid composite gel electrolyte material prepared by the above method.
[0027] The cathode material is selected from lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and nickel-cobalt-manganese ternary materials, preferably lithium iron phosphate.
[0028] The negative electrode material is lithium metal.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] (1) The zeolite imidazole ester framework-ionic liquid composite gel electrolyte based on ZIF-90@PDA provided by this invention provides a stable three-dimensional open solid framework that can constrain the migration of large-volume cations and anions, while the size of lithium ions is only a few times smaller. It can move freely, thus exhibiting excellent electrochemical performance, with a flux of 2.98 × 10⁻⁶ at 30℃. -4 S·cm -1 The ionic conductivity is 0.43 and the lithium-ion transfer number is 0.43.
[0031] (2) The zeolite imidazole ester framework-ionic liquid composite gel electrolyte provided by this invention has improved non-flammability and electrochemical stability of the electrolyte by the ionic liquid, exhibiting a wide electrochemical window of 5.0V. At the same time, when the in-situ click reaction is applied to solid-state lithium batteries, there is good interfacial compatibility between the electrode material and the electrolyte, which inhibits the formation of lithium dendrites and exhibits excellent cycle performance and rate performance.
[0032] (3) The click reaction conditions in this invention are mild and do not require harsh conditions of anhydrous and oxygen-free environments; the preparation method provided by this invention is simple, green and environmentally friendly, and easy to scale up. Attached Figure Description
[0033] Figure 1 The images show the XRD patterns of ZIF-90 and ZIF-90@PDA prepared in Example 1.
[0034] Figure 2 This is a cross-sectional SEM image of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1.
[0035] Figure 3 The diagram shows the ionic conductivity of the zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte prepared in Example 1 at different temperatures.
[0036] Figure 4 The image shows the LSV diagram of the zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte prepared in Example 1.
[0037] Figure 5 The graph shows the lithium-ion transfer rate of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1; the left graph is the current-time graph under DC polarization, and the right graph is the impedance graph before and after polarization.
[0038] Figure 6 The first-week charge-discharge curve of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1 for use in a lithium metal solid-state battery at a rate of 0.5C.
[0039] Figure 7 The cycling performance curve of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1 for lithium metal solid-state batteries at a rate of 0.5C is shown. Detailed Implementation
[0040] The technical solution of the present invention will be further described in detail below through embodiments.
[0041] Unless otherwise specified, all raw materials and reagents used in this invention are from the conventional market.
[0042] The composite gel electrolyte prepared in this invention consists of a polydopamine-modified zeolite imidazole ester backbone (ZIF-90@PDA), a lithium salt, an ionic liquid, fluoroethylene carbonate, and a polymer network formed by a click reaction. ZIF-90@PDA is cast onto the electrode as a support layer, and the lithium salt is dissolved in a mixed precursor solution. The composite gel electrolyte is formed through an in-situ click reaction inside the battery. The addition of the ionic liquid endows the composite gel electrolyte with good thermal stability and safety performance. The composite gel electrolyte of this invention can provide 2.98 × 10⁻⁶ ppm. -4 S·cm -1 Its room-temperature ionic and electronic conductivity, wide electrochemical window, and high ion mobility number make it suitable for use in quasi-solid-state lithium battery systems, resulting in high battery capacity and good cycle stability.
[0043] Example 1
[0044] Preparation of zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte ZIF-90@PDA:
[0045] 1. Preparation of ZIF-90
[0046] 1.29 g of zinc nitrate hexahydrate was dissolved in 50 mL of tert-butanol to obtain solution A; 1.92 g of imidazole-2-carboxaldehyde and 2.00 g of polyvinylpyrrolidone were dissolved in 50 mL of water to obtain solution B; solution A and solution B were mixed and stirred for 1 h, and the yellow precipitate was washed three times with methanol, centrifuged, and dried under vacuum at 60 °C for 12 h to obtain ZIF-90.
[0047] 2. Preparation of ZIF-90@PDA
[0048] 1.00 g of ZIF-90 powder was dispersed in 50 mL of tris(hydroxymethyl)aminomethane buffer (pH = 8.5) and sonicated. 0.05 g of dopamine hydrochloride was added and stirred for 12 h. The mixture was then washed three times with water, centrifuged, and vacuum dried at 60 °C for 12 h to obtain ZIF-90@PDA.
[0049] 3. Electrode preparation
[0050] 0.08g of lithium iron phosphate, 0.01g of carbon powder (Super P), and 0.01g of polyvinylidene fluoride were dispersed in an appropriate amount of N-methylpyrrolidone, mixed evenly, and coated onto carbon-coated aluminum foil. The mixture was then vacuum dried at 80°C for 12 hours to obtain the lithium iron phosphate electrode sheet.
[0051] 4. Preparation of ZIF-90@PDA composite gel electrolyte
[0052] 0.08 g of ZIF-90@PDA and 0.02 g of polyvinylidene fluoride-hexafluoropropylene were dispersed in an appropriate amount of N-methylpyrrolidone. After stirring in a homogenizer for 20 min, the mixture was coated onto an electrode sheet and vacuum dried at 80 °C for 12 h to obtain a support layer composite electrode sheet, which was then cut into circular pieces with a diameter of 14 mm. In a glove box, 0.26 g of lithium bis(trifluoromethanesulfonyl)imide, 0.72 g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 0.18 g of fluoroethylene carbonate, 0.10 g of polyethylene glycol diacrylate, 0.02 g of pentaerythritol tetra(thioglycolic acid) ester, and 0.001 g of azobisisobutyronitrile were mixed evenly and injected onto the support layer to assemble the battery. The battery was placed in a 60 °C oven and allowed to stand for 1 h to complete the click reaction, thus obtaining the ZIF-90@PDA composite gel electrolyte. The electrolyte membrane has a thickness of 60 μm, and electrochemical testing showed that its conductivity at 30 °C was 2.98 × 10⁻⁶. -4 S·cm -1 The lithium-ion transference number is 0.43, and the electrochemical window is 5.0 V.
[0053] in, Figure 1 The images show the XRD patterns of ZIF-90 and ZIF-90@PDA prepared in Example 1. Figure 2 This is a cross-sectional SEM image of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1. Figure 3 The diagram shows the ionic conductivity of the zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte prepared in Example 1 at different temperatures. Figure 4 The image shows the LSV diagram of the zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte prepared in Example 1. Figure 5 The graph shows the lithium-ion transfer rate of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1; the left graph is the current-time graph under DC polarization, and the right graph is the impedance graph before and after polarization. Figure 6 The first-week charge-discharge curve of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1 for use in a lithium metal solid-state battery at a rate of 0.5C. Figure 7 The cycling performance curve of the zeolite imidazole ester framework-ionic liquid composite gel electrolyte prepared in Example 1 for lithium metal solid-state batteries at a rate of 0.5C is shown.
[0054] Example 2
[0055] Preparation of ZIF-90, a zeolite imidazole ester framework-ionic liquid composite gel electrolyte:
[0056] Example 2 provides a method for preparing a ZIF-90-based composite gel electrolyte membrane. The difference from Example 1 is that the ZIF-90 was not modified with polydopamine; the remaining steps are the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness is 100 μm, and electrochemical testing showed a conductivity of 1.90 × 10⁻⁶ at 30 °C. -4 S·cm -1 The lithium-ion transference number is 0.41, and the electrochemical window is 4.9V.
[0057] Example 3
[0058] Preparation of zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte ZIF-90@PDA-2:
[0059] Example 3 provides a method for preparing a composite gel electrolyte membrane based on ZIF-90@PDA. Compared to Example 1, the difference lies in that 2.58 g of zinc nitrate hexahydrate is dissolved in 50 mL of tert-butanol in solution A, and solution A is mixed with solution B and stirred for 0.25 h. The remaining steps are the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness is 150 μm, and electrochemical testing shows a conductivity of 2.18 × 10⁻⁶ at 30 °C. -4 S·cm -1 The lithium-ion transference number is 0.35, and the electrochemical window is 4.9V.
[0060] Example 4
[0061] Preparation of zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte ZIF-90@PDA-3:
[0062] Example 4 provides a method for preparing a composite gel electrolyte membrane based on ZIF-90@PDA. Compared to Example 1, the difference lies in that 3.84 g of imidazole-2-carboxaldehyde and 2.00 g of polyvinylpyrrolidone were dissolved in 50 mL of water in solution B. Solution A and solution B were mixed and stirred for 6 h. The remaining steps were the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness was 180 μm, and electrochemical testing showed a conductivity of 2.03 × 10⁻⁶ at 30 °C. -4 S·cm -1 The lithium-ion transference number is 0.37, and the electrochemical window is 5.0 V.
[0063] Example 5
[0064] Preparation of zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte ZIF-90@PDA-4:
[0065] Example 5 provides a method for preparing a ZIF-90@PDA composite gel electrolyte membrane. Compared to Example 1, the difference lies in the following steps: 2.00 g of ZIF-90 powder is dispersed in 50 mL of tris(hydroxymethyl)aminomethane buffer (pH = 8.2) and sonicated; 0.25 g of dopamine hydrochloride is added; and the mixture is stirred for 24 h. The remaining steps are the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness is 20 μm, and electrochemical testing shows a conductivity of 2.58 × 10⁻⁶ at 30 °C. -4 S·cm -1 The lithium-ion transference number is 0.31, and the electrochemical window is 5.1V.
[0066] Example 6
[0067] Preparation of zeolite imidazole ester skeleton-ionic liquid composite gel electrolyte ZIF-90@PDA-5:
[0068] Example 6 provides a method for preparing a composite gel electrolyte membrane based on ZIF-90@PDA. Compared to Example 1, the difference lies in the following: 0.39 g of lithium bis(trifluoromethanesulfonyl)imide, 0.72 g of N-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 0.18 g of fluoroethylene carbonate, 0.10 g of polyethylene glycol diacrylate, 0.02 g of pentaerythritol tetra(thioglycolic acid) ester, and 0.002 g of azobisisobutyronitrile are mixed uniformly and injected onto a support layer to assemble the battery. The battery is placed in a 50°C oven and left to stand for 6 hours to allow the click reaction to complete. The remaining steps are the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness is 40 μm, and electrochemical testing shows a conductivity of 2.54 × 10⁻⁶ at 30°C. -4 S·cm -1 The lithium-ion transference number is 0.38, and the electrochemical window is 4.8V.
[0069] Comparative Example 1
[0070] Preparation of ionic liquid gel electrolytes:
[0071] Comparative Example 1 provides a method for preparing a gel electrolyte membrane based on a polypropylene (PP) membrane. The difference from Example 1 is the use of a PP membrane (Celgard 2400) as the support layer; the remaining steps are the same as in Example 1 and will not be repeated here. The electrolyte membrane thickness is 40 μm, and electrochemical testing showed a conductivity of 2.66 × 10⁻⁶ at 30 °C. -5 S·cm -1 The lithium-ion transference number is 0.26, and the electrochemical window is 4.8V.
[0072] Table 1 Performance Test of Lithium Iron Phosphate Batteries
[0073]
[0074]
[0075] As shown in Table 1 above, the lithium battery prepared using the zeolite imidazole ester framework-ionic liquid composite gel electrolyte ZIF-90@PDA exhibits significantly higher initial capacity and capacity retention than batteries using other methods. The nanoporous structure of ZIF-90 restricts the movement of larger cations and anions, forming rapid lithium-ion transport channels and accelerating lithium-ion migration within the electrolyte. The exceptional adhesive properties of polydopamine enable ZIF-90 particles to bond with the polymer, while the non-flammable nature of the ionic liquid ensures battery safety. The thiol-ene reaction forms a three-dimensional network structure, enhancing the electrolyte's mechanical strength. This invention employs an in-situ preparation method, which is simple to operate under mild conditions. The precursor solution can penetrate the electrode gaps, improving the interfacial contact between the electrode and the electrolyte.
[0076] The present invention has been described in detail above with reference to its general description and specific embodiments. Modifications or arbitrary combinations can be made without departing from the core principles of the invention, and this is not intended to limit the scope of protection of the invention. Therefore, all related modifications made based on this description fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a zeolite imidazole ester framework-ionic liquid composite gel electrolyte, characterized in that, Includes the following steps: S1. Preparation of ZIF-90: Zinc salt was dissolved in solvent 1 to obtain solution A; imidazole-2-formaldehyde was dissolved in solvent 2 to obtain solution B; solution A and solution B were mixed, stirred, and the pale yellow precipitate was washed, centrifuged, and vacuum dried to obtain ZIF-90 powder; Solvent 1 is tert-butanol; Solvent 2 is one of methanol, water, and N,N-dimethylformamide; S2. Preparation of ZIF-90@PDA: ZIF-90 powder was dispersed in an alkaline solvent and ultrasonically treated. 1 wt% to 15 wt% of dopamine hydrochloride was added and stirred for 5 to 24 hours. Then, the mixture was washed, centrifuged and dried to obtain the modified nanofiller ZIF-90@PDA. S3. Preparation of zeolite imidazole ester framework-ionic liquid composite gel electrolyte: ZIF-90@PDA and polymer were dispersed in an appropriate amount of solvent, stirred evenly, and then coated onto the electrode sheet and vacuum dried to obtain a support layer; in a glove box, lithium salt, ionic liquid, fluoroethylene carbonate, click reaction precursor and initiator were mixed evenly and dropped onto the support layer to assemble the battery; the battery was placed in an oven and allowed to stand to complete the click reaction, thus obtaining the zeolite imidazole ester framework-ionic liquid composite gel electrolyte; The click reaction precursor is a polyethylene glycol monomer with unsaturated double bonds and a thiol with two or more mercapto groups.
2. The method for preparing the zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 1, characterized in that, In step S1: The zinc salt is one of zinc nitrate hexahydrate or zinc acetate dihydrate; The molar ratio of the zinc salt to imidazole-2-carboxaldehyde is 1:1 to 10; The stirring time is 0.25 to 24 hours.
3. The method for preparing the zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 1, characterized in that, In step S2: the mass concentration of the ZIF-90 solution obtained by dispersing ZIF-90 powder in an alkaline solvent is 10-50 mg / mL; the pH value of the alkaline solvent is 8.0-8.
6.
4. The method for preparing the zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 1, characterized in that, In step S3: The polymer is one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, and polyvinyl alcohol; The lithium salt is one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, and lithium bis(fluorosulfonyl)imide; The ionic liquid is one or more combinations of N-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hexylimidazolium trifluoromethanesulfonate, and 1-ethyl-3-methylimidazolium hexafluorophosphate.
5. The method for preparing the zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 1, characterized in that, In step S3: The mass ratio of ZIF-90@PDA to polymer is 1:(0.1~0.25). The concentration of lithium salt in the mixture formed by uniformly mixing lithium salt, ionic liquid, fluoroethylene carbonate, click reaction precursor and initiator is 0.5–2.0 mol / L; The temperature of the click reaction is 25–80°C.
6. A zeolite imidazole ester framework-ionic liquid composite gel electrolyte, characterized in that: It is obtained by the preparation method according to any one of claims 1 to 5.
7. The zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 6, characterized in that, The thickness of the electrolyte is 10–200 μm.
8. A lithium battery with a zeolite imidazole ester framework-ionic liquid composite gel electrolyte, characterized in that, The lithium battery includes a positive electrode, a negative electrode, and a zeolite imidazole ester framework-ionic liquid composite gel electrolyte according to claim 6.
Citation Information
Patent Citations
Molecular sieve imidazole framework doped polymer solid electrolyte and preparation method thereof
CN114709475A
Sulfur-containing polymer gel electrolyte and preparation method and application thereof
CN115133119A