A hydrogel with an inorganic-organic double crosslinked network structure and its preparation method

The inorganic-organic double cross-linked network structure of the hydrogel solves the problem of insufficient mechanical properties of traditional hydrogels, achieving high strength, high toughness and freeze resistance, and broadening its application in fields such as smart clothing, artificial nerves and artificial cartilage.

CN117126427BActive Publication Date: 2026-11-17CHANGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311150606.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-07
Publication Date
2026-11-17
Estimated Expiration
2043-09-07

AI Technical Summary

Technical Problem

Traditional hydrogels have low mechanical strength and poor toughness, and they are prone to expansion in solution, which affects their stability and mechanical strength. Existing nanocomposite and interpenetrating network hydrogel strategies have the problems of complex preparation and high cost.

Method used

An inorganic-organic double crosslinked network structure is adopted, through hydroxyl bridge crosslinking and free radical polymerization between inorganic materials to form densely entangled polymer chains, constructing a high-strength, high-toughness, stretchable, and antifreeze hydrogel. Iron salts are combined to lower the freezing point and form an interpenetrating network structure.

Benefits of technology

It improves the tensile strength and toughness of hydrogels, has antifreeze properties, a rigid skeleton that is not easily broken, maintains stability in low-temperature environments, has good biocompatibility, and is inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004436751450000011
    Figure HDA0004436751450000011
  • Figure HDA0004436751450000012
    Figure HDA0004436751450000012
  • Figure HDA0004436751450000013
    Figure HDA0004436751450000013
Patent Text Reader

Abstract

This invention belongs to the field of multifunctional materials, specifically relating to a hydrogel with an inorganic-organic double crosslinked network structure and its preparation method. Using acrylamide as a monomer, N,N'-methylenebisacrylamide as a crosslinking agent, ammonium persulfate as an initiator, and tetramethylethylenediamine as a catalyst, a densely entangled polymer chain polyacrylamide gel network is formed through free radical polymerization. This network is then mixed with an aqueous solution of ammonium molybdate and stirred thoroughly until a gel is formed. Finally, the gel is immersed in an appropriate amount of ferric chloride solution to form a high-strength, high-toughness, stretchable, and freeze-resistant polyacrylamide-ferric molybdate hydrogel with an inorganic-organic double crosslinked network. This hydrogel exhibits superior mechanical properties, including high strength, high toughness, high elasticity, and freeze resistance. Furthermore, the preparation method is simple, has a short cycle time, and is recyclable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of multifunctional materials, and specifically relates to a high-strength, high-toughness, stretchable, antifreeze hydrogel with an inorganic-organic double cross-linked network structure and its preparation method. Background Technology

[0002] As a porous, soft, and moist material, hydrogels are currently widely used in wastewater treatment, food chemistry, tissue engineering, and drug delivery systems. However, most traditional hydrogels suffer from low mechanical strength and poor toughness, severely limiting their applications. This is because traditional organic gels typically undergo significant volume expansion when immersed in solution, affecting their stability and mechanical strength. To systematically address these issues, creating a relatively rigid and stable gel framework has become a major research focus. Hydrogels with high strength and a rigid, stable framework are less prone to expansion and combustion, while also providing stronger resistance to photodamage and thermal degradation. Currently, strategies for improving the mechanical properties of hydrogels include nanocomposite hydrogels and interpenetrating network hydrogels. Nanocomposite hydrogels introduce nanoparticle crosslinking agents into traditional hydrogels composed of pure organic polymers, thereby improving the mechanical properties of the hydrogel (Chen, X.; Sun, L.; Wang, H.; Cao, S.; Shang, T.; Yan, H.; Lin, Q., Nano-SiO2 reinforced alginate-chitosan-gelatinnanocomposite hydrogels with improved physicochemical properties and biological activity. Colloids and Surfaces B: Biointerfaces 2023, 228, 113413.). However, although the strategies of nanocomposite hydrogels and interpenetrating network hydrogels can yield hydrogels with good mechanical properties, there are still some drawbacks. For example, nanocomposite hydrogels require high-quality nanoparticles, have complex preparation processes, and are costly. Another strategy, interpenetrating network hydrogels, are hydrogel networks formed by two or more polymers interpenetrating and entangled through a network. These networks exhibit superior physicochemical properties compared to single network structures and have been proven to be an effective way to improve the mechanical properties of traditional hydrogels (Li, Jianing.; Wang, Zhaosu.; Khan, Saeed A.; Li, Ning.; Huang, Zhiquan.; Hulin, Zhang., Self-powered information conversion based on thermogalvanic hydrogel with interpenetrating networks for nursing aphasic patients. Nano Energy 113, (2023): 108612.).Acrylamide hydrogels possess a unique three-dimensional cross-linked network structure, which endows them with high water absorption and retention, and significantly improves their mechanical properties. However, single polyacrylamide gels exhibit several problems: excessively high gel concentration results in a hard, brittle gel that is easily broken; while excessively low concentration leads to a soft, difficult-to-handle gel. Overly high cross-linking results in an opaque gel lacking elasticity; insufficient cross-linking results in a paste-like gel and a highly unstable system. Modification into a denser, interpenetrating double network structure can provide the hydrogel with a stronger framework that is less prone to breakage, while simultaneously improving its mechanical properties. Summary of the Invention

[0003] In view of the shortcomings of the prior art, the purpose of this invention is to provide a high-strength, high-toughness, stretchable antifreeze hydrogel with an inorganic-organic dual crosslinked network structure and its preparation method. This high-strength, high-toughness, stretchable antifreeze hydrogel with an inorganic-organic dual crosslinked structure is an inorganic-organic dual network structure hydrogel in which a hydrogel network formed by hydroxyl bridge crosslinking between inorganic materials interpenetrates a polymer chain polyacrylamide gel network formed by free radical polymerization. By constructing a rigid network skeleton of hydrogel and highly entangled free radicals, the hydrogel can transmit tensile tension along the length direction of the polymer chain, thereby improving the tensile strength and toughness of the hydrogel. The formation of the interpenetrating network structure, combined with the effect of iron salt in lowering the freezing point of water, prevents water molecules from forming a solid phase, thus giving the gel antifreeze properties.

[0004] To achieve the objectives of this invention, the technical solution adopted is as follows: This invention provides a high-strength, high-toughness, stretchable, antifreeze hydrogel with an inorganic-organic double crosslinked network structure and its preparation method. Acrylamide is used as a monomer, N,N-methylenebisacrylamide as a crosslinking agent, and ammonium persulfate as an initiator. These are mixed with an aqueous solution of ammonium molybdate. Under the action of a catalyst, tetramethylethylenediamine, the mixture is thoroughly stirred to form a polyacrylamide gel network. The gel is then immersed in an iron salt solution to form an inorganic-organic double crosslinked network polyacrylamide-ferric molybdate hydrogel. In the system, the molar ratio of monomer, crosslinking agent, and initiator is 7000:1:0.7~0.9. The molar ratio of monomer to molybdenum is 100:3.5~14; preferably, the molar ratio of monomer to molybdenum is 100:7~14. The molar ratio of iron to molybdenum in the system is 1~2:1.

[0005] Specifically, the preparation method of the inorganic-organic double crosslinked network polyacrylamide-ferric molybdate hydrogel includes the following steps: Step 1: Add the aqueous solution of N,N'-methylenebisacrylamide to the aqueous solution of acrylamide and stir thoroughly to obtain solution A; Step 2: Add the ammonium persulfate aqueous solution to solution A and stir thoroughly to obtain solution B; Step 3: Add the ammonium molybdate tetrahydrate aqueous solution to solution B and stir thoroughly to obtain solution C; Step 4: Add the catalyst tetramethylethylenediamine to solution C, and a transparent gel will immediately form; Step 5: Immerse the transparent gel in an iron salt solution to obtain a hydrogel with an inorganic-organic double cross-linked network structure.

[0006] The acrylamide aqueous solution has a mass concentration of 2 g / ml; the N,N'-methylenebisacrylamide aqueous solution has a molar concentration of 0.1 mol / L; the ammonium persulfate aqueous solution has a molar concentration of 0.1 mol / L; the ammonium molybdate tetrahydrate aqueous solution has a molar concentration of 0.14~0.56 mol / L; the amount of tetramethylethylenediamine is 1 ml; the iron salt is any one or more of ferric chloride, ferric chloride hydrate, ferric nitrate, and ferric nitrate hydrate, and the molar concentration of the iron salt solution is 1 mol / L.

[0007] The hydrogel prepared by the above method has high strength, high toughness, stretchability and freeze resistance.

[0008] In this invention, the monomer acrylamide is polymerized by a crosslinking agent catalyst to form a highly entangled polyacrylamide organic gel network through free radical polymerization. Then, an inorganic gel network formed by hydroxyl bridges between ammonium molybdate and ferric chloride creates an interpenetrating organic and inorganic gel network, resulting in a denser dual-network structure. On the one hand, it maintains the rigid network skeleton of the inorganic hydrogel, and on the other hand, the high degree of free radical entanglement allows the hydrogel to transmit tensile tension along the length of the polymer chain, thereby improving the tensile strength and toughness of the hydrogel. The combination of the dual networks also plays a water-locking role, giving the hydrogel antifreeze properties.

[0009] Compared with the prior art, the present invention has the following main advantages and beneficial effects: 1. This invention provides a polyacrylamide hydrogel network with low cross-linking density and high entanglement obtained by monomer free radical polymerization, which is then interpenetrated by inorganic and organic networks formed by inorganic mineral materials through hydroxyl bridges.

[0010] 2. The high-strength, high-toughness, stretchable, antifreeze hydrogel with an inorganic-organic dual cross-linked network structure provided by this invention possesses a more robust skeleton that is less prone to breakage, while also exhibiting excellent toughness and superior mechanical properties. This inorganic-organic dual-network composite hydrogel has advantages such as recyclability, controllable mechanical strength, antifreeze properties, good stability in low-temperature environments, good biocompatibility, and low cost, broadening its applications in fields such as smart clothing, artificial nerves, artificial cartilage, and artificial dressings, and has broad market prospects.

[0011] 3. The high-strength, high-toughness, stretchable, and freeze-resistant polyacrylamide-ferric molybdate hydrogel prepared by this invention can maintain its original toughness and not be frozen at low temperatures, exhibiting superior freeze-resistance compared to pure polyacrylamide hydrogel and inorganic ferric molybdate hydrogel. Inorganic ferric molybdate hydrogel can only maintain its freeze-resistance for 40 minutes at -20℃, while pure polyacrylamide hydrogel can maintain it for 24 hours.

[0012] 4. The high-strength, high-toughness, stretchable antifreeze hydrogel with an inorganic-organic double cross-linked network structure prepared by this invention has an elastic modulus of 1.96–12.88 MPa, a tensile strength of 0.42–1.77 MPa, a maximum stress at tensile fracture of 0.11–1.36 MPa, and a maximum force of 4.06–48.06 N. Compared with pure ferric molybdate inorganic hydrogel (elastic modulus of 7 kPa) and pure polyacrylamide hydrogel (elastic modulus of 0.2 MPa, tensile strength of 0.1 MPa, tensile fracture stress of 0.07 MPa, and maximum force of 2.94 N), its mechanical properties are greatly improved. Attached Figure Description

[0013] Figure 1 From left to right, the images illustrate the hydrogel formation described in Examples 1, 4, 7, and 8. Figure 2 This is a 500nm scanning electron microscope schematic diagram of the hydrogels prepared in Examples 1 and 4; Figure 3 This is a tensile schematic diagram of the high-strength, high-toughness, stretchable, antifreeze hydrogel with a polyacrylamide-ferric molybdate double crosslinking structure prepared in Example 4. Detailed Implementation

[0014] This invention is not limited to the specific embodiments listed below. Those skilled in the art can implement this invention using various other specific embodiments based on the content disclosed herein. Any modifications or alterations made to the design structure and concept of this invention fall within the protection scope of this invention. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other. The invention will be further described in detail below with reference to the embodiments: Example 1

[0015] (1) Weigh 0.883g of (NH4)6Mo7O 24 ·4H2O dissolved in 5ml of deionized water.

[0016] (2) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml deionized water, pour the ammonium molybdate solution into the ferric chloride solution, and a white precipitate immediately forms. Continue stirring until the precipitate disappears. Continue stirring for about 30 minutes to form a yellow-green gel. (e.g.) Figure 1At this point, the Fe:Mo molar ratio in the system is approximately 1:1, and it is named Gel-1M.

[0017] (3) The inorganic hydrogel of ferric molybdate was observed to have a porous structure (e.g., using a 500nm scanning electron microscope) Figure 2 a).

[0018] The inorganic hydrogel prepared in this embodiment lacks flexibility, cannot be stretched, and has an elastic modulus of only 0.7 kPa. When 2 g of ferric molybdate inorganic hydrogel was weighed and placed in a -20°C environment, white frost appeared on the surface of the ferric molybdate hydrogel after 40 minutes, indicating that the internal water had frozen and the gel had lost its inherent flexibility. Example 2

[0019] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0020] (2) Weigh 0.154g of N,N'-methylenebisacrylamide and dissolve it in 10ml of water to prepare an N,N'-methylenebisacrylamide aqueous solution with a concentration of 0.1M. Use a pipette to take 100μl of the 0.1M N,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1h.

[0021] (3) Weigh 0.228g of ammonium persulfate and dissolve it in 10ml of water to prepare an aqueous solution of ammonium persulfate with a concentration of 0.1M. Use a pipette to take 70μl of the 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1h.

[0022] (4) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water to prepare a 1mol / L solution. Pour the acrylamide solution from step (3) into the ferric chloride solution and continue stirring.

[0023] (5) Weigh 0.883g of (NH4)6Mo7O 24 ·4H2O is dissolved in 2.5 ml of deionized water. At this point, the Fe:Mo molar ratio in the system is approximately 1:1. Then, it is poured into the acrylamide solution described in step (4) and stirred for at least 1 hour. At this point, the molar ratio of monomer to molybdenum in the system is approximately 100:7:14:1.

[0024] (6) Add 1 ml of the catalyst tetramethylethylenediamine to step (5). At this time, a hydrogel cannot be formed. Example 3

[0025] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0026] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0027] (3) Use a pipette to take 70 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0028] (4) Add 1 ml of tetramethylethylenediamine catalyst to the acrylamide solution in step (3) to form a colorless polyacrylamide hydrogel immediately.

[0029] (5) Weigh 0.883g of (NH4)6Mo7O 24 ·4H2O is dissolved in 2.5ml of deionized water, and then the polyacrylamide hydrogel formed in step (4) is immersed in an ammonium molybdate aqueous solution.

[0030] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water to prepare a 1mol / L solution. Pour the solution into the solution from step (5), and a white precipitate will form. Continue stirring and the precipitate will disappear, but a hydrogel cannot be formed. Example 4

[0031] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0032] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0033] (3) Use a pipette to take 70 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0034] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h. At this point, the molar ratio of monomer to molybdenum in the system is 14:1.

[0035] (5) Add 1 ml of tetramethylethylenediamine catalyst to step (4), and a transparent and hard hydrogel is immediately formed. The tensile strength of the polyacrylamide hydrogel is 0.07 MPa and the elastic modulus is 0.2 MPa. The maximum force it can withstand is 2.94 N.

[0036] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water, and prepare a 1mol / L solution. Immerse the gel obtained in step (5) in a 1M ferric chloride solution for at least 12h. At this time, the Fe:Mo molar ratio in the system is 1:1, forming a yellowish-brown, tough inorganic-organic dual-network composite hydrogel (e.g., Figure 1 It was named PAM-FeMo(14:1:1)-1.

[0037] This polyacrylamide-ferric molybdate composite hydrogel was observed to have a woven network structure (e.g., ...) using a 500nm scanning electron microscope. Figure 2 (b) This demonstrates that the hydrogel possesses dense entanglement. Universal testing showed that the polyacrylamide-ferric molybdate hydrogel exhibited a tensile strength of 1.51 MPa, an elastic modulus of 11.32 MPa, and a maximum force of 45.21 N. Compared to a single polyacrylamide hydrogel, the tensile strength increased by 1.44 MPa, the elastic modulus by approximately 56.6 times, and the maximum force withstood by approximately 15.38 times. 2 g of the prepared hydrogel was placed in a -20°C environment for one month and still maintained its original toughness and stretchability, with a tensile strength of 1.28 MPa. This demonstrates that the organic-inorganic double crosslinked network structure of the polyacrylamide-ferric molybdate hydrogel prepared in this invention possesses antifreeze properties.

[0038] As can be seen from Examples 2, 3, and 4, the order of raw materials in the preparation process of polyacrylamide-ferric molybdate dual-network composite hydrogel is fixed. Only by immersing polyacrylamide gel containing a certain concentration of ammonium molybdate in a ferric chloride solution of appropriate concentration by immersion method can a high-strength, high-toughness, stretchable, and freeze-resistant polyacrylamide-ferric molybdate composite hydrogel be formed. Example 5

[0039] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0040] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0041] (3) Use a pipette to take 80 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0042] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0043] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and a transparent and hard hydrogel will be formed immediately.

[0044] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water, and prepare a 1mol / L solution. The gel obtained in step (5) is soaked in 1M ferric chloride solution for at least 12h to form a yellowish-brown tough inorganic-organic double network composite hydrogel, named PAM-FeMo(14:1:1)-2.

[0045] The tensile strength of the polyacrylamide-ferric molybdate hydrogel reached 1.62 MPa, the elastic modulus was 12.14 MPa, and the maximum force it could withstand was 46.78 N, as tested using a universal testing machine. Two g of the prepared hydrogel was placed in an environment of -20°C for one month and still maintained its original toughness and was stretchable, with a tensile strength of 1.55 MPa. Therefore, this demonstrates that the organic-inorganic double crosslinked network structure of the polyacrylamide-ferric molybdate hydrogel prepared in this invention possesses antifreeze properties. Example 6

[0046] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0047] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0048] (3) Use a pipette to take 90 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0049] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0050] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and a transparent and hard hydrogel will be formed immediately.

[0051] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water to prepare a 1mol / L solution. Immerse the gel obtained in step (5) in ferric chloride solution for at least 12h to form a yellowish-brown tough inorganic-organic double network composite hydrogel. Name it PAM-FeMo(14:1:1)-3.

[0052] The tensile strength of the polyacrylamide-ferric molybdate hydrogel reached 1.77 MPa, the elastic modulus was 12.88 MPa, and the maximum force it could withstand was 48.06 N, as tested using a universal testing machine. Two g of the prepared hydrogel was placed in an environment of -20°C for one month and still maintained its original toughness and was stretchable, with a tensile strength of 1.65 MPa. Therefore, this demonstrates that the organic-inorganic double crosslinked network structure of the polyacrylamide-ferric molybdate hydrogel prepared in this invention possesses antifreeze properties. Example 7

[0053] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0054] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0055] (3) Use a pipette to take 100 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0056] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0057] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) to form a loose, porous, transparent hydrogel immediately.

[0058] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water, and prepare a 1mol / L solution. The gel obtained in step (5) is soaked in ferric chloride solution for at least 12 hours. After soaking, squeezing the gel will cause liquid to seep out, proving that this ratio cannot be used with Fe... 3+ Cross-linking. (e.g.) Figure 1 ) Example 8

[0059] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0060] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0061] (3) Use a pipette to take 70 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0062] (4) Weigh 0.4415g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h. At this point, the molar ratio of monomer to molybdenum in the system is 28:1.

[0063] (5) Adding 1 ml of tetramethylethylenediamine catalyst to step (4) immediately forms a softer, more viscous, but less hard and tough polyacrylamide-ferric molybdate double-network hydrogel prepared in the proportions described in Example 4 (e.g. Figure 1 ).

[0064] (6) Weigh 1.35g FeCl3·6H2O, dissolve it in 5ml of deionized water to prepare a 1mol / L solution. Immerse the gel obtained in step (5) in ferric chloride solution for at least 12h to form a yellowish-brown tough inorganic-organic double network composite hydrogel. At this time, the Fe:Mo molar ratio in the system is 2:1, named PAM-FeMo(28:2:1)-1.

[0065] The tensile strength of the polyacrylamide-ferric molybdate hydrogel was 0.79 MPa, the elastic modulus was 2.28 MPa, and the maximum force it could withstand was 5.12 N, as tested by a universal testing machine. 2 g of the prepared hydrogel was placed in a -20°C environment for one month and still maintained its original toughness and was stretchable, with a tensile strength of 0.7 MPa. Example 9

[0066] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0067] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0068] (3) Use a pipette to take 70 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0069] (4) Weigh out 1.766g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h. At this time, the molar ratio of monomer to molybdenum in the system is 100:14≈7:1.

[0070] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4), and a soft, more viscous, and less hard and tough polyacrylamide-ferric molybdate double network double gel is immediately formed.

[0071] (6) Weigh 2.7g FeCl3·6H2O, dissolve it in 10ml of deionized water, and prepare a 1mol / L solution. Immerse the gel obtained in step (5) in ferric chloride solution for at least 12h to form a yellowish-brown tough inorganic-organic double network composite hydrogel with a rough surface and excessive white precipitate. At this time, the Fe:Mo molar ratio in the system is 1:1, and it is named PAM-FeMo(7:1:1)-1.

[0072] The tensile strength of the polyacrylamide-ferric molybdate hydrogel was 1.66 MPa, the elastic modulus was 11.89 MPa, and the maximum force it could withstand was 50.2 N, as tested by a universal testing machine. 2 g of the prepared hydrogel was placed in a -20°C environment for one month and still maintained its original toughness and was stretchable, with a tensile strength of 1.57 MPa. Example 10

[0073] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, add a magnetic stir bar, and stir for at least 1 hour to form an acrylamide solution.

[0074] (2) Use a pipette to take 10 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0075] (3) Use a pipette to take 10 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0076] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h. At this point, the molar ratio of monomer to molybdenum in the system is 14:1.

[0077] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and continue stirring. No gel was formed. Example 11

[0078] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0079] (2) Use a pipette to take 50 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0080] (3) Use a pipette to take 50 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0081] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0082] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and continue stirring until a gel is formed. Example 12

[0083] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0084] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0085] (3) Use a pipette to take 50 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0086] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0087] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and continue stirring until a gel is formed. Example 13

[0088] (1) Weigh 5g of acrylamide into a 50ml beaker, add 2.5ml of deionized water, sonicate to dissolve, place a magnetic stir bar in the beaker, and stir for at least 1 hour to form an acrylamide solution.

[0089] (2) Use a pipette to take 100 μl of 0.1 MN,N'-methylenebisacrylamide aqueous solution into the acrylamide solution in step (1) and stir for at least 1 h.

[0090] (3) Use a pipette to take 60 μl of 0.1M ammonium persulfate aqueous solution into the acrylamide solution in step (2) and stir for at least 1 h.

[0091] (4) Weigh 0.883g of (NH4)6Mo7O 24 Dissolve 4H2O in 2.5 ml of deionized water, then pour it into the acrylamide solution described in step (3) and stir for at least 1 h.

[0092] (5) Add 1 ml of the catalyst tetramethylethylenediamine to step (4) and continue stirring until a gel is formed.

[0093] As can be seen from the above embodiments, when the molar ratio of monomer to crosslinking agent is 7000:1 and the molar ratio of monomer to initiator is in the range of 7000-10000:1, a polyacrylamide gel network with optimal hardness, elasticity, and toughness can be formed. Furthermore, when the molar ratio of acrylamide, molybdenum, and iron in the system is fixed at 14:1:1, the mechanical properties of the prepared hydrogel increase with the increase of the initiator dosage. Its tensile strength is at least 4 to 18 times that of a single polyacrylamide hydrogel, its elastic modulus is 10 to 65 times, and its tensile breaking stress is 2 to 20 times. However, if the crosslinking agent and initiator dosage is too high, it will cause the system to rapidly release a large amount of heat, resulting in the evaporation of a large amount of water vapor, forming a soft gel with loose pores on the surface, which cannot then react with Fe. 3+ Cross-linking forms a second-layer network structure.

[0094] When the molar ratio of acrylamide, molybdenum, and iron in the system is 28:1:2, the mechanical properties of the prepared hydrogel deteriorate, but are still higher than those of single polyacrylamide hydrogel and inorganic iron molybdate hydrogel. When the molar ratio of acrylamide, molybdenum, and iron in the system is 7:1:1, the excess of iron and molybdenum ions deteriorates the mechanical properties of the prepared hydrogel, but its tensile strength, elastic modulus, and tensile fracture stress are all higher than those of hydrogel with reduced ammonium molybdate concentration, as well as single polyacrylamide hydrogel and inorganic iron molybdate hydrogel.

[0095] The above examples confirm that the prepared polyacrylamide-ferric molybdate hydrogel has the best mechanical properties when the molar ratio of monomer to crosslinking agent in the system is 7000:1, the molar ratio of monomer to initiator is 7778:1, and the molar ratio of monomer to molybdenum and iron is 14:1:1.

[0096] Figure 1 From left to right, these are illustrations of the hydrogel formation described in Examples 1, 4, 7, and 8.

[0097] Figure 3 This is a schematic diagram before and after stretching of the high-strength, high-toughness, stretchable, antifreeze hydrogel with a polyacrylamide-ferric molybdate double crosslinked structure prepared under the optimal conditions described in Example 4.

[0098] In summary, the above are merely preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

[0099] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing a hydrogel with an inorganic-organic double crosslinked network structure, characterized in that, Acrylamide as monomer, N,N'-methylenebisacrylamide as crosslinking agent, ammonium persulfate as initiator, and ammonium molybdate aqueous solution are mixed and stirred thoroughly under the action of tetramethylethylenediamine catalyst to form a polyacrylamide gel network. Then, it is immersed in iron salt solution to form an inorganic-organic double crosslinked network polyacrylamide-ferric molybdate hydrogel. The molar ratio of monomer, crosslinking agent and initiator is 7000:1:0.7~0.9, the molar ratio of monomer to molybdenum is 100:7~14, and the molar ratio of iron to molybdenum is 1~2:

1.

2. The method for preparing a hydrogel having an inorganic-organic double crosslinking network structure according to claim 1, characterized by, The specific steps include the following: (1) Add the aqueous solution of N,N'-methylenebisacrylamide to the aqueous solution of acrylamide and stir thoroughly to obtain solution A; (2) Add the ammonium persulfate aqueous solution to solution A and stir thoroughly to obtain solution B; (3) Add the aqueous solution of ammonium molybdate tetrahydrate to solution B and stir thoroughly to obtain solution C; (4) Adding the catalyst tetramethylethylenediamine to solution C immediately forms a transparent gel; (5) Immerse the transparent gel in an iron salt solution to obtain a hydrogel with an inorganic-organic double cross-linked network structure.

3. The method for producing a hydrogel having an inorganic-organic double crosslinking network structure according to claim 2, characterized by, The mass concentration of the acrylamide aqueous solution is 2 g / mL; the molar concentration of the N,N'-methylenebisacrylamide aqueous solution is 0.1 mol / L; and the molar concentration of the ammonium persulfate aqueous solution is 0.1 mol / L.

4. The method for preparing a hydrogel having an inorganic-organic double crosslinking network structure according to claim 2, characterized by, The molar concentration of the aqueous solution of ammonium molybdate tetrahydrate is 0.14~0.56 mol / L.

5. The method for preparing a hydrogel having an inorganic-organic double crosslinking network structure according to claim 2, characterized by, The iron salt is any one or more of ferric chloride, ferric chloride hydrate, ferric nitrate, and ferric nitrate hydrate; the molar concentration of the iron salt solution is 1 mol / L.

6. The method for preparing a hydrogel having an inorganic-organic double crosslinking network structure according to claim 2, characterized by, In step (5), the transparent gel is soaked in the iron salt solution for more than 12 hours.

7. The high-strength, high-toughness, stretchable, freeze-resistant polyacrylamide-ferric molybdate hydrogel with an inorganic-organic double crosslinked network prepared by the method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Inorganic gel material and preparation method and application thereof

    CN111939850A

  • Preparation method of tough double-network photochromic hydrogel

    CN114316145A