High-rate coal-based hard carbon composite anode material and its preparation method, sodium-ion battery

By introducing a core-shell structure and sodium-doped amorphous carbon coating into coal-based hard carbon materials, the problem of low rate performance of sodium-ion batteries was solved, achieving high rate performance and high-efficiency sodium-ion intercalation/deintercalation, thereby improving the energy density and power performance of the battery.

CN117133900BActive Publication Date: 2026-11-17SICHUAN XINGYAO NEW ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311180374.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2026-11-17
Estimated Expiration
2043-09-13

AI Technical Summary

Technical Problem

In existing technologies, the rate performance of coal-based hard carbon materials used in sodium-ion batteries is relatively low, which affects the energy density and power performance of the batteries.

Method used

A high-rate coal-based hard carbon composite anode material with a core-shell structure is used. The core is hard carbon material and the shell is sodium-doped amorphous carbon. By adding a metal catalyst to the coal-based material for rearrangement and coating the outer layer with sodium-doped amorphous carbon, the isotropy of the material and the sodium ion insertion/extraction rate are improved.

Benefits of technology

It significantly improves the power performance of the material and the sodium ion insertion/extraction rate, thereby enhancing the rate performance and initial efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117133900B_ABST
    Figure CN117133900B_ABST
Patent Text Reader

Abstract

This invention relates to a high-rate coal-based hard carbon composite anode material and its preparation method, as well as a sodium-ion battery, belonging to the field of battery technology. The preparation method of the high-rate coal-based hard carbon composite anode material of this invention includes the following steps: 1) mixing bituminous coal particles, a crosslinking agent, a metal catalyst, and a binder uniformly, hot-pressing into blocks, and then calcining at 1200-1400℃ for 1-6 hours in an atmosphere containing halogen elements, followed by cooling to obtain a hard carbon intermediate; 2) mixing the hard carbon intermediate obtained in step 1) with a carbohydrate compound and an inorganic sodium salt uniformly in an organic solvent, and spray-drying to obtain a precursor material; 3) carbonizing the precursor material obtained in step 2) at 700-1200℃ for 1-6 hours in an inert atmosphere. This invention improves the isotropy of the material by adding a metal catalyst to the coal-based material to rearrange the carbon matrix, thereby reducing the OI value of the final hard carbon material and improving its power performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-rate coal-based hard carbon composite anode material and its preparation method, as well as a sodium-ion battery, belonging to the field of battery technology. Background Technology

[0002] Sodium-ion batteries, as a new type of battery, have a significant cost advantage over lithium-ion batteries due to the relatively low cost of their electrode materials. This cost advantage is even more pronounced as the application scale of power batteries continues to expand.

[0003] The raw materials used in the preparation of anode materials for sodium-ion batteries mainly include biomass, asphalt, polymer materials, and coal-based materials. Coal-based materials mainly include bituminous coal, anthracite, and lignite, which have the characteristics of high carbon content (>80%), low cost, and easy pretreatment, making them an important choice for the development of high-performance carbon anode materials.

[0004] However, coal-based hard carbon as an anode material suffers from problems such as low specific capacity (220-260 mAh / g) and low initial efficiency (86%), which affect the improvement of battery energy density. Although the specific capacity can be improved by optimizing heat treatment, it will reduce the power performance of the material. Coating the surface of hard carbon material with other materials can improve the initial efficiency, but this will also reduce the power performance.

[0005] In the prior art, Chinese patent application No. 202110090432.6 discloses a method for preparing anthracite-based hard carbon materials by combining pre-activation pore-forming and high-temperature carbonization. The method involves pre-activating milled anthracite, followed by introducing an activating atmosphere and holding at that temperature for 1-6 hours; or adding an activator at a mass ratio of 0.5-4:1 to the powder for solid-phase premixing, holding at that temperature for 1-6 hours under an inert atmosphere, and then holding at 800-1800℃ for 0.5-10 hours to obtain the anthracite-based hard carbon material. The hard carbon material prepared by this method has a specific capacity of only 230 mAh / g and exhibits poor rate performance. Summary of the Invention

[0006] This invention provides a high-rate coal-based hard carbon composite anode material and its preparation method, as well as a sodium-ion battery, to solve the problem of low rate performance of coal-based hard carbon materials for sodium-ion batteries in the prior art.

[0007] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows:

[0008] A high-rate coal-based hard carbon composite anode material, wherein the composite anode material has a core-shell structure, the core being hard carbon material and the shell being sodium-doped amorphous carbon.

[0009] Preferably, the mass of the outer shell accounts for 1-10 wt% of the total mass of the composite negative electrode material.

[0010] The high-rate coal-based hard carbon composite anode material is a sodium salt-doped amorphous carbon-coated hard carbon composite material.

[0011] A method for preparing a high-rate coal-based hard carbon composite anode material includes the following steps:

[0012] 1) Mix bituminous coal particles, crosslinking agent, metal catalyst and binder evenly, hot press into blocks, and then calcine at 1200-1400℃ for 1-6 hours in an atmosphere containing halogen elements, and cool to obtain hard carbon intermediate;

[0013] 2) The hard carbon intermediate obtained in step 1) is mixed with sugar compounds and inorganic sodium salt in an organic solvent and spray-dried to obtain the precursor material.

[0014] 3) Carbonize the precursor material obtained in step 2) at 700-1200℃ for 1-6 hours in an inert atmosphere to obtain the final product.

[0015] In step 1), the particle size of the bituminous coal particles is 5-10 μm. Preferably, the bituminous coal particles are obtained by pulverizing bituminous coal. Preferably, the bituminous coal particles are prepared by a method comprising the following steps: soaking bituminous coal in a hydrogen peroxide solution for 10-60 min, then separating the solid and liquid, drying the solid, and holding it in an oxygen-mixed gas at 50-150°C for 1-6 h. The mass fraction of the hydrogen peroxide solution is 10-30%. The soaking process also includes ultrasonic treatment. The drying is microwave drying. The oxygen-mixed gas is composed of oxygen and nitrogen mixed at a volume ratio of 1:3-10. The flow rate of the oxygen-mixed gas is 100-500 mL / min.

[0016] In step 1), the mass ratio of bituminous coal particles to crosslinking agent is 100:1-5. The crosslinking agent mentioned in step 1) is one of triallyl isocyanurate, diacrylate, triacrylate, and tetraacrylate.

[0017] In step 1), the mass ratio of bituminous coal particles to metal catalyst is 100:1-5. Preferably, the metal catalyst is a metallocene compound. The metal catalyst is one of ferrocene, cobalt dicene, and nickel dicene.

[0018] In step 1), the mass ratio of bituminous coal particles to binder is 100:5-10. Preferably, the binder is asphalt. The binder is one of petroleum asphalt, coal tar pitch, or mesophase asphalt.

[0019] The halogen gas mentioned in step 1) is one or more of fluorine, chlorine, and bromine. The atmosphere containing the halogen is a mixture of the halogen and an inert gas. The volume ratio of the halogen to the inert gas is 1-5:10. Preferably, the volume ratio is 1-3:10. The flow rate of the halogen-inert gas mixture is 10-100 mL / min.

[0020] In step 1), hot pressing is carried out at 100-200℃ and 1-5MPa.

[0021] The mass ratio of the hard carbon intermediate to the carbohydrate compound in step 2) is 100:1-10.

[0022] The mass ratio of the hard carbon intermediate to the inorganic sodium salt in step 2) is 100:1-5.

[0023] The carbohydrate compound mentioned in step 2) is at least one of glucose, sucrose, starch, and cellulose.

[0024] The inorganic sodium salt mentioned in step 2) is at least one of sodium acetate, sodium difluorooxalate borate, and sodium dodecyl sulfonate.

[0025] In step 2), the hard carbon intermediate, carbohydrate compound, and inorganic sodium salt are mixed uniformly in an organic solvent by first adding the inorganic sodium salt to a solution of the carbohydrate compound in an organic solvent and mixing thoroughly, and then adding the hard carbon intermediate and mixing thoroughly. The organic solvent is one or a mixture of methanol, ethylene glycol, and butanediol. The mass fraction of the carbohydrate compound in the organic solvent solution is 1-10%. Preferably, the mass fraction is 1-8%.

[0026] The inert atmosphere mentioned in step 3) is nitrogen or argon.

[0027] A sodium-ion battery includes a battery casing and a positive electrode, a negative electrode, a separator, and an electrolyte disposed within the battery casing. The negative electrode includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, which is the aforementioned high-rate coal-based hard carbon composite negative electrode material.

[0028] Beneficial effects:

[0029] This invention improves the isotropy of coal-based materials by adding a metal catalyst to rearrange the carbon-based structure, thereby reducing the OI value of the final hard carbon material and enhancing its power performance. Furthermore, the sodium doping in the outer coating material increases the sodium ion insertion / extraction rate during charge and discharge, further improving rate performance. Attached Figure Description

[0030] Figure 1This is a SEM image of the high-rate coal-based hard carbon composite anode material in Example 1. Detailed Implementation

[0031] To make the technical problems, technical solutions, and beneficial effects of this invention easier to understand, the invention will be described in detail below with reference to specific embodiments.

[0032] Preparation Example 1

[0033] The preparation method of the bituminous coal particles in this example includes the following steps:

[0034] 1) The bituminous coal was crushed, soaked in a 25% hydrogen peroxide solution, ultrasonically dispersed for 45 min, filtered, and the solid was dried by microwave. Then it was transferred to a tube furnace, and a mixed gas consisting of oxygen and nitrogen in a volume ratio of 1:5 was introduced at a flow rate of 350 mL / min. The furnace was kept at 100℃ for 3 h, cooled to room temperature, and then sieved to obtain bituminous coal particles with particle sizes of 5 μm, 8 μm, and 10 μm.

[0035] Preparation Example 2

[0036] The preparation method of the bituminous coal particles in this example includes the following steps:

[0037] 1) The bituminous coal was pulverized, soaked in a 10% hydrogen peroxide solution, ultrasonically dispersed for 60 min, filtered, and the solid was dried by microwave. Then, it was transferred to a tube furnace, through which a mixed gas of oxygen and nitrogen in a 1:3 volume ratio was introduced at a flow rate of 100 mL / min. The furnace was kept at 50℃ for 6 h, cooled to room temperature, and then sieved to obtain bituminous coal particles with particle sizes of 5 μm, 8 μm, and 10 μm.

[0038] Example 1

[0039] The preparation method of the high-rate coal-based hard carbon anode material in this embodiment includes the following steps:

[0040] 1) Take 100g of bituminous coal particles with a particle size of 8μm prepared in Example 1, and then mix them evenly with 3g of triallyl isocyanurate, 3g of ferrocene, and 7g of petroleum asphalt. Then, briquette the mixture at a temperature of 150℃ and a pressure of 3MPa.

[0041] The briquetted material was transferred to a tube furnace, and a mixed gas of chlorine and argon with a volume ratio of 3:10 was introduced at a flow rate of 50 mL / min. The material was calcined at 1300℃ for 1 h, then cooled to room temperature and pulverized to a particle size D50 of 10 μm to obtain a hard carbon intermediate.

[0042] 2) Add 5g of glucose to 100g of methanol organic solvent to prepare a solution, then add 3g of sodium acetate to the solution and disperse evenly; then add 100g of the above hard carbon intermediate, mix evenly, then spray dry and pulverize.

[0043] The pulverized powder was transferred to a tube furnace and carbonized at 900℃ for 3 hours under an inert argon atmosphere to obtain a sodium salt-doped amorphous carbon-coated hard carbon composite material.

[0044] The sodium-ion battery of this embodiment includes a battery casing and a positive electrode plate, a negative electrode plate, a separator, and an electrolyte disposed within the battery casing. The positive electrode plate includes a positive current collector and a positive electrode material layer disposed on the surface of the positive current collector. The positive electrode material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder. The positive electrode active material is a ternary material LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3O2. The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The negative electrode active material is the above-mentioned sodium salt doped amorphous carbon-coated hard carbon composite material.

[0045] Example 2

[0046] The preparation method of the high-rate coal-based hard carbon anode material in this embodiment includes the following steps:

[0047] 1) Take 100g of bituminous coal particles with a particle size of 5μm prepared in Example 1, and then mix them evenly with 1g of diacrylate, 1g of cobalt thiocyanate, and 5g of coal tar pitch. Then, briquette the mixture at a temperature of 100℃ and a pressure of 5MPa.

[0048] The briquetted material was transferred to a tube furnace and a mixed gas of fluorine and argon with a volume ratio of 1:10 was introduced at a flow rate of 10 mL / min. The material was calcined at 1200℃ for 6 h, then cooled to room temperature and pulverized to a particle size D50 of 10 μm to obtain a hard carbon intermediate.

[0049] 2) Add 1g of sucrose to 100g of ethylene glycol organic solvent to prepare a solution, then add 1g of sodium difluorooxalate borate to the solution and disperse evenly; then add 100g of the above hard carbon intermediate, mix evenly, then spray dry and pulverize.

[0050] The pulverized powder was transferred to a tube furnace and carbonized at 700℃ for 6 hours under an inert argon atmosphere to obtain a sodium salt-doped amorphous carbon-coated hard carbon composite material.

[0051] The sodium-ion battery of this embodiment includes a battery casing and a positive electrode plate, a negative electrode plate, a separator, and an electrolyte disposed within the battery casing. The positive electrode plate includes a positive current collector and a positive electrode material layer disposed on the surface of the positive current collector. The positive electrode material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder. The positive electrode active material is a ternary material LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3O2. The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The negative electrode active material is the above-mentioned sodium salt doped amorphous carbon-coated hard carbon composite material.

[0052] Example 3

[0053] The preparation method of the high-rate coal-based hard carbon anode material in this embodiment includes the following steps:

[0054] 1) Take 100g of bituminous coal particles with a particle size of 10μm prepared in Example 1, and then mix them evenly with 5g of triacrylate, 5g of nickel dicene, and 10g of mesophase pitch. Then, briquette the mixture at a temperature of 200℃ and a pressure of 1MPa.

[0055] The briquetted material was transferred to a tube furnace, and a mixed gas of bromine and argon with a volume ratio of 5:10 was introduced at a flow rate of 100 mL / min. The material was calcined at 1400℃ for 1 h, then cooled to room temperature and pulverized to a particle size D50 of 10 μm to obtain a hard carbon intermediate.

[0056] 2) Add 10g of starch to 100g of butanediol organic solvent to prepare a solution, then add 5g of sodium dodecyl sulfonate to the solution and disperse evenly; then add 100g of the above hard carbon intermediate, mix evenly, then spray dry and pulverize.

[0057] The pulverized powder was transferred to a tube furnace and carbonized at 1200℃ for 1 hour under an inert argon atmosphere to obtain a sodium salt-doped amorphous carbon-coated hard carbon composite material.

[0058] The sodium-ion battery of this embodiment includes a battery casing and a positive electrode plate, a negative electrode plate, a separator, and an electrolyte disposed within the battery casing. The positive electrode plate includes a positive current collector and a positive electrode material layer disposed on the surface of the positive current collector. The positive electrode material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder. The positive electrode active material is a ternary material LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3O2. The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The negative electrode active material is the above-mentioned sodium salt doped amorphous carbon-coated hard carbon composite material.

[0059] Example 4

[0060] The preparation method of the high-rate coal-based hard carbon anode material in this embodiment includes the following steps:

[0061] 1) Take 100g of bituminous coal particles with a particle size of 8μm prepared in Example 1, and then mix them evenly with 3g of triallyl isocyanurate, 3g of ferrocene, and 7g of petroleum asphalt. Then, briquette the mixture at a temperature of 150℃ and a pressure of 3MPa.

[0062] The briquetted material was transferred to a tube furnace, and a mixed gas of fluorine and argon with a volume ratio of 3:10 was introduced at a flow rate of 100 mL / min. The material was calcined at 1200℃ for 2.5 h, then cooled to room temperature and pulverized to a particle size D50 of 10 μm to obtain a hard carbon intermediate.

[0063] 2) Add 8g of glucose to 100g of ethylene glycol organic solvent to prepare a solution, then add 3g of sodium difluorooxalate borate to the solution and disperse evenly; then add 100g of the above hard carbon intermediate, mix evenly, then spray dry and pulverize.

[0064] The pulverized powder was transferred to a tube furnace and carbonized at 900℃ for 3 hours under an inert argon atmosphere to obtain a sodium salt-doped amorphous carbon-coated hard carbon composite material.

[0065] The sodium-ion battery of this embodiment includes a battery casing and a positive electrode plate, a negative electrode plate, a separator, and an electrolyte disposed within the battery casing. The positive electrode plate includes a positive current collector and a positive electrode material layer disposed on the surface of the positive current collector. The positive electrode material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder. The positive electrode active material is a ternary material LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3O2. The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The negative electrode active material is the above-mentioned sodium salt doped amorphous carbon-coated hard carbon composite material.

[0066] Comparative Example 1

[0067] The difference between this comparative example and Example 1 is that triallyl isocyanurate, ferrocene, and petroleum asphalt are not added during mixing; otherwise, they are the same as in Example 1.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 1 is that sodium acetate is not added; otherwise, they are the same as in Example 1.

[0070] Comparative Example 3

[0071] The difference between this comparative example and Example 1 is that the bituminous coal particles used are the bituminous coal particles with a particle size of 8 μm obtained in Preparation Example 2, while the rest are the same as in Example 1.

[0072] Experimental Example

[0073] (1) SEM testing

[0074] The sodium salt-doped amorphous carbon-coated hard carbon composite material prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 1 As shown.

[0075] Depend on Figure 1 It can be seen that the material exhibits a spherical structure with a slight granulation structure, and the particle size is between 10-15 μm.

[0076] (2) Physicochemical performance testing

[0077] The powder conductivity, powder OI value, specific surface area, and particle size of the composite materials in Examples 1-4 and Comparative Examples 1-3 were tested according to the test methods in standard GB / T-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries". The test results are shown in Table 1.

[0078] Table 1

[0079] As can be seen from Table 1, the OI values ​​of the composite materials prepared in Examples 1-4 are significantly lower than those in Comparative Examples 1-3. This may be because the metal catalysts in the examples rearranged the carbon-based structure to improve the isotropy of the materials and reduce the OI value, while the doping with sodium salts with high electronic conductivity improved the electronic conductivity of the materials.

[0080] (3) Button test

[0081] The composite materials obtained in Examples 1-4 were assembled into button cells according to the following methods:

[0082] The composite materials prepared in Examples 1-4 and Comparative Examples 1-3 were used as negative electrodes and assembled into coin cells with sodium sheets, electrolytes, and separators in a glove box with argon and water contents both below 0.1 ppm. The separator was Celegard 2400; the electrolyte was a NaPF6 solution with a NaPF6 concentration of 1.1 mol / L, and the solvent was a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DMC) at a weight ratio of 1:1.

[0083]

[0084] The prepared button cells were labeled as A-1, B-1, C-1, D-1, and E-1, respectively. The performance of the button cells was then tested using a blue electric tester. The test conditions were: 0.1C charge-discharge rate, voltage range of 0.05-2V, and 3 cycles were performed before stopping. At the same time, the rate performance (1C / 0.1C) of the button cells was tested. The test results are shown in Table 2.

[0085] Table 2

[0086]

[0087] As shown in Table 2, the coin cells prepared using the composite materials of Examples 1-4 exhibit significantly higher discharge capacity and efficiency than the comparative examples. Experimental results indicate that doping the materials in these embodiments with sodium salts improves the sodium ion insertion / extraction rate during charge / discharge, thereby enhancing the rate capability and initial efficiency.

[0088] (4) Performance testing of pouch batteries

[0089] Using the composite materials of Examples 1-4 and Comparative Examples 1-3 as the negative electrode active material, layered oxide (NaFe) 1 / 3Mn 1 / 3 Ni 1 / 3 O2 was used as the positive electrode material, electrolyte, and separator to assemble a 5Ah pouch battery. The separator was Celegard 2400, and the electrolyte was a NaPF6 solution (a 1:1 volume ratio mixture of EC and DEC, with a NaPF6 concentration of 1.3 mol / L). The fabricated pouch batteries were labeled A-2, B-2, C-2, D-2, and E-2, respectively. Their cycle and rate performance were tested under the following conditions:

[0090] 1) Cyclic performance: The cycle performance of the battery was tested at a charge / discharge rate of 1C / 1C, a voltage range of 1.5V-4.0V, and a temperature of 25±3℃.

[0091] 2) Rate performance: The battery is charged to 100% SOC at a rate of 1C using constant current + constant voltage mode. Then the constant current ratio is calculated as constant current capacity / (constant current capacity + constant voltage capacity).

[0092] The test results are shown in Table 3.

[0093] Table 3

[0094]

[0095]

[0096] Table 3 compares the cycle performance and fast charging performance of the soft-pack batteries prepared with the obtained negative electrode materials. It can be seen that the cycle performance of the battery in the example is significantly better than that of the comparative example. The reason is that the material in the example has a lower OI value, which reduces expansion and improves cycle performance; at the same time, the sodium salt coating on the surface of the material in the example increases the number of sodium ions during charging and discharging, thus improving the rate performance.

Claims

1. A high-rate coal-based hard carbon composite negative material, characterized in that, The composite negative electrode material has a core-shell structure, with the core being hard carbon material and the shell being sodium-doped amorphous carbon. The preparation method of the high-rate coal-based hard carbon composite anode material includes the following steps: 1) Mix bituminous coal particles, crosslinking agent, metal catalyst and binder evenly, hot press into blocks, and then calcine at 1200-1400℃ for 1-6 hours in an atmosphere containing halogen elements, and cool to obtain hard carbon intermediate; 2) The hard carbon intermediate obtained in step 1) is mixed evenly with sugar compounds and inorganic sodium salts in an organic solvent and spray-dried to obtain the precursor material; 3) Carbonize the precursor material obtained in step 2) at 700-1200℃ for 1-6 hours in an inert atmosphere to obtain the final product; The metal catalyst is a metallocene compound.

2. A method for preparing the high-rate coal-based hard carbon composite anode material as described in claim 1, characterized in that, Includes the following steps: 1) Mix bituminous coal particles, crosslinking agent, metal catalyst and binder evenly, hot press into blocks, and then calcine at 1200-1400℃ for 1-6 hours in an atmosphere containing halogen elements, and cool to obtain hard carbon intermediate; 2) The hard carbon intermediate obtained in step 1) is mixed evenly with sugar compounds and inorganic sodium salts in an organic solvent and spray-dried to obtain the precursor material; 3) Carbonize the precursor material obtained in step 2) at 700-1200℃ for 1-6 hours in an inert atmosphere to obtain the final product.

3. The method for preparing the high-rate coal-based hard carbon composite anode material according to claim 2, characterized in that, Bituminous coal particles are prepared by a method including the following steps: soaking bituminous coal in hydrogen peroxide solution for 10-60 min, then separating the solid and liquid, drying the solid, and keeping it at 50-150℃ for 1-6 h in an oxygen mixture.

4. The preparation method of the high-rate coal-based hard carbon composite anode material according to claim 3, characterized in that, The oxygen mixture is composed of oxygen and nitrogen mixed in a volume ratio of 1:3-10.

5. The method for preparing the high-rate coal-based hard carbon composite anode material according to claim 2 or 3, characterized in that, The crosslinking agent mentioned in step 1) is one of triallyl isocyanurate, diacrylate, triacrylate and tetraacrylate.

6. The method for preparing the high-rate coal-based hard carbon composite anode material according to claim 2 or 3, characterized in that, The binder is one of petroleum asphalt, coal tar pitch, or mesophase asphalt.

7. The method for preparing the high-rate coal-based hard carbon composite anode material according to claim 2 or 3, characterized in that, The carbohydrate compound mentioned in step 2) is at least one of glucose, sucrose, starch, and cellulose.

8. The method for preparing the high-rate coal-based hard carbon composite anode material according to claim 2 or 3, characterized in that, The inorganic sodium salt mentioned in step 2) is at least one of sodium acetate, sodium difluorooxalate borate, and sodium dodecyl sulfonate.

9. A sodium-ion battery, characterized in that, The battery includes a battery casing and a positive electrode, a negative electrode, a separator, and an electrolyte disposed within the battery casing. The negative electrode includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode material layer includes a negative electrode active material, which is the high-rate coal-based hard carbon composite negative electrode material as described in claim 1.

Citation Information

Patent Citations

  • A method for preparing anthracite-based hard carbon materials by combining pre-activated pore formation and high-temperature carbonization

    CN112645305B

  • Performance improvement method of coal-based sodium ion battery negative electrode material and application thereof

    CN111293309A

  • Hard carbon-dopant coated anthracite composite negative electrode material, preparation method thereof and lithium ion battery

    CN113889605A