A 46kg-grade low-yield ratio steel for offshore wind power and its production method

By controlling the content of Al and Si and adding elements such as Sb and Sn, combined with RE, optimizing the smelting and rolling processes, the problem of offshore wind power steel being difficult to meet the requirements of high thickness, low yield ratio and corrosion resistance has been solved, and low cost has been achieved , the production of high-performance 46kg low-yield-strength steel for offshore wind power.

CN117165843BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310438297.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-22
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

It is difficult for existing offshore wind power steel to meet the requirements of high thickness, low yield-to-strength ratio, good impact toughness, aging performance and corrosion resistance at the same time, and it contains precious metal elements, which increases production costs.

Method used

By controlling the content ratio of Al and Si, and adding a small amount of Sb and Sn, combined with RE elements, 46kg low-yield steel for offshore wind power is prepared. Specific smelting, continuous casting and rolling processes are used to control the chemical composition of the steel plate. and mechanical properties, reduce yield ratio and aging sensitivity, improve corrosion resistance, and optimize performance uniformity in the thickness direction.

Benefits of technology

It achieves a low yield ratio, excellent Z-direction performance and thickness-direction performance uniformity of the steel plate, reduces production costs, improves resistance to marine atmospheric corrosion rate and aging sensitivity coefficient, and meets the comprehensive performance requirements of offshore wind power steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004999448600000081
    Figure GDA0004999448600000081
  • Figure GDA0004999448600000091
    Figure GDA0004999448600000091
Patent Text Reader

Abstract

The present invention relates to a 46kg-grade low-yield ratio offshore wind power steel and a production method. The chemical composition of the steel plate is C: 0.14%-0.16%, Si: 0.20%-0.30%, Mn: 1.65%-1.75%, P≤0.015%, S≤0.005%, V: 0.055%-0.075%, Sn: 0.06%-0.08%, Sb: 0.10%-0.30%, RE: 0.04%-0.06%, Als: 0.065%-0.095%, N≤0.003%; the rest is Fe and impurities. The steel of the present invention does not contain precious metal elements such as Cr, Ni, and Mo. By controlling the proportion of Al element content and Si element content, and adding a small amount of Sb+Sn and RE in combination, the yield ratio and aging sensitivity of the steel plate are greatly reduced, the corrosion resistance of the steel plate is improved, and the steel plate has excellent Z-direction performance and thickness direction performance uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel production, and in particular to a 46kg-grade low-yield ratio steel for offshore wind power and a production method thereof. Background Art

[0002] With the transformation of the global energy structure and the need to respond to climate change, clean energy has become the main direction of future energy development; offshore wind energy resources are abundant and stable, and the coastal areas have large power grid capacity and good wind power access conditions, so offshore wind power is an ideal clean energy. As the capacity of single units in offshore wind power projects becomes larger and larger, the wind power industry has put forward higher requirements for the performance of steel, such as greater thickness, lower yield strength ratio, better impact toughness, good aging performance, better Z-direction performance and uniformity of performance in the thickness direction, etc., and also better corrosion resistance. It is difficult for existing conventional steels to meet the above performance requirements at the same time.

[0003] The PCT international patent application with application number 201780071626.3 discloses a "low yield ratio ultra-high strength steel and its manufacturing method", which is a low yield ratio ultra-high strength steel with low yield ratio and high tensile strength suitable for use as construction steel and its manufacturing method, which can produce steel with tensile strength greater than or equal to 800MPa, yield ratio less than or equal to 0.85, -5℃ impact energy greater than or equal to 150J, and thickness less than or equal to 100mm. However, it cannot meet the current requirements of wind power steel with -20℃ impact toughness and thickness greater than 100mm. In addition, it contains precious metals Cr 0.1-0.5%, Ni 0.1-0.5%, Mo 0.1-0.5%, which increases the manufacturing cost; and it cannot meet the requirements of aging performance and corrosion resistance of offshore wind power steel.

[0004] The Chinese patent application with application number 201510314696.X discloses "a low yield ratio weather-resistant wind power tower steel and production method", with yield strength ≥420MPa, tensile strength 640~850MPa, elongation A ≥25%, yield ratio ≤0.64, corrosion resistance index I not less than 6.44, -50℃ KV2 ≥200J, -60℃ KV2 ≥185J. However, the steel contains precious metals such as Cu0.25~0.45%, Cr 0.63~0.996%, Ni 0.10~0.40%, etc., which increases the production cost; and it does not record the maximum thickness of the steel plate, and there is no aging performance evaluation, so it is impossible to determine whether it can meet the requirements of offshore wind power projects for thick steel plates and corrosion resistance.

[0005] The Chinese patent application with application number 201310677610.0 discloses "a steel for mobile offshore platform with yield ratio ≤ 0.65 and production method", with yield strength ReL ≥ 360MPa, tensile strength R m ≥ 560MPa, yield ratio ≤ 0.65, elongation A ≥ 26%, -40℃ Charpy impact absorption energy transversely > 100J, CE ≤ 0.43%. The maximum thickness of the steel plate is only 80mm, and it contains precious metals such as Ni 0.10-0.15%, Mo 0.07-0.17% and Cr 0.10-0.20%, which increases the alloy cost. In addition, it has no aging performance evaluation and cannot meet the requirements of offshore wind power projects for thick steel plates, aging performance and corrosion resistance; its production process adopts post-rolling normalizing heat treatment, which prolongs the process time and increases the process cost.

[0006] The Chinese patent application with application number 202010654393.3 discloses "a high fracture toughness and low aging sensitivity offshore wind power steel and its production method", and the steel plate has good aging impact toughness, and the -40℃ aging impact sensitivity is ≤20%. However, its composition contains 0.10-0.20% of precious metal Ni and 0.05-0.15% of Mo, which increases the alloy cost and cannot meet the requirements of uniformity of performance in the thickness direction, Z-direction performance and corrosion resistance of offshore wind power steel.

[0007] The Chinese patent application with application number 202010654392.9 discloses "a heavy unit weight and extra-thick offshore wind power steel and its production method". The steel plate has excellent welding performance while meeting the specifications of heavy unit weight and extra-thickness. It can produce steel plates with a maximum thickness of 150mm, with a yield strength of ≥355MPa, a tensile strength of ≥490MPa, and an elongation of ≥24%. The impact toughness of the steel plate at -40℃ is stably controlled at more than 100J, and the lamellar tearing resistance meets the Z35 requirements. However, the steel contains 0.10% Ni and 0.15% Cr, which increases the alloy cost, does not solve the problem of uniformity of performance in the thickness direction, and cannot simultaneously meet the requirements for aging performance and corrosion resistance.

[0008] In summary, the current offshore wind power steel or structural steel has the following shortcomings: 1. The addition of more precious metal elements Cr, Ni, and Mo increases the alloy cost; 2. The maximum thickness of the steel plate cannot meet the demand for offshore wind power steel; 3. The problem of uniformity of the Z-direction performance or thickness method performance of thick steel plates has not been solved; 4. The requirements for aging sensitivity and corrosion resistance cannot be met at the same time. Summary of the invention

[0009] The present invention provides a 46kg-grade low-yield ratio steel for offshore wind power and a production method thereof. The steel does not contain precious metal elements such as Cr, Ni, and Mo. By controlling the ratio of Al element content and Si element content and adding a small amount of Sb+Sn and RE in combination, the yield ratio and aging sensitivity of the steel plate are greatly reduced, the corrosion resistance of the steel plate is improved, and the steel plate has excellent Z-direction performance and thickness direction performance uniformity.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A 46kg-grade low-yield ratio steel for offshore wind power generation, wherein the chemical composition of the steel plate is, by weight percentage, C: 0.14%-0.16%, Si: 0.20%-0.30%, Mn: 1.65%-1.75%, P≤0.015%, S≤0.005%, V: 0.055%-0.075%, Sn: 0.06%-0.08%, Sb: 0.10%-0.30%, RE: 0.04%-0.06%, Als: 0.065%-0.095%, N≤0.003%; wherein RE / V≥0.5, Si / Al≥2.5, Sn+Sb≥0.2%; and the rest is Fe and unavoidable impurities.

[0012] The comprehensive mechanical properties of the steel plate are: yield strength 460-500Mpa, yield strength ratio ≤0.80, elongation ≥21%, and -40°C impact energy ≥180J.

[0013] The marine atmosphere corrosion resistance rate of the steel plate is less than 0.09 mm / a.

[0014] The aging sensitivity coefficient of the steel plate after aging treatment is less than 0.20; the conditions of the aging treatment are: aging strain of 5%, insulation temperature of 250°C, and insulation time of 1h; the aging sensitivity coefficient = (impact absorption energy before aging treatment - impact absorption energy after aging treatment) / impact absorption energy before aging treatment.

[0015] The maximum thickness of the steel plate is 150 mm; the Z-direction performance of the steel plate is ≥45%; the yield strength deviation between the 1 / 4 position and the 1 / 2 position in the thickness direction is ≤30 MPa, and the impact energy deviation is ≤30 J.

[0016] A method for producing 46kg-grade low-yield ratio offshore wind power steel includes smelting, continuous casting, heating and rolling processes; wherein the heating and rolling processes are controlled as follows:

[0017] 1) The heating rate during heating is ≥100℃ / h, the temperature of the soaking section is controlled at 1180~1200℃, and the heating time is controlled at 4~6h;

[0018] 2) The starting temperature of rough rolling is controlled at 1150-1180°C, low speed and large reduction are adopted during rolling, the pass reduction rate is controlled at 15%-25%, and the rolling speed is controlled at 1.2-1.8 m / s;

[0019] 3) The starting temperature of finishing rolling is 880-920°C, and the final rolling temperature is controlled at 850-880°C; the relaxation time is 20-50s;

[0020] 4) The cooling rate of the rolled steel plate during laminar cooling is controlled at 5-15°C / s, and the red-return temperature is controlled at 450-500°C.

[0021] The smelting process adopts RH vacuum treatment, the RH cycle time is 15 to 18 minutes, and the [H] in the steel is controlled below 2ppm and the [O] is controlled below 20ppm.

[0022] The target superheat of the intermediate ladle in the continuous casting process is 20-25°C; the casting is protected throughout the whole process, and the ladle is statically blown with argon for 5-10 minutes before being put on the machine; after the cast billet is off the line, it is stacked with the hot billet and slowly cooled for 24-30 hours.

[0023] The upper and lower surfaces of the steel billet are descaled before rolling, and the descaling pressure is ≥22MPa.

[0024] When the thickness of the rolling intermediate billet is 1.5 to 2 times the thickness of the finished steel plate, it is kept warm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1) The steel does not contain precious metals such as Cr, Ni and Mo, but contains a small amount of RE, Sn, Al and Si, which can control the production cost and improve the corrosion resistance of the steel plate; the marine atmospheric corrosion rate of the steel plate is less than 0.09mm / a;

[0027] 2) The steel plate has good comprehensive mechanical properties, with yield strength of 460-500Mpa, yield strength ratio ≤0.80, elongation ≥21%, and impact energy of -40℃ ≥180J;

[0028] 3) Aging sensitivity coefficient after aging treatment (aging effect is reduced to 5%, holding temperature is 250℃, holding time is 1h) is less than 0.20;

[0029] 4) The thickness specification range that can be produced is wide, the maximum thickness can reach 150mm, and the Z-direction performance is ≥45%; the yield strength deviation at the 1 / 4 position and the 1 / 2 position in the thickness direction is ≤30MPa, and the impact energy deviation is ≤30J. DETAILED DESCRIPTION

[0030] The invention discloses a 46kg-grade steel for offshore wind power with low yield ratio, wherein the chemical composition of the steel plate is, by weight percentage, C: 0.14%-0.16%, Si: 0.20%-0.30%, Mn: 1.65%-1.75%, P≤0.015%, S≤0.005%, V: 0.055%-0.075%, Sn: 0.06%-0.08%, Sb: 0.10%-0.30%, RE: 0.04%-0.06%, Als: 0.065%-0.095%, and N≤0.003%; wherein, RE / V≥0.5, Si / Al≥2.5, Sn+Sb≥0.2%; and the rest is Fe and unavoidable impurities.

[0031] The comprehensive mechanical properties of the steel plate are: yield strength 460-500Mpa, yield strength ratio ≤0.80, elongation ≥21%, and -40°C impact energy ≥180J.

[0032] The marine atmosphere corrosion resistance rate of the steel plate is less than 0.09 mm / a.

[0033] The aging sensitivity coefficient of the steel plate after aging treatment is less than 0.20; the conditions of the aging treatment are: aging strain of 5%, insulation temperature of 250°C, and insulation time of 1h; the aging sensitivity coefficient = (impact absorption energy before aging treatment - impact absorption energy after aging treatment) / impact absorption energy before aging treatment.

[0034] The maximum thickness of the steel plate is 150 mm; the Z-direction performance of the steel plate is ≥45%; the yield strength deviation between the 1 / 4 position and the 1 / 2 position in the thickness direction is ≤30 MPa, and the impact energy deviation is ≤30 J.

[0035] The production method of a 46kg-grade low-yield ratio offshore wind power steel of the present invention comprises smelting, continuous casting, heating and rolling processes; wherein the heating and rolling processes are controlled as follows:

[0036] 1) The heating rate during heating is ≥100℃ / h, the temperature of the soaking section is controlled at 1180~1200℃, and the heating time is controlled at 4~6h;

[0037] 2) The starting temperature of rough rolling is controlled at 1150-1180°C, low speed and large reduction are adopted during rolling, the pass reduction rate is controlled at 15%-25%, and the rolling speed is controlled at 1.2-1.8 m / s;

[0038] 3) The starting temperature of finishing rolling is 880-920°C, and the final rolling temperature is controlled at 850-880°C; the relaxation time is 20-50s;

[0039] 4) The cooling rate of the rolled steel plate during laminar cooling is controlled at 5-15°C / s, and the red-return temperature is controlled at 450-500°C.

[0040] The smelting process adopts RH vacuum treatment, the RH cycle time is 15 to 18 minutes, and the [H] in the steel is controlled below 2ppm and the [O] is controlled below 20ppm.

[0041] The target superheat of the intermediate ladle in the continuous casting process is 20-25°C; the casting is protected throughout the whole process, and the ladle is statically blown with argon for 5-10 minutes before being put on the machine; after the cast billet is off the line, it is stacked with the hot billet and slowly cooled for 24-30 hours.

[0042] The upper and lower surfaces of the steel billet are descaled before rolling, and the descaling pressure is ≥22MPa.

[0043] When the thickness of the rolling intermediate billet is 1.5 to 2 times the thickness of the finished steel plate, it is kept warm.

[0044] The reasons for selecting the types and contents of alloy elements in the 46kg-grade low-yield ratio offshore wind power steel of the present invention, namely, the functions of each element in the steel plate are as follows:

[0045] C: Carbon is a key element that affects the structural properties of steel plates. Different carbon contents can obtain different matching relationships between hardness and toughness. Carbon is the most effective element for improving the strength of steel plates. Low carbon content will significantly reduce the strength of steel plates. Carbon contributes less to yield strength than to tensile strength, so a high carbon content design can reduce the yield strength ratio of steel. The present invention controls the C content to 0.14% to 0.16%.

[0046] Si: Silicon is a necessary element for steelmaking deoxidation. When aluminum is used for deoxidation, adding a certain amount of silicon can significantly improve the deoxidation capacity of aluminum. Si can improve the strength of steel plates through solid solution strengthening. A certain Si content can effectively improve the marine corrosion resistance of steel, especially when combined with Al, N, etc., it can improve the resistance to marine atmospheric corrosion and high-temperature oxidation. However, high silicon will make steel tend to graphitize, making the steel brittle, reducing plasticity, and deteriorating toughness. The present invention controls the Si content to 0.20% to 0.30%, and requires Si / Al ≥ 2.5.

[0047] Mn: Manganese is the main element for improving strength and toughness, and its cost is very low. It is the main additive element in steel. When the C content is low, a higher Mn content can effectively improve the hardenability of steel, and improve the strength of the steel plate by refining the structure and promoting bainite transformation. Manganese can expand the austenite region and promote grain enlargement. It can effectively refine the grains in combination with Nb alloying and controlled rolling. However, too high a Mn content will worsen the center segregation, causing the thermal conductivity of the steel to drop sharply, the linear expansion coefficient to rise, and a large internal stress to form during rapid heating or cooling, which increases the cracking tendency of the workpiece. The present invention controls the Mn content to 1.65% to 1.75%.

[0048] P: Although phosphorus dissolved in ferrite can improve the strength and hardness of steel, its biggest harm is that it causes severe segregation, increases temper brittleness, and significantly reduces the plasticity and toughness of steel, causing the steel to easily crack during cold working, resulting in the "cold brittle" phenomenon. As an impurity element, P has an adverse effect on the low-temperature toughness of the parent material and the toughness of the welding heat-affected zone, so its content should be controlled within a reasonable range as much as possible. The present invention controls the P content to be ≤0.015%.

[0049] S: Sulfur segregates severely in steel, which will deteriorate the quality of steel. Sulfur is an inclusion-forming element, forming inclusions such as FeS and MnS, thereby reducing the ductility of steel, and the area near the inclusions will become the source of corrosion, which is not conducive to the corrosion resistance of the steel plate. The present invention controls the S content to ≤0.005%.

[0050] N: Nitrogen, like carbon, can be dissolved in iron to form interstitial solid solutions. Nitrogen in steel can form nitrides and can also dissolve and remain in the gaps after solidification, making the steel brittle and unsuitable for cold processing. Therefore, in order to produce soft steel with high plasticity, the nitrogen content must be less than 0.003%. In addition, excessive residual nitrogen in steel can lead to loose macrostructure or pores. During tempering after rapid cooling or when it stays at room temperature for a long time, precipitation hardening can occur due to the precipitation of ultra-microscopic nitrides. Nitrogen can also cause strain aging in low-carbon steel, which reduces the toughness of the steel and increases the notch sensitivity while increasing the strength and hardness. The present invention controls the N content to ≤ 0.003%.

[0051] V: V has a great affinity with O and N, and is a strong carbide-forming element. Generally, the dispersion of VC is very high and extremely stable, so it is conducive to deoxidation and degassing to obtain dense fine-grained structure, improve plasticity, toughness and high strength, and its impact performance and fatigue strength are higher than those of vanadium-free steel. Since the high dispersion of vanadium carbide can prevent the coarse grains of the weld, it can improve the weldability of steel, but it will cause the steel crystal to grow strongly after heating to the VC dissolution temperature; when dissolved in the solid solution at high temperature, it increases the hardenability; vanadium can increase the tempering stability of quenched steel and produce a secondary hardening effect. V can also increase the solid solution amount of rare earth in steel, thereby improving the corrosion resistance of steel. The present invention controls the V content to 0.055% to 0.075%.

[0052] Al: Aluminum is mainly used for deoxidation and grain refinement. Aluminum and nitrogen or oxygen form effective fine dispersions to inhibit grain growth when steel is heated. When steel is cooled, it promotes the decomposition of austenite, improves the hardenability of steel, and can also become a nucleation point for recrystallization, promote ferrite nucleation and refine grains. Aluminum can inhibit the aging of low-carbon steel, and can be stored for a long time after fine rolling without strain aging; AlN itself has high stability when heated, so it can improve the thermal stability of steel, which is conducive to reducing the overheating tendency of steel and improving the oxidation resistance of steel; aluminum generates an effective surface hardening layer through the low-temperature diffusion (nitridation) of nitrogen, which can improve the oxidation resistance and corrosion resistance of steel; when aluminum is used for deoxidation, adding a certain amount of silicon as appropriate can significantly improve the deoxidation of aluminum; but if the amount of aluminum is too much, it will cause abnormal structure of steel and promote the graphitization tendency of steel. The present invention controls the Al content to 0.065% to 0.095%.

[0053] Sn, Sb: Antimony (Sb) in steel at austenite temperature precipitates at MnS inclusions and along the original austenite grain boundaries, thereby inhibiting the enrichment and precipitation of MnS inclusions at the grain boundaries. Antimony can also refine the size of secondary recrystallized grains, refine the structure of steel and improve toughness, thereby improving the corrosion resistance of steel. The composite addition of Sn and Sb elements in steel can significantly improve the corrosion resistance of the material. Sn and Sb form SnO2 and Sb2O5 corrosion-resistant oxide films on the surface of steel, which effectively prevent the interaction between the matrix and the corrosive medium and inhibit the corrosion of steel in the corrosive medium. Sn and Sb obtained after hydration 2+ , Sb 3+ The precipitates formed in the anode micro-area fill the corrosion cracks or cavities, improving the barrier to corrosion. - Sn and Sb can also penetrate through Cl - Hydration in ambient media inhibits Fe 3+ Hydrolysis produces H + The process of Sn and Sb is improved, the pH value of the corrosion micro-area is improved, and the anode dissolution process is alleviated. Sn and Sb act as corrosion inhibitors and change the cathode and anode reaction process. The present invention controls the content of Sn and Sb to 0.06% to 0.08% and 0.10% to 0.30%; and Sn+Sb≥0.2.

[0054] RE: Rare earth (RE) atoms are active and have strong binding force. Adding rare earth to steel can improve solidification structure, change solid phase change structure, form harmless low melting point inclusions, strengthen interface through segregation, passivate surface rust layer, etc. Rare earth can improve the self-corrosion potential and polarization resistance of weathering steel, thereby inhibiting anodic reaction, increasing the resistance of the entire electrochemical reaction, and significantly reducing the corrosion rate of steel; rare earth is enriched at the grain boundary through diffusion mechanism, inhibiting the segregation of inclusions at the grain boundary, and improving the low temperature performance and corrosion resistance of steel; RE added to V-containing steel can reduce the aging precipitation effect of vanadium steel and reduce the aging sensitivity of V-containing steel. However, rare earth is a scarce resource, and its addition amount must be controlled. The present invention controls the RE content to 0.04% to 0.06%.

[0055] The production method of a 46kg-grade low-yield ratio offshore wind power steel of the present invention includes smelting, continuous casting, heating and rolling processes, and the specific process is as follows:

[0056] 1. Refining:

[0057] RH is used for vacuum treatment, with an RH cycle time of 15 to 18 minutes. [H] in the steel is controlled below 2ppm and [O] is controlled below 20ppm.

[0058] 2. Continuous casting;

[0059] The target superheat of the tundish is 20-25℃; the pouring is protected throughout the whole process, and the ladle is guaranteed to be statically blown with argon for 5-10 minutes before being put on the machine; after the ingot comes off the line, it is stacked with the hot ingot for slow cooling, and the slow cooling time is 24-30 hours.

[0060] 3. Heating;

[0061] When charging the furnace, the heating rate is required to be ≥100℃ / hour, which can effectively control the diffusion and dissolution rate of carbon and increase the austenite nucleation point; the temperature of the soaking section is controlled at 1180-1200℃, and the heating time is controlled at 4-6 hours, which can not only ensure that the billet is heated sufficiently and evenly, so that the undissolved "residual cementite" and V element in the heating process are fully dissolved, but also control the original austenite grains in the steel from being coarse.

[0062] Before rolling, the upper and lower surfaces of the billet are descaled with a descaling pressure ≥ 22MPa to ensure that foreign matter on the upper surface of the billet is removed completely.

[0063] 4. Rolling;

[0064] The starting temperature of rough rolling is controlled at 1150-1180℃, low speed and large reduction are adopted during rolling, the pass reduction rate is controlled at 15%-25%, and the rolling speed is controlled at 1.2-1.8m / s, which can ensure that the rolling force fully penetrates into the core of the steel plate and improve the uniformity of the performance in the thickness direction of the steel plate.

[0065] When the thickness of the rolling intermediate billet is 1.5 to 2 times the thickness of the finished steel plate, it is kept warm; the secondary rolling temperature is 880 to 920°C, and the final rolling temperature is controlled at 850 to 880°C; the relaxation time is 20 to 50s, so that the deformed structure can be restored, the deformation dislocation becomes polygonal, the amount of proeutectoid ferrite increases (the amount of precipitates also increases, there will be precipitation strengthening, and the precipitates can also pin the grain boundaries to refine the grains), reduce the yield strength of the steel and control the yield ratio of the steel.

[0066] After rolling, the steel plate enters laminar cooling, the cooling rate is controlled at 5-15℃ / s, and the red-return temperature is controlled at 450-500℃.

[0067] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0068] [Example]

[0069] According to the chemical composition and production process described in the present invention, 46kg grade low yield ratio offshore wind power steel is produced. The smelting composition of each actual example steel is shown in Table 1, the production process parameters are shown in Table 2, and the performance of the finished steel plate is shown in Table 3.

[0070] Table 1 Melting composition of steel

[0071] Example C Si Mn P S V Als Sn Sb RE N RE / V Si / Al Sn+Sb 1 0.14 0.30 1.75 0.013 0.005 0.075 0.095 0.078 0.13 0.043 0.002 0.57 3.15 0.21 2 0.16 0.30 1.65 0.014 0.005 0.055 0.065 0.065 0.2 0.056 0.002 1.02 4.12 0.27 3 0.15 0.25 1.70 0.012 0.005 0.065 0.07 0.073 0.25 0.044 0.0025 0.68 3.57 0.32 4 0.14 0.25 1.65 0.015 0.005 0.06 0.085 0.062 0.25 0.045 0.002 0.75 2.94 0.31 5 0.14 0.25 1.65 0.012 0.005 0.075 0.08 0.065 0.25 0.055 0.0025 0.73 3.13 0.32 6 0.15 0.30 1.75 0.012 0.003 0.065 0.075 0.066 0.25 0.045 0.002 0.69 4 0.32 7 0.16 0.20 1.75 0.014 0.003 0.06 0.07 0.068 0.2 0.060 0.002 1 2.86 0.27 8 0.15 0.30 1.70 0.013 0.004 0.065 0.065 0.077 0.2 0.058 0.002 0.89 4.62 0.28 9 0.15 0.21 1.70 0.015 0.004 0.075 0.082 0.067 0.3 0.042 0.002 0.56 2.56 0.37 10 0.16 0.22 1.72 0.012 0.004 0.065 0.085 0.062 0.18 0.056 0.0025 0.86 2.59 0.24

[0072] Note: Except for RE / V and Si / Al in Table 1, the units of other values ​​are all Wt%.

[0073] Table 2 Production process parameters

[0074]

[0075] Table 3 Finished steel plate properties

[0076]

[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A 46kg-grade low-yield ratio steel for offshore wind power, characterized in that: The chemical composition of the steel plate is C: 0.14%-0.16%, Si: 0.20%-0.30%, Mn: 1.65%-1.75%, P≤0.015%, S≤0.005%, V: 0.055%-0.075%, Sn: 0.06%-0.08%, Sb: 0.10%-0.30%, RE: 0.04%-0.06%, Als: 0.065%-0.095%, N≤0.003% by weight; wherein RE / V≥0.5, Si / Al≥2.5, Sn+Sb≥0.2%; the rest is Fe and unavoidable impurities; the comprehensive mechanical properties of the steel plate are: yield strength 460-500MPa, yield strength ratio≤0.80, elongation≥21%, -40℃ impact energy≥180J.

2. The 46kg-grade low-yield ratio offshore wind power steel according to claim 1, characterized in that: The marine atmosphere corrosion resistance rate of the steel plate is less than 0.09 mm / a.

3. The 46kg-grade low-yield ratio offshore wind power steel according to claim 1, characterized in that: The aging sensitivity coefficient of the steel plate after aging treatment is less than 0.20; the conditions of the aging treatment are: aging strain of 5%, insulation temperature of 250°C, and insulation time of 1h; the aging sensitivity coefficient = (impact absorption energy before aging treatment - impact absorption energy after aging treatment) / impact absorption energy before aging treatment.

4. The 46kg-grade low-yield ratio offshore wind power steel according to claim 1, characterized in that: The maximum thickness of the steel plate is 150 mm; the Z-direction performance of the steel plate is ≥45%; the yield strength deviation between the 1 / 4 position and the 1 / 2 position in the thickness direction is ≤30 MPa, and the impact energy deviation is ≤30 J.

5. The method for producing the 46kg-grade low-yield ratio offshore wind power steel according to any one of claims 1 to 4, characterized in that: It includes smelting, continuous casting, heating and rolling processes; the heating and rolling processes are controlled as follows: 1) The heating rate during heating is ≥100℃ / h, the temperature of the soaking section is controlled at 1180~1200℃, and the heating time is controlled at 4~6h; 2) The starting temperature of rough rolling is controlled at 1150-1180°C, low speed and large reduction are adopted during rolling, the pass reduction rate is controlled at 15%-25%, and the rolling speed is controlled at 1.2-1.8 m / s; 3) The starting temperature of finishing rolling is 880-920°C, and the final rolling temperature is controlled at 850-880°C; the relaxation time is 20-50s; 4) The cooling rate of the rolled steel plate during laminar cooling is controlled at 5-15°C / s, and the red-return temperature is controlled at 450-500°C.

6. The method for producing a 46kg-grade low-yield ratio offshore wind power steel according to claim 5, characterized in that: The smelting process adopts RH vacuum treatment, the RH cycle time is 15 to 18 minutes, and the [H] in the steel is controlled below 2ppm and the [O] is controlled below 20ppm.

7. The method for producing a 46kg-grade low-yield ratio offshore wind power steel according to claim 5, characterized in that: The target superheat of the intermediate ladle in the continuous casting process is 20-25°C; the casting is protected throughout the whole process, and the ladle is statically blown with argon for 5-10 minutes before being put on the machine; after the cast billet is off the line, it is stacked with the hot billet and slowly cooled for 24-30 hours.

8. The method for producing 46kg-grade low-yield ratio offshore wind power steel according to claim 5, characterized in that: The upper and lower surfaces of the steel billet are descaled before rolling, and the descaling pressure is ≥22MPa.

9. The method for producing a 46kg-grade low-yield ratio offshore wind power steel according to claim 5, characterized in that: When the thickness of the rolling intermediate billet is 1.5 to 2 times the thickness of the finished steel plate, it is kept warm.