A Multi-Frequency Eddy Current Evaluation Method and Apparatus for Creep Damage State of High-Temperature Alloys
By using a multi-frequency eddy current evaluation device and method, the problem of non-destructive testing of creep damage in high-temperature alloys has been solved, enabling early warning and efficient evaluation, and improving the automation and intelligence of the testing process.
Patent Information
- Application Number
- CN202310945652.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-07-28
AI Technical Summary
Existing technologies cannot achieve simple, rapid, in-situ, adaptable, and non-destructive evaluation of creep damage in high-temperature alloys, resulting in creep damage being detected only in its late stages, which may lead to equipment failure and pose safety hazards.
A multi-frequency eddy current evaluation device is adopted, including a detector, a detection probe, an AB axis rotation module and an XYZ axis movement module. Induced eddy currents are generated by multi-frequency AC signals, impedance values are measured and differential mixing is performed, and the impedance characteristic values of the creep damage state are obtained by combining the least squares method fitting.
It enables a simple, rapid, in-situ, adaptable, and non-destructive evaluation of the creep damage state of high-temperature alloys, providing a basis for early warning and improving the automation and intelligence of the evaluation.
Smart Images

Figure CN117054515B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of creep damage assessment technology, specifically to a multi-frequency eddy current evaluation method and apparatus for creep damage state of high-temperature alloys. Background Technology
[0002] High-temperature alloys are alloy materials capable of operating under high temperature and stress conditions for extended periods. They possess high thermal strength and strong resistance to oxidation and corrosion, making them widely used in aerospace, petrochemical, and other industries. They are key materials in components such as aero-engines, gas turbines, hydrogen production converters, and pyrolysis furnaces. However, during operation, high-temperature alloys can still experience a continuous decline in material properties due to the evolution of their microstructure and the formation and aggregation of micropores under sustained deformation. This creep damage process, after reaching a certain stage, causes a sharp decrease in material strength and hardness, leading to numerous cracks and even fracture, ultimately resulting in complete material failure. Traditional non-destructive testing methods often target defects occurring in the final stage of this rapid and destructive creep damage development. Without timely detection, alarm, and shutdown for repair, this can potentially lead to fatal consequences for equipment, property, and personnel safety. Furthermore, microscopic methods such as metallographic analysis and scanning tunneling microscopy suffer from drawbacks such as difficult sample preparation, complex testing, low efficiency, and material destructiveness, making them unsuitable for engineering applications.
[0003] Given the problems with existing methods and devices for evaluating the creep damage state of high-temperature alloys, there is an urgent need for a simple, rapid, in-situ, surface-adaptive, and non-destructive method and device to evaluate the creep damage state of high-temperature alloys, thereby providing an important reference for early warning of creep failure in high-temperature alloys. Summary of the Invention
[0004] To address the above problems, this invention provides a multi-frequency eddy current evaluation method and apparatus for creep damage state of high-temperature alloys.
[0005] The present invention adopts the following technical solution:
[0006] A multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys includes a detector, a detector connected to a detection probe, a detection probe connected to an AB-axis rotation module, and an AB-axis rotation module connected to an XYZ-axis movement module.
[0007] The detection probe includes an excitation coil and a receiving coil.
[0008] Furthermore, the detection probe is connected to the AB axis rotation module via fasteners, and the AB axis rotation module is connected to the XYZ axis movement module via fasteners.
[0009] Furthermore, the detector is connected to the detection probe via a wire.
[0010] Based on the above-described apparatus, another aspect of the present invention provides a multi-frequency eddy current evaluation method for creep damage state of high-temperature alloys, comprising the following steps:
[0011] Step 1: Place the detection probe 3 vertically on the surface of the high-temperature alloy specimen and perform a full-coverage scan of the surface of the high-temperature alloy specimen;
[0012] Step 2: The detector 6 controls the detection probe 3 via wires, feeding the excitation coil 4 with values f1, f2, ..., f1 from high to low. n An alternating current signal is generated, which in turn produces a positive magnetic field, inducing eddy currents on the surface of the high-temperature alloy specimen. The detector 6 measures the impedance value of the receiving coil 5 under multi-frequency eddy currents and performs frequency mixing in a differential manner.
[0013] Step 3: Denote the impedance value Z mentioned in Step 2 as Z(R,X), where R is the resistance, X is the reactance, and the relationship between the three is Z=R+jX;
[0014] Step 4: Plot the changes in impedance values (R, X) to obtain the impedance curve and impedance plane diagram;
[0015] Step 5: The length of the projected line segment after fitting the impedance value to a straight line using the least total squares method is taken as the impedance characteristic value of the creep damage state.
[0016] Furthermore, in step 2, the formula for the difference method is as follows:
[0017] S = Z1 - Z2 - ... - Z n -Z 01 -Z 02 -...-Z 0n ,
[0018] Where Z1, Z2, ..., Z n The impedance value of the receiving coil under multi-frequency eddy current is obtained by measuring the detector; Z 01 Z 02 , ..., Z 0n To detect the reference impedance value of the receiving coil of the probe at excitation frequencies f1, f2, ..., fn.
[0019] Furthermore, the calculation of the fitted line X = kR + b in step 5 is shown in formula (1):
[0020]
[0021] Where N is the total number of sampling points, R is the resistance, X is the reactance, and k and b are the slope and intercept of the fitted line.
[0022] Furthermore, the projection points (R', X') of the impedance value onto the fitted straight line are shown in Equation (2):
[0023]
[0024] Furthermore, the length l of the projected line segment is calculated using the following formula:
[0025]
[0026] Where R' max and R' min Let R' be the maximum and minimum values of the impedance projection points (R', X'), and X' be the minimum and maximum values of the impedance projection points (R', X'). max and X' min Yes, X' has its maximum and minimum values.
[0027] The beneficial effects of this invention are:
[0028] This invention enables a simple, rapid, in-situ, surface-adaptive, and non-destructive evaluation of the creep damage state of high-temperature alloys, providing an important reference for early warning of creep failure in high-temperature alloys and improving the automation and intelligence of creep damage state evaluation. Attached Figure Description
[0029] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings of the embodiments will be briefly described below. Obviously, the drawings described below only relate to some embodiments of the present invention and are not intended to limit the present invention.
[0030] Figure 1 This is a schematic diagram of a multi-frequency eddy current evaluation method and device for creep damage state of high-temperature alloys in an embodiment.
[0031] Figure 2 This is a schematic diagram illustrating the principle of multi-frequency eddy current detection for creep damage in high-temperature alloys, as shown in the example.
[0032] Figure 3 Impedance planar diagram of multi-frequency eddy current detection for creep damage in high-temperature alloys, as shown in the example.
[0033] In the picture:
[0034] 1 – XYZ axis moving module, 2 – AB axis rotating module, 3 – detection probe, 4 – excitation coil, 5 – receiving coil, 6 – detector, 7 – wire, 8 – high-temperature alloy specimen Detailed Implementation
[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0036] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0037] like Figures 1 to 3 As shown, a multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys includes a detector 6, which is connected to a detection probe 3. Specifically, the detector 6 is connected to the detection probe 3 via a wire 7. The detection probe 3 is connected to an AB-axis rotation module 2, which is connected to an XYZ-axis movement module 1. Specifically, the detection probe 3 is connected to the AB-axis rotation module 2 via fasteners, and the AB-axis rotation module 2 is connected to the XYZ-axis movement module 1 via fasteners. The detection probe 3 includes an excitation coil 4 and a receiving coil 5.
[0038] Based on the above-mentioned device, a multi-frequency eddy current evaluation method for creep damage state of high-temperature alloys is characterized by comprising the following steps:
[0039] Step 1: Place the detection probe 3 vertically on the surface of the high-temperature alloy specimen 8 and perform a full-coverage scan of the surface of the high-temperature alloy specimen 8.
[0040] In practical operation, the high-temperature alloy specimen 8 is first fixed in place. Then, the XYZ axis moving module 1, the AB axis rotating module 2, and the detection probe 3 are assembled. This allows the detection probe 3 to scan the high-temperature alloy specimen according to a predetermined trajectory under the drive of the XYZ axis moving module 1 and the AB axis rotating module 2. During detection, the detection probe 3 contacts or is lifted away from the high-temperature alloy specimen 8 at a certain height. The XYZ axis moving module 1 controls the position of the detection probe, and the AB axis rotating module 2 controls the posture of the detection probe. Under the posture control of the XYZ axis moving module 1 and the AB axis rotating module 2, the detection probe 3 can always be perpendicular to the surface of the high-temperature alloy specimen 8 and perform a full-coverage scan of the surface of the high-temperature alloy specimen 8.
[0041] Step 2: The detector 6 controls the detection probe 3 via wires, feeding the excitation coil 4 with values f1, f2, ..., f1 from high to low. n The alternating current signal is transmitted, thereby generating a positive magnetic field, which induces eddy currents on the surface of the high-temperature alloy specimen. The detector 6 measures the impedance value of the receiving coil 5 under multi-frequency eddy current and performs frequency mixing in a differential manner.
[0042] Detection principle as follows Figure 2As shown, the detector 6 controls the detection probe via the wire 7, and passes through the excitation coil 4 at frequencies ranging from high to low: f1, f2, ..., f... i , ..., f n Alternating current signals, such as 1mHz, 500kHz, 250kHz, 100kHz, and 50kHz, generate a positive magnetic field B. 1,1 B 1,2 B 1,i B 1,n Induced eddy currents I1, I2, ..., I are generated on the surface of the high-temperature alloy specimen. i , ..., I n Eddy currents flowing in the high-temperature alloy specimen generate a reverse magnetic field B. 2,1 B 2,2 B 2,i B 2,n The impedance value of the receiving coil 5 is directionally changed, and the impedance values of the receiving coil 5 under multi-frequency eddy current are measured by the detector 6 as z1, z2, ..., z n And mixing is performed using a differential method as shown in formula (1):
[0043] S = Z1 - Z2 - ... - Z n -Z 01 -Z 02 -...-Z 0n (1)
[0044] Where Z1, Z2, ..., Z n The impedance value of the receiving coil under multi-frequency eddy current is obtained by measuring the detector; Z 01 Z 02 , ..., Z 0n To detect the reference impedance value of the receiving coil of the probe at excitation frequencies f1, f2, ..., fn.
[0045] Step 3: Denote the impedance value Z mentioned in Step 2 as Z(R,X), where R is the resistance, X is the reactance, and the relationship between the three is Z=R+jX.
[0046] In the early stages of creep damage in high-temperature alloys, the generation and aggregation of micropores increase the surface resistivity and decrease the conductivity of the high-temperature alloy specimen, thereby increasing the impedance modulus ||z|| of the receiving coil.
[0047] Step 4: Plot the changes in impedance values (R,X) to obtain impedance curves and impedance plane diagrams.
[0048] The detection probe 3 scans the surface of the high-temperature alloy specimen 8. Due to the conductivity characteristics of the high-temperature alloy material, especially the distortion of surface conductivity caused by the generation and aggregation of micropores due to creep damage, the impedance changes significantly. The changes in impedance values (R, X) during the scanning process are plotted, and the resulting curve is called the impedance curve. The resulting planar diagram is called the impedance plane diagram, such as... Figure 3 As shown, this visually reflects the creep damage state as a change in impedance characteristics.
[0049] Step 5: The length of the projected line segment after fitting the impedance value to a straight line using the least total squares method is taken as the impedance characteristic value of the creep damage state.
[0050] The calculation of the fitted line X = kR + b in step 5 is shown in formula (1):
[0051]
[0052] Where N is the total number of sampling points, R is the resistance, X is the reactance, and k and b are the slope and intercept of the fitted line.
[0053] The projection points (R', X') of the impedance value onto the fitted straight line are shown in formula (2):
[0054]
[0055] The length l of the projected line segment is calculated using the following formula:
[0056]
[0057] Where R' max and R' min Let R' be the maximum and minimum values of the impedance projection points (R', X'), and X' be the minimum and maximum values of the impedance projection points (R', X'). max and X' min Yes, X' has its maximum and minimum values.
[0058] The longer the creep time of a high-temperature alloy, the more severe the creep damage, and the larger the impedance characteristic value obtained by multi-frequency eddy current detection. The evaluation method of this invention achieves a simple, rapid, in-situ, surface-adaptive, and non-destructive evaluation of the creep damage state of high-temperature alloys, providing an important reference for early warning of creep failure in high-temperature alloys and improving the automation and intelligence of creep damage state evaluation.
[0059] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys, characterized in that, The system includes a detector, a detector connected to a detector probe, a detector probe connected to an AB-axis rotation module, and an AB-axis rotation module connected to an XYZ-axis movement module; the detector probe includes an excitation coil and a receiving coil. The device employs the following method for multi-frequency eddy current evaluation of creep damage state in high-temperature alloys: Step 1: Place the detection probe vertically on the surface of the high-temperature alloy specimen and perform a full-coverage scan of the surface of the high-temperature alloy specimen; Step 2: The detector controls the detection probe via wires, passing signals from high to low, namely f1, f2, ..., f, into the excitation coil. n The alternating current signal is received, thereby generating a positive magnetic field, which induces eddy currents on the surface of the high-temperature alloy specimen. The detector measures the impedance value of the receiving coil under multi-frequency eddy currents and performs frequency mixing in a differential manner. Step 3: Denote the impedance value Z mentioned in Step 2 as Z(R, X), where R is the resistance, X is the reactance, and the relationship between the three is Z = R + jX; Step 4: Plot the changes in impedance values (R, X) to obtain the impedance curve and impedance plane diagram; Step 5: The length of the projected line segment after fitting the impedance value to a straight line using the least total squares method is taken as the impedance characteristic value of the creep damage state.
2. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 1, characterized in that, The detection probe is connected to the AB axis rotating module via fasteners, and the AB axis rotating module is connected to the XYZ axis moving module via fasteners.
3. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 1, characterized in that, The detector is connected to the detection probe via a wire.
4. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 1, characterized in that, In step 2, the formula for the difference method is as follows: S=Z1+Z2+...+Z n -WITH 01 -WITH 02 -...-WITH 0n , Where Z1, Z2, ..., Z n The impedance value of the receiving coil under multi-frequency eddy current is obtained by measuring the detector; Z 01 Z 02 , ... , Z 0n To detect the probe at excitation frequencies f1, f2, ..., f n The reference impedance value of the lower receiving coil.
5. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 4, characterized in that, The calculation of the fitted line X=kR+b in step 5 is shown in formula (1): (1) Where N is the total number of sampling points, R is the resistance, X is the reactance, and k and b are the slope and intercept of the fitted line.
6. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 5, characterized in that, The projection points (R', X') of the impedance value onto the fitted straight line are shown in formula (2): (2)。 7. The multi-frequency eddy current evaluation device for creep damage state of high-temperature alloys according to claim 5, characterized in that, The length l of the projected line segment is calculated using the following formula: ; Where R'max and R'min are the maximum and minimum values of R' at the impedance projection point (R',X'), and X'max and X'min are the maximum and minimum values of X'.
Citation Information
Patent Citations
Multiple coil eddy current probe and method of flaw detection
US4855677A