Perovskite layer and its preparation method, perovskite solar cell and its preparation method

By employing a high-porosity first lead iodide layer and a dense second lead iodide layer in the perovskite layer, the problem of excess lead iodide was solved, improving the charge transport and stability of the perovskite solar cell and enhancing its efficiency.

CN116997235BActive Publication Date: 2026-11-10TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310838032.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2026-11-10
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

In existing perovskite solar cells, lead iodide tends to remain during the fabrication of the perovskite layer, which hinders charge transport and results in low cell efficiency.

Method used

A first lead iodide layer with a higher porosity than the second lead iodide layer is used as the bottom layer. The loose first lead iodide layer is located at the bottom, and the dense second lead iodide layer is located at the top. By controlling the thickness and preparation method, the cationic solution is ensured to diffuse and react fully, thereby reducing the amount of lead iodide remaining.

Benefits of technology

It effectively reduces the residual lead iodide at the bottom of the perovskite layer, improves the stability and efficiency of the battery, avoids collapse, and enhances the battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116997235B_ABST
    Figure CN116997235B_ABST
Patent Text Reader

Abstract

This application discloses a perovskite layer and its preparation method, as well as a perovskite solar cell and its preparation method. The perovskite layer is prepared by reacting a lead iodide framework layer with a cation solution. The lead iodide framework layer includes a first lead iodide layer deposited on a substrate and a second lead iodide layer deposited on the first lead iodide layer. The porosity of the first lead iodide layer is higher than that of the second lead iodide layer. The perovskite layer of this application is less prone to lead iodide residue, exhibits better shape retention, is less prone to collapse, and significantly improves cell efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solar cells, and more particularly to a perovskite layer and its preparation method, and a perovskite solar cell and its preparation method. Background Technology

[0002] Currently, the most suitable method for manufacturing perovskite solar cells for industrial production involves a combination of vapor deposition and spin coating to prepare the perovskite layer. This involves vacuum-depositing a lead iodide framework layer on a substrate using vapor deposition, followed by spin-coating a cationic solution onto the lead iodide framework layer. The cationic solution reacts with the lead iodide to form the perovskite layer. However, the perovskite layer prepared using this combination method often results in residual lead iodide at the bottom. This residual lead iodide hinders the transfer of charge at the perovskite layer interface, leading to lower cell efficiency. Summary of the Invention

[0003] To address the issue of lead iodide residue easily occurring in perovskite layers, this application discloses a perovskite layer and its preparation method, as well as a perovskite solar cell and its preparation method.

[0004] In one aspect, this application provides a perovskite layer.

[0005] The perovskite layer is used in solar cells. The perovskite layer is prepared by reacting a lead iodide framework layer with a cation solution. The lead iodide framework layer includes a first lead iodide layer deposited on a substrate and a second lead iodide layer deposited on the first lead iodide layer. The porosity of the first lead iodide layer is higher than that of the second lead iodide layer.

[0006] As an optional implementation, in the embodiments of this application, the thickness of the perovskite layer is 450nm to 550nm, the thickness of the lead iodide framework layer is 300nm to 450nm, and the thickness of the first lead iodide layer is 50nm to 150nm.

[0007] As an optional implementation, in the embodiments of this application, the first lead iodide layer is obtained by solution treatment or vapor deposition, and the second lead iodide layer is obtained by vapor deposition.

[0008] As an optional implementation, in the embodiments of this application, the solution for preparing the first lead iodide layer is a lead iodide precursor solution, and the concentration of the lead iodide precursor solution is 0.5 mol / L to 1.3 mol / L.

[0009] As an optional implementation, in the embodiments of this application, the solute of the lead iodide precursor solution includes lead iodide and cesium bromide, and the mass ratio of lead iodide to cesium bromide is 5-10:1; and / or,

[0010] The solvent of the lead iodide precursor solution includes N,N-dimethylformamide and dimethyl sulfoxide, wherein the mass ratio of N,N-dimethylformamide to dimethyl sulfoxide is 4 to 9:1.

[0011] As an optional implementation, in the embodiments of this application, the solute of the cation solution includes at least two of the following: formamidine iodoformidium, formamidine bromoformidium, methyl bromide, and methyl chloroformide; and / or, the solvent of the cation solution is one or a combination of anhydrous ethanol and isopropanol.

[0012] As an optional implementation, in the embodiments of this application, when the cation solution contains the formamidinium iodoformidium, the formamidinium bromoformidium, the methyl bromide, and the methyl bromide, the concentration of the formamidinium iodoformidium is 0.3 mol / L to 0.6 mol / L, the concentration of the formamidinium bromoformidium is 0.05 mol / L to 0.2 mol / L, the concentration of the methyl bromide is 0.1 mol / L to 0.2 mol / L, and the concentration of the methyl bromide is 0.05 mol / L to 0.15 mol / L.

[0013] Secondly, this application provides a method for preparing a perovskite layer as described in the first aspect.

[0014] The method for preparing this perovskite layer includes the following steps:

[0015] Preparation of lead iodide framework layer: A first lead iodide layer is prepared on a substrate, and a second lead iodide layer is prepared on the first lead iodide layer, wherein the porosity of the first lead iodide layer is higher than that of the second lead iodide layer;

[0016] Preparation of the perovskite layer: A cationic solution is spin-coated onto the second lead iodide layer, and after annealing, the perovskite layer as described in the first aspect is obtained.

[0017] As an optional implementation, in the embodiments of this application, the first lead iodide layer is prepared by solution method or vapor deposition method.

[0018] As an optional implementation, in the embodiments of this application, the method for preparing the first lead iodide layer using the solution method includes: depositing a lead iodide precursor solution by spraying or spin coating, followed by annealing treatment. The spraying method is as follows: under an inert atmosphere, a lead iodide precursor solution at a temperature of 60℃~70℃ is sprayed onto the substrate, the spraying speed is 100mm / s~200mm / s, and the spraying time is 30s~60s.

[0019] The spin coating method is as follows: Under an inert atmosphere, a lead iodide precursor solution at a temperature of 60℃~70℃ is spin-coated onto the substrate. The spin coating speed is 5000rpm~7000rpm and the spin coating time is 30s~60s.

[0020] As an optional implementation, in the embodiments of this application, the vacuum degree for preparing the first lead iodide using the vapor deposition method is 1×10⁻⁶. -3 pa~1×10 -4 pa, transmission speed is 10mm / s~15mm / s, evaporation rate is

[0021] As an optional implementation, in the embodiments of this application, the annealing temperature of the first lead iodide layer is 60°C to 70°C, and the annealing time is 30s to 90s.

[0022] As an optional implementation, in the embodiments of this application, the second lead iodide layer is prepared by the aforementioned vapor deposition method, and the vacuum degree during the preparation of the second lead iodide layer is controlled to be 1×10⁻⁶. -3 pa~1×10 -4 pa, transmission speed is 10mm / s~15mm / s, evaporation rate is

[0023] As an optional implementation, in the embodiments of this application, the second lead iodide layer is prepared using a dual-source co-evaporation process or a triple-source co-evaporation process. The evaporation source materials of the dual-source co-evaporation process are lead iodide and cesium bromide, and the evaporation rate ratio of lead iodide to cesium bromide is 5 to 10:1. The evaporation source materials of the triple-source co-evaporation process are lead iodide, cesium bromide, and S component, and the S component is any one of lead bromide, lead chloride, cesium iodide, and cesium chloride, and the evaporation rate ratio of lead iodide, cesium bromide, and S component is 5 to 10:1:1.

[0024] As an optional implementation, in the embodiments of this application, after spin-coating the cationic solution, it is annealed at 100°C to 170°C for 15 min to 30 min under conditions of 5%RH to 40%RH.

[0025] Thirdly, this application provides a perovskite solar cell.

[0026] A perovskite solar cell includes the perovskite layer described in the first aspect or the perovskite layer prepared by the preparation method described in the second aspect.

[0027] As an optional implementation, in the embodiments of this application, the perovskite solar cell further includes a bottom cell, a composite layer, a hole transport layer, an electron transport layer, a transparent electrode layer, a positive electrode, and a negative electrode stacked sequentially. The perovskite layer is located between the hole transport layer and the electron transport layer. The positive electrode forms an ohmic contact with the transparent electrode layer, and the negative electrode forms an ohmic contact with the bottom cell.

[0028] As an optional implementation, in the embodiments of this application, the thickness of the composite layer is 20nm to 30nm; and / or, the thickness of the hole transport layer is 20nm to 30nm; and / or, the thickness of the electron transport layer is 15nm to 20nm; the thickness of the transparent electrode layer is 80nm to 120nm; and / or, the thicknesses of the positive electrode and the negative electrode are 150nm to 300nm respectively.

[0029] As an optional implementation, in the embodiments of this application, the bottom cell is a heterojunction cell; and / or, the composite layer is made of one or a combination of indium tin oxide and indium zinc oxide; and / or, the hole transport layer is made of nickel oxide; and / or, the electron transport layer is made of C. 60 ; and / or, the material of the transparent electrode layer is one or a combination of indium tin oxide and indium zinc oxide; and / or, the materials of the positive electrode and the negative electrode are any one of silver, copper and aluminum, respectively.

[0030] As an optional implementation, in the embodiments of this application, the perovskite tandem solar cell further includes a hole modification layer, the hole modification layer being located between the hole transport layer and the perovskite layer; and / or,

[0031] The perovskite tandem solar cell further includes a passivation layer, which is located between the perovskite layer and the electron transport layer, and has a thickness of 0.5 nm to 1 nm; and / or,

[0032] The perovskite tandem solar cell further includes a buffer layer, which is located between the electron transport layer and the transparent electrode layer, and has a thickness of 20 nm to 30 nm; and / or,

[0033] The perovskite tandem solar cell also includes an antireflection layer, which is located on the side of the transparent electrode layer opposite to the bottom cell and has a thickness of 100nm to 120nm.

[0034] As an optional implementation, in the embodiments of this application, the hole modification layer is made of 2PACz and Meo-2PACz; and / or, the passivation layer is made of lithium fluoride; and / or, the buffer layer is made of tin dioxide; and / or, the antireflection layer is made of magnesium fluoride or lithium fluoride.

[0035] Fourthly, this application provides a method for preparing a perovskite solar cell as described in the third aspect.

[0036] The fabrication method of this perovskite solar cell includes the following steps:

[0037] Provide a base battery;

[0038] A composite layer is prepared on the bottom battery;

[0039] A hole transport layer is prepared on the side of the composite layer away from the bottom cell.

[0040] The perovskite layer described above is prepared on the side of the hole transport layer away from the bottom cell.

[0041] An electron transport layer is prepared on the side of the perovskite layer away from the bottom cell.

[0042] A transparent electrode layer is fabricated on the side of the electron transport layer away from the bottom battery.

[0043] A positive electrode and a negative electrode are prepared to obtain the perovskite tandem solar cell.

[0044] As an optional implementation, in the embodiments of this application, a hole modification layer is prepared between the hole transport layer and the perovskite layer; and / or, a passivation film layer is prepared between the perovskite layer and the electron transport layer; and / or, a buffer layer is prepared between the electron transport layer and the transparent electrode layer; and / or, an antireflection layer is prepared on the side of the transparent electrode layer away from the bottom cell.

[0045] Compared with the prior art, the beneficial effects of this application are as follows:

[0046] In the perovskite layer provided in this application embodiment, the porosity of the first lead iodide layer is higher than that of the second lead iodide layer. It can be seen that compared with the structure of the second lead iodide layer, the structure of the first lead iodide layer is relatively loose, while the structure of the second lead iodide layer is relatively dense, and the structural stability of the second lead iodide layer is relatively high.

[0047] A relatively loosely structured first lead iodide layer is located at the bottom, while a relatively dense second lead iodide layer is located on top of the first lead iodide layer. The top second lead iodide layer reacts first with a large amount of cationic solution, and during cationic spin coating, the second lead iodide layer is not easily damaged, nor is it prone to collapse or deformation. During the subsequent annealing process, some of the cationic solution that has not reacted with the second lead iodide layer continues to diffuse and penetrate the top second lead iodide layer, entering the bottom first lead iodide layer. It then fully contacts and reacts with the relatively loosely structured first lead iodide layer, thus solving the problem of residual lead iodide at the bottom of the perovskite layer. At the same time, the cationic solution that comes into contact with the relatively loosely structured first lead iodide layer is the portion of the cationic solution that has not reacted with the second lead iodide layer. Therefore, after the cationic solution is coated, it is not easy to damage the relatively loosely structured first lead iodide layer, and the first lead iodide layer can also maintain good stability. The perovskite layer prepared in this way is less prone to residual lead iodide, has better shape retention, is not prone to collapse, and is conducive to improving battery efficiency. Attached Figure Description

[0048] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0049] Figure 1 This is a schematic diagram of the perovskite solar cell disclosed in Embodiment 1 of this application.

[0050] Figure 2 This is a surface SEM image of the first lead iodide layer prepared in Example 1 of this application.

[0051] Figure 3 This is a surface SEM image of the second lead iodide layer prepared in Example 1 of this application.

[0052] Icons: 1. Heterojunction base cell; 2. Composite layer; 3. Hole transport layer; 31. Hole modification layer; 4. Perovskite layer; 41. Passivation layer; 5. Electron transport layer; 51. Buffer layer; 6. Transparent electrode layer; 71. Positive electrode; 72. Negative electrode; 8. Antireflection layer. Detailed Implementation

[0053] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0054] The technical solution of this application will be further described below with reference to the embodiments and accompanying drawings.

[0055] In one aspect, this application provides a perovskite layer.

[0056] A perovskite layer for use in solar cells is prepared by reacting a lead iodide framework layer with a cation solution. The lead iodide framework layer includes a first lead iodide layer deposited on a substrate and a second lead iodide layer deposited on the first lead iodide layer. The porosity of the first lead iodide layer is higher than that of the second lead iodide layer.

[0057] In this application, the porosity of the first lead iodide layer is higher than that of the second lead iodide layer. It can be seen that compared with the structure of the second lead iodide layer, the structure of the first lead iodide layer is relatively loose, while the structure of the second lead iodide layer is relatively dense, and the structural stability of the second lead iodide layer is relatively high.

[0058] During the cation spin coating process, if a large amount of cation solution comes into contact with the relatively loose first lead iodide layer, and the spin coating operation can easily bring additional pressure to the first lead iodide layer, the relatively loose first lead iodide layer is easily damaged, leading to the collapse of the perovskite layer.

[0059] A relatively loosely structured first lead iodide layer is located at the bottom, while a relatively dense second lead iodide layer is located on top of the first lead iodide layer. The top second lead iodide layer reacts first with a large amount of cationic solution, and during cationic spin coating, the second lead iodide layer is not easily damaged, nor is it prone to collapse or deformation. During the subsequent annealing process, some of the cationic solution that has not reacted with the second lead iodide layer continues to diffuse and penetrate through the top second lead iodide layer, entering the bottom first lead iodide layer. It then fully contacts and reacts with the relatively loosely structured first lead iodide layer, thus solving the problem of residual lead iodide at the bottom of the perovskite layer. At the same time, the cationic solution that comes into contact with the relatively loosely structured first lead iodide layer at the bottom is the portion of the cationic solution that has not reacted with the second lead iodide. Therefore, after the cationic solution is coated, it is not easy to damage the relatively loosely structured first lead iodide layer, and the first lead iodide layer can also maintain good stability. The perovskite layer prepared in this way is less prone to residual lead iodide, has better shape retention, is not prone to collapse, and is conducive to improving battery efficiency.

[0060] In some embodiments, the thickness of the perovskite layer is 450 nm to 550 nm, the thickness of the lead iodide framework layer is 300 nm to 450 nm, and the thickness of the first lead iodide layer is 50 nm to 150 nm.

[0061] The thickness of the second lead iodide layer is the difference between the thickness of the lead iodide framework layer and the thickness of the first lead iodide framework layer. By controlling the thickness of the first and second lead iodide layers, the cation solution can penetrate the second lead iodide layer of the aforementioned thickness and effectively diffuse into the bottom first lead iodide layer, fully contacting and reacting with the relatively loosely structured first lead iodide layer, thereby significantly reducing the amount of lead iodide remaining in the perovskite layer.

[0062] The smaller the thickness of the first lead iodide layer, the larger the corresponding thickness of the second lead iodide layer. When the thickness of the first lead iodide layer is too small, the cation solution cannot effectively diffuse through the relatively dense second lead iodide layer, making it difficult for the cation solution to fully react with the relatively loose first lead iodide layer at the bottom. As a result, the lead iodide in the first lead iodide layer does not react completely, leaving a large amount remaining.

[0063] The greater the thickness of the first lead iodide layer, the smaller the corresponding thickness of the second lead iodide layer. When the thickness of the first lead iodide layer is too large, its structure is relatively loose, which is not conducive to maintaining good stability of the overall lead iodide framework layer. When this perovskite layer is applied to silicon substrate solar cells with a pyramid structure, the first lead iodide layer cannot achieve conformal and complete coverage on the silicon substrate. During the subsequent spin coating process with cation solution, the lead iodide framework layer at the top of the pyramid is prone to collapse, leading to reduced solar cell efficiency or short circuits.

[0064] In some embodiments, the first lead iodide layer is obtained by solution treatment or vapor deposition, and the second lead iodide layer is obtained by vapor deposition.

[0065] The first lead iodide layer is prepared by solution method, such as by spin coating or spray coating to deposit the lead iodide precursor solution on the substrate. The resulting first lead iodide layer has high porosity and a high degree of loose structure.

[0066] By depositing the first or second lead iodide layer using the vapor deposition method, the first lead iodide layer with higher porosity and a looser structure, or the second lead iodide layer with lower porosity and a denser structure, can be obtained by adjusting the process parameters during the preparation of the lead iodide layer.

[0067] In some embodiments, the solution used to prepare the first lead iodide layer is a lead iodide precursor solution with a concentration of 0.5 mol / L to 1.3 mol / L.

[0068] The concentration of the lead iodide precursor solution has a significant impact on the thickness of the first lead iodide layer. The thickness of the first lead iodide layer obtained using the lead iodide solution at the concentration mentioned above is relatively suitable. If the lead iodide solution concentration is too high, the thickness of the first lead iodide layer will be too high; if the concentration is too low, the thickness will be too low. It is evident that both excessively high and low concentrations of the lead iodide precursor solution can easily lead to significant deviations in the thickness of the perovskite layer, which is detrimental to the overall thickness control of the lead iodide framework layer and adversely affects the light absorption of the perovskite layer.

[0069] In some embodiments, the solute of the lead iodide precursor solution includes lead iodide and cesium bromide, with a mass ratio of lead iodide to cesium bromide of 5 to 10:1; and / or, the solvent of the lead iodide precursor solution includes N,N-dimethylformamide and dimethyl sulfoxide, with a mass ratio of N,N-dimethylformamide to dimethyl sulfoxide of 4 to 9:1.

[0070] By controlling the mass ratio of lead iodide to cesium bromide to 5–10:1, a certain amount of cesium bromide is doped into the lead iodide precursor solution, which is beneficial to further improve the porosity and structural looseness of the first lead iodide layer. The cationic solution is in full contact with the first lead iodide layer with higher porosity and looser structure, resulting in better reaction effect. This is conducive to the full reaction of lead iodide, reduces the residual lead iodide reaction, and thus produces a perovskite layer with better crystal quality, better interfacial contact performance and excellent electron transport performance.

[0071] The above mass ratio of N,N-dimethylformamide and dimethyl sulfoxide, used as solvents for the lead iodide precursor solution, provides good dissolution and stable dispersion of lead iodide and cesium bromide, and has a wide viscosity adjustment range, which facilitates subsequent spin coating or spray coating processes.

[0072] In some embodiments, the solute of the cation solution comprises at least two of formamidine iodoformidium, formamidine bromoformidium, methyl bromide, and methyl chloroformide; and / or, the solvent of the cation solution is one or a combination of anhydrous ethanol and isopropanol.

[0073] When the cationic solution contains formamidinium iodoformidium, formamidinium bromide, methyl bromide, and methyl bromide, the concentration of formamidinium iodoformidium is 0.3 mol / L to 0.6 mol / L, the concentration of formamidinium bromide is 0.05 mol / L to 0.2 mol / L, the concentration of methyl bromide is 0.1 mol / L to 0.2 mol / L, and the concentration of methyl bromide is 0.05 mol / L to 0.15 mol / L.

[0074] Iodoformamidine, bromoformamidine, bromomethylamine, and chloromethylamine are all common components in the preparation of cationic solutions. By controlling the above components and their concentrations in the cationic solution, the cationic solution can achieve better fluidity. Furthermore, the cationic solution has a better band gap matching effect with the first lead iodide layer and the second lead iodide layer, which is beneficial for preparing perovskite layers with higher crystal quality.

[0075] Furthermore, the cationic solution partially reacts with the relatively dense second lead iodide layer at the top, while the remaining portion diffuses through the second lead iodide layer and enters the bottom, where it fully contacts and reacts with the relatively loose first lead iodide layer, effectively reducing the amount of lead iodide remaining at the bottom.

[0076] Anhydrous ethanol, isopropanol, or a mixture of both can be used as solvents for the above-mentioned cation solutions. When anhydrous ethanol and isopropanol are mixed and used together as solvents, the polarity of the cation solution can be adjusted, thereby improving the film quality of the perovskite layer.

[0077] Secondly, this application provides a method for preparing a perovskite layer as described in the first aspect.

[0078] The method for preparing the perovskite layer includes the following steps:

[0079] Preparation of lead iodide framework layer: A first lead iodide layer is prepared on the substrate, and a second lead iodide layer is prepared on the first lead iodide layer. The porosity of the first lead iodide layer is higher than that of the second lead iodide layer.

[0080] Preparation of perovskite layer: A cationic solution is spin-coated onto the second lead iodide layer, and the perovskite layer is obtained after annealing.

[0081] The cationic solution is first spin-coated onto the second lead iodide layer. The second lead iodide layer has low porosity, high density, and relatively stable structure. Therefore, after spin-coating with the cationic solution, the second lead iodide layer is not prone to collapse and can maintain good stability. Part of the cationic solution reacts with the second lead iodide layer, while the remainder diffuses into the first lead iodide layer, which has higher porosity, through the pores of the second lead iodide layer. Since the first lead iodide layer has higher porosity, the cationic solution can enter more easily, which is conducive to the full contact and reaction between the lead iodide at the bottom and the cationic solution, thereby reducing the residual lead iodide reaction and improving the interfacial contact and charge transport effect of the perovskite layer.

[0082] In some embodiments, the first lead iodide layer is prepared by solution deposition or vapor deposition.

[0083] The method for preparing the first lead iodide layer using a solution method includes spraying or spin coating, followed by annealing after depositing the lead iodide precursor solution using spraying or spin coating.

[0084] The spraying method is as follows: Under an inert atmosphere, a lead iodide precursor solution with a temperature of 60℃~70℃ is sprayed onto the substrate at a spraying speed of 100mm / s~200mm / s and a spraying time of 30s~60s.

[0085] The spin coating method is as follows: Under an inert atmosphere, a lead iodide precursor solution at a temperature of 60℃~70℃ is spin-coated onto the substrate at a spin speed of 5000rpm~7000rpm and a spin time of 30s~60s.

[0086] Both solution deposition and vapor deposition methods can be used to prepare a first lead iodide layer with high porosity and a relatively loose structure. In particular, controlling the speed and time of preparation using spraying and spin coating methods is beneficial for producing a first lead iodide layer with better uniformity, higher crystal quality, a looser structure, and higher porosity.

[0087] Furthermore, during the spraying or spin coating process, the temperature of the lead iodide precursor solution is controlled at 60℃~70℃. Lead iodide is less likely to precipitate due to excessively low temperature, thus maintaining the dispersion stability of the lead iodide precursor solution and obtaining a first lead iodide layer with high porosity and relatively loose structure.

[0088] In some embodiments, when the first lead iodide layer is prepared by vapor deposition, the vacuum level is controlled to be 1×10⁻⁶. -3 pa~1×10 -4 pa, the transmission speed is 10mm / s~15mm / s, and the evaporation rate is

[0089] The evaporation rate affects the density of the lead iodide film; the higher the evaporation rate, the more porous and less porous the lead iodide film. Therefore, by controlling the evaporation rate during the evaporation process, the thickness of the lead iodide film can be controlled, resulting in a first lead iodide layer with higher porosity and greater looseness, and a second lead iodide layer with lower porosity and greater density.

[0090] In some embodiments, the annealing temperature of the first lead iodide layer is 60°C to 70°C, and the annealing time is 30s to 90s.

[0091] At the above-mentioned annealing temperature, the solvent in the first lead iodide layer can be removed, which promotes the drying degree of the lead iodide framework layer. This facilitates the diffusion of more cationic solution into the bottom first lead iodide layer and its reaction with the relatively loosely structured lead iodide, thereby reducing the reaction residue of lead iodide and improving the interfacial contact performance and electron transport capability of the perovskite layer.

[0092] In some embodiments, the second lead iodide layer is prepared by vapor deposition, and the vacuum degree is controlled to be 1×10⁻⁶ when preparing the second lead iodide layer by vapor deposition. -3 pa~1×10 -4 pa, transmission speed is 10mm / s~15mm / s, evaporation rate is

[0093] When the first lead iodide layer is prepared by vapor deposition, the deposition rate is: Its evaporation rate is relatively fast, resulting in a relatively loose structure in the first lead iodide layer, while the deposition rate of the second lead iodide layer is... The second lead iodide layer has a slower evaporation rate, resulting in a relatively dense structure and strong structural stability.

[0094] The process can employ either a dual-source co-evaporation process or a triple-source co-evaporation process. In the dual-source co-evaporation process, the evaporation source materials are lead iodide and cesium bromide, with an evaporation rate ratio of 5 to 10:1. In the triple-source co-evaporation process, the evaporation source materials are lead iodide, cesium bromide, and an S component, where the S component is any one of lead bromide, lead chloride, cesium iodide, or cesium chloride, and the evaporation rate ratio of lead iodide, cesium bromide, and the S component is 5 to 10:1:1.

[0095] Both dual-source and triple-source co-evaporation processes can be used to prepare the second lead iodide layer. During production, users can adjust the composition and proportion of the lead iodide layer according to the performance requirements of different types of solar cells, thus preparing various perovskite layers with different compositions and proportions to better adapt to different types of solar cells and improve their performance.

[0096] In some embodiments, after spin-coating the cationic solution, it is annealed at 100°C to 170°C for 15 min to 30 min under conditions of 5%RH to 40%RH.

[0097] During the annealing process under the above conditions, the spin-coated cations react completely with the relatively dense second lead iodide layer at the top, and some of the cation solution can diffuse to the bottom and react with the relatively loose first lead iodide layer to form a perovskite layer with better crystallization effect.

[0098] Thirdly, this application provides a perovskite solar cell.

[0099] The perovskite solar cell includes a perovskite layer prepared by the first aspect or a perovskite layer prepared by the second aspect.

[0100] The perovskite layer structure prepared in this application exhibits high stability and is not prone to collapse, demonstrating excellent shape retention. It is suitable as a light-absorbing layer for different types of solar cells, such as single-junction perovskite solar cells or tandem perovskite solar cells. When using a silicon substrate with a pyramidal textured surface for a tandem perovskite solar cell, other films prepared on top of the silicon substrate cell must maintain the same pyramidal shape to ensure better adhesion between the other films and the silicon substrate cell. By using this perovskite layer as a light-absorbing layer on a silicon substrate cell, the perovskite layer maintains a superior pyramidal textured surface, thereby ensuring excellent adhesion and interfacial transport performance with the other films on the silicon substrate cell, ultimately improving the energy conversion efficiency of the solar cell.

[0101] In some embodiments, the perovskite solar cell includes a bottom cell, a composite layer, a hole transport layer, a perovskite layer, an electron transport layer, and a transparent electrode layer stacked sequentially. The perovskite layer also includes a positive electrode and a negative electrode. The positive electrode forms an ohmic contact with the transparent electrode layer, and the negative electrode forms an ohmic contact with the bottom cell.

[0102] In some embodiments, the thickness of the composite layer is 20 nm to 30 nm; and / or, the thickness of the hole transport layer is 20 nm to 30 nm; and / or, the thickness of the electron transport layer is 15 nm to 20 nm; the thickness of the transparent electrode layer is 80 nm to 120 nm; and / or, the thicknesses of the positive electrode and the negative electrode are 150 nm to 300 nm, respectively.

[0103] In some embodiments, the bottom cell is a heterojunction cell; and / or, the composite layer is made of one or a combination of indium tin oxide and indium zinc oxide; and / or, the hole transport layer is made of nickel oxide; and / or, the electron transport layer is made of C. 60 ; and / or, the material of the transparent electrode layer is one or a combination of indium tin oxide and indium zinc oxide; and / or, the materials of the positive electrode and the negative electrode are any one of silver, copper and aluminum, respectively.

[0104] In some embodiments, the perovskite tandem solar cell further includes a hole-modifying layer located between the hole transport layer and the perovskite layer; and / or,

[0105] The perovskite tandem solar cell also includes a passivation layer, located between the perovskite layer and the electron transport layer, with a thickness of 0.5 nm to 1 nm; and / or,

[0106] Perovskite tandem solar cells also include a buffer layer, located between the electron transport layer and the transparent electrode layer, with a thickness of 20 nm to 30 nm; and / or,

[0107] The perovskite tandem solar cell also includes an antireflection layer, which is located on the side of the transparent electrode layer away from the bottom cell and has a thickness of 100nm to 120nm.

[0108] In some embodiments, the hole-modifying layer is made of 2PACz (CAS No. 20999-38-6) and Meo-2PACz (CAS No. 2377770-18-6); and / or, the passivation layer is made of lithium fluoride; and / or, the buffer layer is made of tin dioxide; and / or, the antireflection layer is made of magnesium fluoride or lithium fluoride.

[0109] Fourthly, this application provides a method for fabricating a perovskite solar cell as described in the third aspect, the perovskite solar cell comprising the following steps:

[0110] Provide a base battery;

[0111] A composite layer is fabricated on the bottom battery;

[0112] A hole transport layer is prepared on the side of the composite layer away from the bottom cell;

[0113] The perovskite layer described above was prepared on the side of the hole transport layer away from the bottom cell.

[0114] An electron transport layer is fabricated on the side of the perovskite layer away from the bottom cell;

[0115] A transparent electrode layer is fabricated on the side of the electron transport layer away from the bottom cell.

[0116] Positive and negative electrodes were prepared to obtain a perovskite tandem solar cell.

[0117] In some embodiments, a hole-modifying layer is prepared between the hole transport layer and the perovskite layer; and / or, a passivation film is prepared between the perovskite layer and the electron transport layer; and / or, a buffer layer is prepared between the electron transport layer and the transparent electrode layer; and / or, an antireflection layer is prepared on the side of the transparent electrode layer away from the bottom cell.

[0118] The technical solutions of this application will be further described below with reference to more specific embodiments and accompanying drawings.

[0119] Example 1

[0120] This application provides a perovskite solar cell, referring to... Figure 1 The perovskite solar cell includes a heterojunction base cell 1, a composite layer 2, a hole transport layer 3, a hole modification layer 31, a perovskite layer 4, a passivation layer 41, an electron transport layer 5, a buffer layer 51, a transparent electrode layer 6, and an antireflection layer 8, which are stacked sequentially from bottom to top. Each film layer on the heterojunction base cell 1 is grown conformally along a pyramid shape. The perovskite solar cell also includes a positive electrode 71 and a negative electrode 72. The transparent electrode layer 6 forms an ohmic contact with the positive electrode 71, and the heterojunction base cell 1 forms an ohmic contact with the negative electrode 72.

[0121] Among them, composite layer 2 is an indium tin oxide layer with a thickness of 25nm.

[0122] Hole transport layer 3 is a nickel oxide layer with a thickness of 25 nm.

[0123] Hole-modified layer 31 is a 2PACz layer, which is a monolayer.

[0124] The perovskite layer 4 has a thickness of 500 nm and is prepared by reacting a lead iodide framework layer with a cation solution. The lead iodide framework layer includes a first lead iodide layer deposited on the hole transport layer 3 and a second lead iodide layer deposited on the first lead iodide layer. The thickness of the first lead iodide layer is 100 nm and the thickness of the second lead iodide layer is 275 nm.

[0125] The passivation layer 41 is a lithium fluoride layer with a thickness of 1 nm.

[0126] Electron transport layer 5 is a C60 layer with a thickness of 17.5 nm.

[0127] The buffer layer 51 is a tin dioxide layer with a thickness of 25 nm.

[0128] The transparent electrode layer 6 is an indium tin oxide layer with a thickness of 100 nm.

[0129] Antireflection layer 8 is a magnesium fluoride layer with a thickness of 110 nm.

[0130] The positive electrode 71 is a silver positive electrode 71 with a thickness of 225 nm.

[0131] The negative electrode 72 is a silver negative electrode 72 with a thickness of 225 nm.

[0132] The above-mentioned method for preparing perovskite solar cells includes the following steps:

[0133] Provide heterojunction bottom cell 1;

[0134] A composite layer 2 is prepared on the front side of the heterojunction bottom cell 1 by magnetron sputtering.

[0135] Hole transport layer 3 is prepared by physical vapor deposition on the side of composite layer 2 away from heterojunction bottom cell 1;

[0136] Hole modification layer 31 is prepared on the side of hole transport layer 3 away from heterojunction bottom cell 1. Hole modification layer 31 is prepared by spin coating with 0.9 mg / mL 2PACz solution at a spin coating speed of 4000 rpm, annealing temperature of 100℃ and annealing time of 12 min.

[0137] Using the hole-modified layer 31 as the substrate for preparing the perovskite layer 4, the perovskite layer 4 is prepared on the side of the hole-modified layer 31 away from the heterojunction bottom cell 1, specifically as follows:

[0138] Preparation of the first lead iodide layer: A lead iodide precursor solution with a concentration of 0.5 mol / L was taken and sprayed onto the hole modification layer 31 using a spraying process. The solutes of the lead iodide precursor solution were lead iodide and cesium bromide, with a mass ratio of lead iodide to cesium bromide of 7.5:1. The solvent of the lead iodide precursor solution was a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide, with a mass ratio of N,N-dimethylformamide to dimethyl sulfoxide of 6.5:1. The spraying process was carried out in a nitrogen atmosphere, maintaining the temperature of the lead iodide precursor solution at 65℃. The hole modification layer 31 was facing upwards, and the nozzle was facing downwards accordingly. The spraying speed was 150 mm / s, and the time was 30 s. After the spraying was completed, annealing was performed at a temperature of 70℃ for 60 s to obtain the first lead iodide layer.

[0139] Preparation of the second lead iodide layer: A dual-source co-evaporation process was used to deposit the second lead iodide layer on the first lead iodide layer. The evaporation source materials were lead iodide and cesium bromide, with an evaporation rate ratio of 7.5:1 and a vacuum degree requirement of 10. -4 During the vapor deposition process, the first lead iodide layer faces downwards, the evaporation source opposite to the first lead iodide layer faces upwards, the evaporation temperature is room temperature, the evaporation source and the first lead iodide layer are kept at a certain distance, the transmission speed is 12.5 mm / s, and the evaporation rate is... A second lead iodide layer was obtained;

[0140] Preparation of perovskite layer 4: A cationic solution was spin-coated onto the second lead iodide layer. The solutes in the cationic solution included formamidinium iodoformide, formamidinium bromide, methyl bromide, and methyl chloride, and the solvent was anhydrous ethanol. The concentrations of formamidinium iodoformide, formamidinium bromide, methyl bromide, and methyl chloride were 0.45 mol / L, 0.1 mol / L, 0.15 mol / L, and 0.1 mol / L, respectively. The spin-coating environment required a relative humidity of less than 10%, a temperature of 25℃, a spin-coating speed of 4500 rpm, and a spin-coating time of 30 s. After spin-coating, the perovskite layer 4 was obtained by annealing at 135℃ for 22 min at a relative humidity of 22.5%.

[0141] A passivation layer 41 with a thickness of 1 nm was prepared by vapor deposition on the side of the perovskite layer 4 away from the heterojunction bottom cell 1. The evaporation rate was [missing information].

[0142] An electron transport layer 5 is prepared by vapor deposition on the side of the passivation layer 41 away from the heterojunction bottom cell 1.

[0143] A buffer layer 51 with a thickness of 25 nm is prepared by atomic deposition on the side of the electron transport layer 5 away from the heterojunction bottom cell 1.

[0144] A patterned transparent electrode layer 6 is fabricated by magnetron sputtering on the side of the buffer layer 51 away from the heterojunction bottom cell 1.

[0145] A patterned positive electrode 71 is deposited on the side of the transparent electrode layer 6 away from the heterojunction bottom cell 1, so that the transparent electrode layer 6 and the positive electrode 71 form an ohmic contact. A patterned negative electrode 72 is deposited on the back side of the heterojunction bottom cell 1, so that the heterojunction bottom cell 1 and the negative electrode 72 form an ohmic contact.

[0146] An antireflection layer 8 is prepared on the side of the positive electrode 71 away from the heterojunction bottom cell 1 using a vapor deposition process. The thickness of the antireflection layer 8 is 110 nm, and the evaporation rate is... The refractive index n is 1.4.

[0147] Example 2

[0148] This application provides a perovskite solar cell, which differs from Embodiment 1 in that: the thickness of the first lead iodide layer is 50 nm, the thickness of the second lead iodide layer is 325 nm, and the preparation steps of the first lead iodide layer are different. Specifically, a 0.5 mol / L lead iodide precursor solution is taken and spin-coated onto the hole modification layer 31 using a spin-coating process. The solutes in the lead iodide precursor solution are lead iodide and cesium bromide, and the mass of lead iodide and cesium bromide... The ratio of N,N-dimethylformamide to dimethyl sulfoxide was 7.5:1. The solvent for the lead iodide precursor solution was a mixture of N,N-dimethylformamide and dimethyl sulfoxide, with a mass ratio of 6.5:1. The spin coating process was carried out under nitrogen atmosphere, maintaining the temperature of the lead iodide precursor solution at 65°C, the spin coating speed at 6000 rpm, and the time at 30 s. After spin coating, annealing was performed at 70°C for 60 s, with the rest consistent with Example 1.

[0149] Example 3

[0150] This application provides a perovskite solar cell, which differs from Embodiment 1 in that: the thickness of the first lead iodide layer is 150 nm, the thickness of the second lead iodide layer is 225 nm, and the steps for preparing the first lead iodide layer are different. Specifically, the first lead iodide layer is deposited onto the hole modification layer 31 using a vapor deposition process. The vapor deposition process employs a dual-source co-evaporation process, with lead iodide and cesium bromide as the evaporation source materials. The evaporation rate ratio of lead iodide to cesium bromide is 7.5:1, and the vacuum degree requirement is 10. -4 During the vapor deposition process, the hole modification layer 31 faces downwards, the evaporation source opposite to the hole modification layer 31 faces upwards, the evaporation temperature is room temperature, the evaporation source and the hole modification layer 31 maintain a certain distance, the transmission speed is 12.5 mm / s, and the vapor deposition rate is... Everything else remains the same as in Example 1.

[0151] Example 4

[0152] This application provides a perovskite solar cell, which differs from Embodiment 1 in that the thickness of the first lead iodide layer is 40 nm and the thickness of the second lead iodide layer is 335 nm, while the rest remains the same as Embodiment 1.

[0153] Example 5

[0154] This application provides a perovskite solar cell, which differs from Embodiment 1 in that the thickness of the first lead iodide layer is 160 nm and the thickness of the second lead iodide layer is 215 nm, while the rest remains the same as Embodiment 1.

[0155] Example 6

[0156] This application provides a perovskite solar cell, which differs from Example 1 in that, when preparing the first lead iodide layer using a spray coating method, the solute in the lead iodide precursor solution is lead iodide, cesium bromide, and lead chloride; the second lead iodide layer is prepared using a three-source co-evaporation process, as detailed below:

[0157] Preparation of the first lead iodide layer: A lead iodide precursor solution with a concentration of 0.5 mol / L was taken and sprayed onto the cavity modification layer 31 using a spraying process. The solutes of the lead iodide precursor solution were lead iodide, cesium bromide, and lead chloride, with a mass ratio of 7.5:1:1. The solvent of the lead iodide precursor solution was a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide, with a mass ratio of 6.5:1. The spraying process was carried out in a nitrogen atmosphere, maintaining the temperature of the lead iodide precursor solution at 65°C. The cavity modification layer 31 was facing upwards, and the nozzle was facing downwards for spraying. The spraying speed was 150 mm / s, and the time was 30 s. After spraying, annealing was performed at a temperature of 70°C for 60 s to obtain the first lead iodide layer.

[0158] Preparation of the second lead iodide layer: The second lead iodide layer is deposited on the first lead iodide layer by evaporation. The evaporation source materials are lead iodide, cesium bromide, and lead chloride, respectively. The evaporation rate ratio of lead iodide, cesium bromide, and lead chloride is 7.5:1:1, and the required vacuum level is 10. -4 During the vapor deposition process, the first lead iodide layer faces downwards, the evaporation source opposite to the first lead iodide layer faces upwards, the evaporation temperature is room temperature, the evaporation source and the first lead iodide layer are kept at a certain distance, the transmission speed is 12.5 mm / s, and the evaporation rate is... A second lead iodide layer was obtained, and the rest remained the same as in Example 1.

[0159] Comparative Example 1

[0160] This application provides a perovskite solar cell as a comparative example, which differs from Example 1 in that: in the step of preparing the lead iodide framework layer, only the second lead iodide layer is deposited as the lead iodide framework layer, and the first lead iodide layer is not deposited, and the thickness of the second lead iodide layer is 375 nm. The specific method for preparing the lead iodide framework layer is as follows:

[0161] Preparation of lead iodide framework layer:

[0162] A dual-source co-evaporation process is employed, with lead iodide and cesium bromide as the evaporation source materials. The evaporation rate ratio of lead iodide to cesium bromide is 7.5:1, and a vacuum level of 10 is required. -4 During the vapor deposition process, the hole modification layer 31 faces downwards, and the evaporation source opposite to the hole modification layer 31 faces upwards. The evaporation temperature is room temperature, and the evaporation source and the hole modification layer 31 are kept at a certain distance. The transmission speed is 12.5 mm / s, and the evaporation rate is... A second lead iodide layer with a thickness of 375 nm was obtained.

[0163] Experiment 1

[0164] SEM scans were performed on the surfaces of the first and second lead iodide layers in Example 1. Figure 2 This is a SEM image of the surface of the first lead iodide layer. Figure 3 This is a SEM image of the surface of the second lead iodide layer.

[0165] Depend on Figure 2 and Figure 3 The comparison shows that there is a significant difference in porosity between the first and second lead iodide layers. Compared with the surface of the second lead iodide layer, the first lead iodide layer has significantly larger pores and a higher degree of porosity, while the second lead iodide layer has a higher degree of density.

[0166] Experiment 2

[0167] The performance of perovskite solar cells was tested using the Wavelabs solar simulator under the following conditions: AM1.5, 1000 W / m. 2 The test environment temperature was 25℃. Before testing, the light source was calibrated to simulate sunlight intensity using a standard silicon cell. Performance tests included energy conversion efficiency, open-circuit voltage, short-circuit current, and fill factor.

[0168] The test results of the above embodiments and comparative perovskite solar cells are shown in Table 1.

[0169] Table 1

[0170]

[0171] As can be seen from the data in Table 1, compared with Comparative Example 1, Example 1 shows an improvement of 3.07% in energy conversion efficiency, 0.054V in open-circuit voltage, and 0.71mA / cm² in short-circuit current. 2 With a fill factor of 4%, it can be seen that in the preparation step of the lead iodide framework layer, the addition of a first lead iodide layer between the substrate and the second lead iodide framework layer is more conducive to the entry of the cation solution into the bottom first lead iodide layer and its reaction with the bottom lead iodide layer. This reduces the residual lead iodide in the bottom first lead iodide layer, lowers the lead iodide content in the perovskite layer, improves the interfacial contact performance and electron transport efficiency of the perovskite layer, and significantly improves the energy conversion efficiency of the perovskite solar cell.

[0172] The data from Examples 1, 4, and 5 show that the thickness of the first lead iodide layer has a significant impact on the short-circuit current, open-circuit voltage, fill factor, and energy conversion efficiency of perovskite solar cells. At a specific thickness, the short-circuit current, open-circuit voltage, fill factor, and energy conversion efficiency of perovskite solar cells are relatively high. If the thickness of the first lead iodide layer is too high or too low, the short-circuit current, open-circuit voltage, fill factor, and energy conversion efficiency of perovskite solar cells will decrease.

[0173] The perovskite layer and its preparation method, as well as the perovskite solar cell and its preparation method disclosed in the embodiments of this application, have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the perovskite layer and its preparation method, the perovskite solar cell and its preparation method, and their core ideas. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A perovskite layer for use in solar cells, characterized in that: The perovskite layer is prepared by reacting a lead iodide framework layer with a cationic solution. The lead iodide framework layer includes a first lead iodide layer deposited on a substrate and a second lead iodide layer deposited on the first lead iodide layer. The porosity of the first lead iodide layer is higher than that of the second lead iodide layer. The thickness of the lead iodide framework layer is 300 nm to 450 nm, and the thickness of the first lead iodide layer is 50 nm to 150 nm. The solar cell includes a perovskite solar cell, which includes a silicon substrate cell with a pyramidal textured structure, and the perovskite layer is disposed on top of the silicon substrate cell with the pyramidal textured structure.

2. The perovskite layer according to claim 1, characterized in that: The thickness of the perovskite layer is 450 nm to 550 nm.

3. The perovskite layer according to claim 1, characterized in that: The first lead iodide layer is obtained by solution treatment or vapor deposition, and the second lead iodide layer is obtained by vapor deposition.

4. The perovskite layer according to claim 3, characterized in that: The solution used to prepare the first lead iodide layer is a lead iodide precursor solution with a concentration of 0.5 mol / L to 1.3 mol / L.

5. A perovskite layer according to claim 4, characterized in that: The solute in the lead iodide precursor solution includes lead iodide and cesium bromide, wherein the mass ratio of lead iodide to cesium bromide is 5-10:1; and / or, The solvent of the lead iodide precursor solution includes N,N-dimethylformamide and dimethyl sulfoxide, wherein the mass ratio of N,N-dimethylformamide to dimethyl sulfoxide is 4~9:

1.

6. The perovskite layer according to claim 1, characterized in that: The solute in the cation solution comprises at least two of the following: formamidine iodoformidium, formamidine bromoformidium, methyl bromide, and chloromethylamine; and / or, the solvent of the cation solution is one or a combination of two of anhydrous ethanol and isopropanol.

7. A perovskite layer according to claim 6, characterized in that: When the cationic solution contains the formamidinium iodoformidium, the formamidinium bromoformidium, the methyl bromide, and the methyl bromide, the concentration of the formamidinium iodoformidium is 0.3 mol / L to 0.6 mol / L, the concentration of the formamidinium bromoformidium is 0.05 mol / L to 0.2 mol / L, the concentration of the methyl bromide is 0.1 mol / L to 0.2 mol / L, and the concentration of the methyl bromide is 0.05 mol / L to 0.15 mol / L.

8. A method for preparing a perovskite layer, characterized in that: Includes the following steps: Preparation of lead iodide framework layer: A first lead iodide layer is prepared on a substrate, and a second lead iodide layer is prepared on the first lead iodide layer, wherein the porosity of the first lead iodide layer is higher than that of the second lead iodide layer; Preparation of perovskite layer: A cationic solution is spin-coated onto the second lead iodide layer, and after annealing, the perovskite layer according to any one of claims 1-7 is obtained.

9. The method for preparing a perovskite layer according to claim 8, characterized in that: The first lead iodide layer is prepared by solution method or vapor deposition method.

10. The method for preparing a perovskite layer according to claim 9, characterized in that: The method for preparing the first lead iodide layer using the solution method includes: depositing a lead iodide precursor solution by spraying or spin coating, followed by annealing. The spraying method is as follows: under an inert atmosphere, a lead iodide precursor solution at a temperature of 60℃~70℃ is sprayed onto the substrate at a spraying speed of 100 mm / s~200 mm / s and a spraying time of 30 s~60 s. The spin coating method is as follows: Under an inert atmosphere, a lead iodide precursor solution at a temperature of 60℃~70℃ is spin-coated onto the substrate. The spin coating speed is 5000 rpm~7000 rpm, and the spin coating time is 30 s~60 s.

11. The method for preparing a perovskite layer according to claim 9, characterized in that: The vacuum degree for preparing the first lead iodide using the aforementioned vapor deposition method is 1×10⁻⁶. -3 pa~1×10 -4 The transmission speed is 10 mm / s to 15 mm / s, and the evaporation rate is 3 Å / s to 5 Å / s.

12. The method for preparing a perovskite layer according to claim 10, characterized in that: The annealing temperature of the first lead iodide layer is 60℃~70℃, and the annealing time is 30 s~90 s.

13. The method for preparing a perovskite layer according to claim 8, characterized in that: When the second lead iodide layer is prepared by vapor deposition, the vacuum degree during the preparation process is controlled to be 1×10⁻⁶. -3 pa~1×10 -4 The transmission speed is 10 mm / s to 15 mm / s, and the evaporation rate is 1 Å / s to 2 Å / s.

14. The method for preparing a perovskite layer according to claim 8, characterized in that: The second lead iodide layer is prepared using a dual-source co-evaporation process or a triple-source co-evaporation process. In the dual-source co-evaporation process, the evaporation source materials are lead iodide and cesium bromide, and the evaporation rate ratio of lead iodide to cesium bromide is 5~10:

1. In the triple-source co-evaporation process, the evaporation source materials are lead iodide, cesium bromide, and S component, and the S component is any one of lead bromide, lead chloride, cesium iodide, and cesium chloride, and the evaporation rate ratio of lead iodide, cesium bromide, and S component is 5~10:1:

1.

15. The method for preparing a perovskite layer according to claim 8, characterized in that: After spin-coating the cationic solution, it is annealed at 100℃~170℃ for 15 min~30 min under conditions of 5%RH~40%RH.

16. A perovskite solar cell, characterized in that: The perovskite layer includes the perovskite layer according to any one of claims 1-7 or the perovskite layer prepared by any one of claims 8-15.

17. A perovskite solar cell according to claim 16, characterized in that: The perovskite solar cell further includes a bottom cell, a composite layer, a hole transport layer, an electron transport layer, a transparent electrode layer, a positive electrode, and a negative electrode stacked in sequence. The perovskite layer is located between the hole transport layer and the electron transport layer. The positive electrode forms an ohmic contact with the transparent electrode layer, and the negative electrode forms an ohmic contact with the bottom cell.

18. A perovskite solar cell according to claim 17, characterized in that: The thickness of the composite layer is 20 nm to 30 nm; and / or, the thickness of the hole transport layer is 20 nm to 30 nm; and / or, the thickness of the electron transport layer is 15 nm to 20 nm; the thickness of the transparent electrode layer is 80 nm to 120 nm; and / or, the thickness of the positive electrode is 150 nm to 300 nm; and / or, the thickness of the negative electrode is 150 nm to 300 nm.

19. A perovskite solar cell according to claim 17, characterized in that: The bottom cell is a heterojunction cell; and / or, the composite layer is made of one or a combination of indium tin oxide and indium zinc oxide; and / or, the hole transport layer is made of nickel oxide; and / or, the electron transport layer is made of C. 60 ; and / or, the material of the transparent electrode layer is one or a combination of indium tin oxide and indium zinc oxide; and / or, the materials of the positive electrode and the negative electrode are any one of silver, copper and aluminum, respectively.

20. A perovskite solar cell according to claim 17, characterized in that: The perovskite solar cell further includes a hole modification layer, which is located between the hole transport layer and the perovskite layer, and / or, The perovskite solar cell further includes a passivation layer, which is located between the perovskite layer and the electron transport layer, and has a thickness of 0.5 nm to 1 nm; and / or, The perovskite solar cell further includes a buffer layer, located between the electron transport layer and the transparent electrode layer, with a thickness of 20 nm to 30 nm; and / or, The perovskite solar cell also includes an antireflection layer, which is located on the side of the transparent electrode layer opposite to the bottom cell and has a thickness of 100 nm to 120 nm.

21. A perovskite solar cell according to claim 20, characterized in that: The hole-modifying layer is made of 2PACz and Meo-2PACz; and / or, the passivation layer is made of lithium fluoride; and / or, the buffer layer is made of tin dioxide; and / or, the antireflection layer is made of magnesium fluoride or lithium fluoride.

22. A method for preparing a perovskite solar cell, characterized in that: Includes the following steps: Provide a base battery; A composite layer is prepared on the bottom battery; A hole transport layer is prepared on the side of the composite layer away from the bottom cell. A perovskite layer is prepared on the side of the hole transport layer away from the bottom cell. The perovskite layer is the perovskite layer according to any one of claims 1-7 or the perovskite layer prepared by any one of claims 8-15. An electron transport layer is prepared on the side of the perovskite layer away from the bottom cell. A transparent electrode layer is fabricated on the side of the electron transport layer away from the bottom battery. A positive electrode and a negative electrode are prepared to obtain the perovskite solar cell.

23. The method for preparing a perovskite solar cell according to claim 22, characterized in that: A hole-modifying layer is prepared between the hole transport layer and the perovskite layer; and / or a passivation film is prepared between the perovskite layer and the electron transport layer; and / or a buffer layer is prepared between the electron transport layer and the transparent electrode layer; and / or an antireflection layer is prepared on the side of the transparent electrode layer away from the bottom cell.

Citation Information

Patent Citations

  • Preparation method of perovskite device

    CN115915777A