Negative electrode material and preparation method thereof, and sodium ion battery

By preparing carbon-based anode materials with high microscopic disorder and modifying them with organic functional groups and metal elements, a large number of nanoporous structures are formed, which solves the problem of insufficient capacity of carbon anode materials for lithium-ion batteries in the sodium battery field, and realizes the high capacity and long life performance of sodium-ion batteries.

CN117334811BActive Publication Date: 2026-11-24SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210724744.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2026-11-24
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

Existing carbon anode materials for lithium-ion batteries have limited capacity improvement in the sodium battery field, failing to meet the demand for high energy density. Furthermore, existing modification methods cannot effectively improve the capacity, initial efficiency, and lifespan performance of anode materials for sodium-ion batteries.

Method used

A negative electrode material is prepared by mixing a modified additive containing organic functional groups and metal elements with a carbon source, followed by heat treatment and pre-carbonization to form a carbon matrix with high microscopic disorder, containing a large number of highly dispersed nanoporous structures. The powder conductivity and electrical contact environment of the material are improved by acid washing and heat treatment.

Benefits of technology

This significantly improves the sodium storage capacity and cycle performance of sodium-ion batteries, resulting in a high-capacity, fast-chargeable, and long-life anode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117334811B_ABST
    Figure CN117334811B_ABST
Patent Text Reader

Abstract

This application relates to an anode material and its preparation method, and a sodium-ion battery. The anode material comprises a carbon matrix composed of graphite microcrystalline structural units. Pores are distributed between the graphite microcrystalline structural units. The microscopic disorder S of the anode material is 65%–80%, where: S = (A / B) * 100% (I). In the above formula, A is the ordinate value of the peak-valley formed by connecting the baseline of the XRD curve of the anode material between 2Theta = 10° and 20° and the 002 diffraction peak. B is the ordinate value of the peak value of the 002 diffraction peak in the XRD curve of the anode material. The microscopic disorder S of the anode material of this application is 65%–80%, indicating a relatively high degree of disorder in the arrangement of graphite microcrystalline units. The interstices between the graphite microcrystals inside the anode material generate a large number of highly dispersed nanoporous structures with sodium storage activity, which can significantly improve sodium storage capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of negative electrode material technology, specifically, it relates to negative electrode materials and their preparation methods, and sodium-ion batteries. Background Technology

[0002] With increasingly scarce lithium resources, the price of raw materials for lithium-ion batteries has risen significantly, inevitably leading to resource constraints on the development of lithium batteries. Sodium resources are abundant, inexpensive, and readily available, with low processing costs, making sodium-based batteries significantly cheaper than lithium-ion batteries. Therefore, sodium-based batteries have a broader development prospect than lithium-ion batteries. Compared to other anode materials, carbon anode materials have advantages such as low cost, large carbon interlayer spacing, low operating voltage, good conductivity, and good cycle performance, and are considered the most advantageous anode material for sodium-based batteries.

[0003] If existing carbon anode materials used in lithium-ion batteries are applied to sodium batteries, it is difficult to increase their capacity. Therefore, in order to meet the high energy density requirements of sodium batteries, it is urgent to develop anode materials with high sodium storage capacity. Summary of the Invention

[0004] In order to overcome the above-mentioned defects, this application provides a negative electrode material and its preparation method, as well as a sodium-ion battery, which solves the technical problem that it is difficult to improve the capacity, initial efficiency and life performance of the negative electrode material for sodium-ion batteries.

[0005] In a first aspect, this application provides a negative electrode material comprising a carbon matrix composed of graphite microcrystalline structural units, wherein porous structures are distributed between the graphite microcrystalline structural units, and the microscopic disorder S of the negative electrode material is 65%–80%, wherein:

[0006] S = (A / B) * 100% (I)

[0007] In the above formula, A is the ordinate value of the peak and valley formed by connecting the baseline and the 002 diffraction peak curve of the XRD curve of the negative electrode material between 2Theta=10°~20°, and B is the ordinate value of the peak value of the 002 diffraction peak in the XRD curve of the negative electrode material.

[0008] In conjunction with the first aspect, the negative electrode material includes soft carbon and hard carbon.

[0009] In conjunction with the first aspect, the carbon interlayer spacing of the negative electrode material is 0.34 nm to 0.40 nm.

[0010] In conjunction with the first aspect, the pore volume V of the negative electrode material 孔 It is 0.05cm 3 / g~0.35cm 3 / g.

[0011] In conjunction with the first aspect, the true density ρ of the negative electrode material is 1.2 g / cm³.3 ~2.2g / cm 3 .

[0012] In conjunction with the first aspect, the porosity W of the negative electrode material is 10% to 40%, wherein:

[0013] W = V 孔 / (V 孔 +1 / ρ)*100% (II)

[0014] In the above formula, ρ is the true density, with units of g / cm³. 3 V 孔 The volume is the pore volume, expressed in cm³ / g; where the volume of the carbon matrix is ​​1 / ρ.

[0015] In conjunction with the first aspect, the median particle size of the negative electrode material is 1 μm to 40 μm.

[0016] In conjunction with the first aspect, the specific surface area SA of the negative electrode material is: 5m² 2 / g<SA≤250m 2 / g.

[0017] In conjunction with the first aspect, the powder conductivity of the negative electrode material is 30 S / cm to 55 S / cm.

[0018] In conjunction with the first aspect, the oxygen content of the negative electrode material is 0.1% to 1.0%.

[0019] In conjunction with the first aspect, the oil absorption value of the negative electrode material is 45mL / 100g to 90mL / 100g.

[0020] In conjunction with the first aspect, the Raman spectrum of the negative electrode material obtained by Raman spectroscopy using a measurement light source with a wavelength of 532 nm is shown to show that at 1000 cm⁻¹... -1 Up to 1400cm -1 G-band was observed at 1500 cm. -1 Up to 2000cm -1 The D band was observed, and the peak intensity I of the D band was... D With the peak intensity I of the G-band G The ratio between I D / I G It ranges from 1.1 to 1.7.

[0021] Secondly, this application provides a method for preparing a negative electrode material, comprising the following steps:

[0022] A first precursor is obtained by subjecting a mixture containing a carbon source and a modifying additive to a first heat treatment, wherein the modifying additive includes an RM compound, wherein R includes an organic functional group and M includes a metal element.

[0023] The first precursor is pre-carbonized to obtain the second precursor;

[0024] The second precursor is subjected to acid washing and a second heat treatment to obtain the negative electrode material.

[0025] In conjunction with the second aspect, the organic functional group R includes a carbon-based functional group or a combination of a carbon-based functional group and a heteroatom functional group.

[0026] In conjunction with the second aspect, the carbon-based functional group includes at least one of alkyl, alkenyl, alkynyl, phenyl, and carbon chains containing benzene rings.

[0027] In conjunction with the second aspect, the heteroatom functional group includes at least one selected from hydroxyl, aldehyde, carboxyl, amino, acyl, amide, nitro, carbonyl, carboxylate, and sulfonate groups.

[0028] In conjunction with the second aspect, the metallic element M includes at least one selected from lithium, sodium, magnesium, potassium, calcium, zinc, copper, and tin.

[0029] In conjunction with the second aspect, the RM compound includes R′(OH). x (COO) y M 1 / z ] i , where x, y, z, and i are positive integers, and R′ includes organic functional groups.

[0030] In conjunction with the second aspect, the RM compound includes at least one of lithium tartrate, sodium tartrate, magnesium tartrate, potassium tartrate, calcium tartrate, zinc tartrate, copper tartrate, lithium maleate, sodium maleate, magnesium maleate, potassium maleate, calcium maleate, zinc maleate, copper maleate, lithium citrate, sodium citrate, magnesium citrate, potassium citrate, calcium citrate, zinc citrate, copper citrate, lithium glycolate, sodium glycolate, magnesium glycolate, potassium glycolate, calcium glycolate, zinc glycolate, copper glycolate, lithium salicylate, sodium salicylate, magnesium salicylate, potassium salicylate, calcium salicylate, zinc salicylate, and copper salicylate.

[0031] In conjunction with the second aspect, the carbon source includes a first carbon source, and the process of subjecting a mixture containing the first carbon source and a modifying additive to a first heat treatment to obtain a first precursor includes: mixing the first carbon source and the modifying additive and then sequentially performing a first addition reaction and a first curing reaction to obtain the first precursor.

[0032] In conjunction with the second aspect, the first carbon source includes at least one of glucose, fructose, maltose, sucrose, thermoplastic phenolic resin, starch, cellulose, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt, and asphalt.

[0033] In conjunction with the second aspect, the mass ratio of the first carbon source to the modified additive is (40:60) to (99:1).

[0034] In conjunction with the second aspect, the temperature of the first addition reaction is 80℃~160℃.

[0035] In conjunction with the second aspect, the time for the first addition reaction is 0.5 h to 24 h.

[0036] In conjunction with the second aspect, the process further includes a step of adding a first curing agent to the reaction product of the first carbon source and the modified additive before the first curing reaction.

[0037] In conjunction with the second aspect, before the first curing reaction, the step of adding a first curing agent to the reaction product of the first carbon source and the modified additive is also included, wherein the mass ratio of the first carbon source to the first curing agent is (60:40) to (95:5).

[0038] In conjunction with the second aspect, prior to the first curing reaction, the method further includes adding a first curing agent to the reaction product of the first carbon source and the modified additive. The first curing agent includes at least one of ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate.

[0039] In conjunction with the second aspect, the temperature of the first curing reaction is 80℃~300℃.

[0040] In conjunction with the second aspect, the time for the first curing reaction is 0.5h to 24h.

[0041] In conjunction with the second aspect, the process further includes a first crushing and a first sieving step of mixing the first carbon source and the modified additive before mixing them.

[0042] In conjunction with the second aspect, the carbon source includes a second carbon source, and the first heat treatment of the mixture containing the second carbon source and the modifying additive to obtain the first precursor includes: mixing the second carbon source, the modifying additive and the second curing agent and simultaneously carrying out a second addition reaction and a second curing reaction to obtain the first precursor.

[0043] In conjunction with the second aspect, the second carbon source includes at least one of starch, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt, lignin, cellulose, coconut shell, almond shell, walnut shell, peach kernel shell, peanut shell, pistachio shell, hazelnut shell, sawdust, and straw.

[0044] In conjunction with the second aspect, the mass ratio of the second carbon source to the modified additive is (40:60) to (99:1).

[0045] In conjunction with the second aspect, the temperature at which the second addition reaction and the second curing reaction are carried out simultaneously is 80℃~300℃.

[0046] In conjunction with the second aspect, the time for the simultaneous second addition reaction and second curing reaction is 0.5h to 24h.

[0047] In conjunction with the second aspect, the mass ratio of the second carbon source to the second curing agent is (60:40) to (100:0) (inclusive of 0).

[0048] In conjunction with the second aspect, the second curing agent includes at least one of ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate.

[0049] In conjunction with the second aspect, before mixing the second carbon source, the modified additive, and the second curing agent, the process further includes a second crushing and a second sieving step of the second carbon source, the modified additive, and the second curing agent.

[0050] In conjunction with the second aspect, the pre-carbonization treatment is carried out in a first protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon, and krypton.

[0051] In conjunction with the second aspect, the pre-carbonization temperature is 500℃~800℃.

[0052] In conjunction with the second aspect, the pre-carbonization time is 0.5h to 24h.

[0053] In conjunction with the second aspect, the pre-carbonization equipment includes at least one of a tube furnace, a box furnace, a pusher kiln, and a roasting kiln.

[0054] In conjunction with the second aspect, after obtaining the second precursor through pre-carbonization, the process further includes a third crushing and a third sieving step on the second precursor.

[0055] In conjunction with the second aspect, the acid solution used for pickling includes a solution of at least one selected from hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, acetic acid, oxalic acid, benzoic acid, hydrosulfuric acid, hydrobromic acid, and hydroiodic acid.

[0056] In conjunction with the second aspect, the mass ratio of the second precursor to the pickling acid solution is 1:(3-15).

[0057] In conjunction with the second aspect, the mass concentration of the acid solution used for pickling is 10% to 50%.

[0058] In conjunction with the second aspect, the temperature of the second heat treatment is 900℃~1800℃.

[0059] In conjunction with the second aspect, the duration of the second heat treatment is 1 hour to 24 hours.

[0060] In conjunction with the second aspect, the second heat treatment is carried out in a second protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon, and krypton.

[0061] In conjunction with the second aspect, the second heat treatment also includes a step of performing a fourth screening of the obtained material, wherein the screen size of the fourth screening is 200 mesh to 325 mesh.

[0062] Thirdly, this application provides a sodium-ion battery, which includes the negative electrode material described in the first aspect or the negative electrode material described in the second aspect.

[0063] The technical solution of this application has at least the following beneficial effects:

[0064] The negative electrode material of this application includes a carbon matrix, which comprises graphite microcrystalline structural units. Pores are distributed in the gaps between the graphite microcrystalline structural units. The microscopic disorder S of the negative electrode material is 65% to 80%, indicating that the graphite microcrystalline units in the negative electrode material have a relatively high degree of disorder. This results in the formation of a large number of highly dispersed nano-sized pores with sodium storage activity in the graphite microcrystalline gaps inside the negative electrode material, which can significantly improve the sodium storage capacity and cycle performance.

[0065] This application obtains a first precursor with a "rigid structure" by mixing a modified additive containing organic functional groups and metal elements with a carbon source and then subjecting the mixture to a first heat treatment. The metal elements are highly dispersed within the first precursor and their positions are fixed, exhibiting strong chemical bonding with adjacent groups. This characteristic provides favorable conditions for increasing the microscopic disorder of the negative electrode and constructing a large number of highly dispersed nano-sized pores. The first precursor is then pre-carbonized to obtain a second precursor. Metal elements in similar positions within the material are transformed into nano-metal oxide microcrystals, and the carbon-containing components are transformed into graphite microcrystalline units. The nano-metal oxide microcrystals hinder the orderly arrangement of the graphite microcrystals, increasing the microscopic disorder of the negative electrode and resulting in a highly disordered arrangement of the graphite microcrystalline units. Finally, the second precursor is acid-washed to remove the nano-metal oxide microcrystals, resulting in a large number of highly dispersed nano-sized pore structures inside the material, providing favorable conditions for sodium storage. After the second heat treatment, the structural defects (dangling bonds, free radicals, etc.) of the negative electrode material are burned off, improving the powder conductivity, reducing polarization, and improving the electrical contact environment of the pore structure. This increases the sodium storage electrochemical activity of the negative electrode pore structure, significantly improving the sodium storage capacity and cycle performance, ultimately obtaining a high-capacity, fast-chargeable, and long-life negative electrode material for sodium-ion batteries. Attached Figure Description

[0066] The present application will be further described below with reference to the accompanying drawings and embodiments.

[0067] Figure 1 This is a schematic diagram of the structure of the negative electrode material in this application;

[0068] Figure 2 The preparation process of the negative electrode material of this application is as follows. Figure 1 ;

[0069] Figure 3 The preparation process of the negative electrode material of this application is as follows. Figure 2 ;

[0070] Figure 4 Here is a SEM image of the negative electrode material obtained in Example 1 of this application;

[0071] Figure 5 The image shows the XRD pattern of the negative electrode material in this application;

[0072] Figure 6 This is a schematic diagram of the microstructure of the negative electrode material obtained in Comparative Example 1;

[0073] Figure 7 The first charge-discharge curve of the negative electrode material obtained in Example 1 of this application is shown. Detailed Implementation

[0074] To better understand the technical solution of this application, the embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0075] It should be understood that the described embodiments are merely some, not all, of the embodiments in this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.

[0076] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0077] It should be understood that the term "and / or" used in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this article generally indicates that the preceding and following related objects have an "or" relationship.

[0078] In existing technologies, heteroatom doping and pore structure construction methods are commonly used to improve the capacity performance of anodes for sodium-ion batteries. Heteroatom doping improves the sodium storage capacity of carbon materials by doping with hetero-elements (B, N, S, P, etc.), but this often results in an increase in reversible capacity, a decrease in initial efficiency and available capacity ratio, voltage lag, and a decline in safety performance. Pore structure construction improves sodium storage capacity performance by constructing pore structures: (1) constructing pore structures with organic template agents (ethanol, surfactants, etc.); (2) constructing pore structures with inorganic template agents (silicon oxide, inorganic salts, etc.); (3) constructing pores by activation. However, the above methods cannot obtain highly dispersed nanoscale pores for pore construction modification, and there are many defects, resulting in low initial efficiency and cycle performance of the anode material, and the improvement in sodium storage performance is not significant.

[0079] Therefore, this application provides a negative electrode material, such as Figure 1 As shown, the negative electrode material includes a carbon matrix, which comprises graphite microcrystalline structural units. Pores are distributed between these units. The microscopic disorder S of the negative electrode material is 65%–80%, wherein:

[0080] S = (A / B) * 100% (I)

[0081] In the above formula, A is the ordinate value of the peak and valley formed by connecting the baseline and the 002 diffraction peak curve of the XRD curve of the negative electrode material between 2Theta=10°~20°, and B is the ordinate value of the peak value of the 002 diffraction peak in the XRD curve of the negative electrode material.

[0082] In the above scheme, the microscopic disorder S of the negative electrode material of this application is 65% to 80%, which indicates that the disorder of the graphite microcrystal units in the negative electrode material is appropriate, and the graphite microcrystal gaps inside the negative electrode material have a large number of highly dispersed nano-sized pore structures with sodium storage activity. The negative electrode material has excellent sodium storage capacity and cycle performance.

[0083] The microscopic disorder of the negative electrode material in this application can specifically be 65%, 68%, 70%, 75%, and 80%, etc., or other values ​​within the above range, which are not limited here. When the microscopic disorder S of the negative electrode material is less than 65%, the arrangement disorder of the graphite microcrystalline units in the negative electrode material is too low, there are fewer nano-sized pores in the graphite microcrystalline gaps, and the capacity performance of the negative electrode material is low. When the microscopic disorder S of the negative electrode material is greater than 80%, there is a lack of effective electrical contact between the graphite microcrystalline units inside the negative electrode material, resulting in low sodium storage activity of the nano-sized pores, low capacity performance, and side reactions that easily occur during cycling to form "dead sodium," leading to a decrease in cycling performance. Preferably, the microscopic disorder of the negative electrode material is 65% to 80%, and more preferably, the microscopic disorder of the negative electrode material is 70% to 80%.

[0084] Furthermore, this application also provides a negative electrode material, which includes a carbon matrix comprising graphite microcrystalline structural units, wherein a porous structure is distributed between the graphite microcrystalline structural units, and the porosity W of the negative electrode material is 10%-40%, wherein:

[0085] W = V 孔 / (V 孔 +1 / ρ)*100% (II)

[0086] In the above formula, ρ is the true density, with units of cm. 3 / g;V 孔 Porosity W is the pore volume, which is the total pore volume of a single point adsorption obtained by nitrogen adsorption method, and the unit is cm3 / g. The physical meaning of porosity W of negative electrode material is: the average ratio between the pore volume contained in the negative electrode material particles and the total volume of the particles (pore volume + carbon matrix volume), where the volume of carbon matrix = 1 / ρ.

[0087] The porosity W of the negative electrode material in this application can specifically be 10%, 15%, 20%, 25%, 30%, 35%, and 40%, etc., or other values ​​within the above range, which are not limited here. When the porosity of the negative electrode material is less than 10%, the pore volume of the negative electrode material is too small, the number of active sodium storage sites provided by the pores is too small, and the capacity performance of the negative electrode material is low. When the porosity of the negative electrode material is greater than 40%, the volume ratio of the pores that can actively store sodium is too small, the capacity performance of the negative electrode material is also low, and the inactive sodium storage pore structure is prone to electrochemical side reactions during cycling, resulting in low cycling performance. Preferably, the porosity of the negative electrode material is 15% to 35%, and more preferably, the porosity of the negative electrode material is 20% to 30%.

[0088] In some embodiments, the pore volume V of the negative electrode material 孔 It is 0.05cm 3 / g~0.35cm 3 / g, specifically, the pore volume V of the negative electrode material. 孔 It is 0.05cm 3 / g, 0.10cm 3 / g, 0.15cm 3 / g, 0.20cm 3 / g, 0.25cm 3 / g, 0.30cm 3 / g and 0.35cm 3 / g, etc., can also be other values ​​within the above range, and are not limited here. Preferably, the pore volume V of the negative electrode material is... 孔 It is 0.08cm 3 / g~0.2cm 3 / g.

[0089] In some embodiments, the true density ρ of the negative electrode material is 1.2 g / cm³. 3 ~2.2g / cm 3 Specifically, the true density ρ of the negative electrode material is 1.2 g / cm³. 3 1.3g / cm 3 14g / cm 3 1.5g / cm 3 1.6g / cm 3 1.7g / cm 3 1.8g / cm 3 1.9g / cm 3 2.0g / cm 3 2.1g / cm 3 and 2.2g / cm 3 Of course, other values ​​within the above range are also possible and are not limited here. Preferably, the true density ρ of the negative electrode material is 1.5 cm³.3 / g~2.0cm 3 / g.

[0090] In some embodiments, the graphite microcrystalline structure unit of the negative electrode material is composed of several layers of graphene carbon layers arranged in parallel. The carbon layer spacing of the negative electrode material is 0.34 nm to 0.40 nm. Specifically, the carbon layer spacing of the negative electrode material can be, for example, 0.34 nm, 0.35 nm, 0.36 nm, 0.37 nm, 0.38 nm, 0.39 nm and 0.40 nm, etc., or other values ​​within the above range, which are not limited here.

[0091] In some embodiments, the median particle size of the negative electrode material is 1 μm to 40 μm. Specifically, the median particle size of the negative electrode material can be, for example, 1 μm, 5 μm, 10 μm, 20 μm, 30 μm and 40 μm, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0092] In some embodiments, the specific surface area SA of the negative electrode material is: 5m² 2 / g<SA≤250m 2 / g, specifically, the specific surface area SA of the negative electrode material can be, for example, 8m². 2 / g, 10m 2 / g、20m 2 / g, 50m 2 / g、70m 2 / g, 100m 2 / g, 150m 2 / g、180m 2 / g、200m 2 / g、230m 2 / g、245m 2 / g and 250m 2 / g, etc., can also be other values ​​within the above range, and are not limited here.

[0093] In some embodiments, the powder conductivity of the negative electrode material is 30 S / cm to 55 S / cm. Specifically, the powder conductivity of the negative electrode material can be, for example, 30 S / cm, 35 S / cm, 40 S / cm, 41 S / cm, 42 S / cm, 43 S / cm, 44 S / cm, 45 S / cm, 46 S / cm, 47 S / cm, 48 S / cm, 49 S / cm, 50 S / cm, 53 S / cm, and 55 S / cm, etc., and of course, other values ​​within the above range are also possible and are not limited here. Preferably, the powder conductivity of the negative electrode material is 40 S / cm to 50 S / cm.

[0094] In some embodiments, the oxygen content of the negative electrode material is 0.1% to 1.0%. Specifically, the oxygen content of the negative electrode material can be, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, and 1.0%, etc., and of course, other values ​​within the above range are also possible and are not limited herein. The applicant has found that controlling the oxygen content of the negative electrode material within the above range is beneficial to improving the sodium storage capacity of the negative electrode material and the electrolyte wettability of the carbon material, and also results in a higher initial efficiency. Preferably, the oxygen content of the negative electrode material is 0.2% to 0.6%.

[0095] In some embodiments, the oil absorption value of the negative electrode material is 45 mL / 100g to 90 mL / 100g. Specifically, the oil absorption value of the negative electrode material can be, for example, 45 mL / 100g, 50 mL / 100g, 55 mL / 100g, 60 mL / 100g, 70 mL / 100g, 80 mL / 100g, and 90 mL / 100g, etc., or other values ​​within the above range, which are not limited here. It is understood that the oil absorption value is used to characterize the pore structure of the nanopores formed by the disordered stacking of graphite microcrystals in the negative electrode material. The greater the number of pores, the larger the pore size, and the larger the pore volume, the greater the oil absorption value. An oil absorption value within the above-defined range indicates that the negative electrode with an oil absorption value of 45 mL / 100g to 90 mL / 100g has the optimal sodium storage pore structure, thereby possessing the optimal sodium storage capacity and cycle performance. The applicant discovered that when the oil absorption value is below 45 mL / 100 g, the negative electrode material lacks nanopores to provide sodium storage sites, resulting in a low sodium storage capacity. When the oil absorption value is above 90 mL / 100 g, the graphite microcrystals of the negative electrode are too porous and / or contain many defects. It is difficult to form an electric field sufficient to ensure sodium ion filling / extraction within the pores between the graphite microcrystals, leading to numerous side reactions during charge and discharge, thus resulting in poor sodium storage capacity and cycle performance. Preferably, the oil absorption value of the negative electrode material is between 60 mL / 100 g and 90 mL / 100 g.

[0096] In some embodiments, the negative electrode material includes soft carbon and hard carbon.

[0097] In some embodiments, the negative electrode material is shown in the Raman spectrum obtained by Raman spectroscopy using a measuring light source with a wavelength of 532 nm, at a wavelength of 1000 cm⁻¹. -1 Up to 1400cm -1 G-band was observed at 1500 cm. -1 Up to 2000cm -1 The D band was observed, and the peak intensity I of the D band was... D With the peak intensity I of the G-band G The ratio between I D / I G The values ​​range from 1.1 to 1.7. The peak value of the D band is at 1350 cm⁻¹. -1Nearby, the peak value of the G-band is at 1600 cm. -1 Nearby. Specifically, the peak intensity I of band D. D With the peak intensity I of the G-band G The ratio between I D / I G It can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, and 1.7, or other values ​​within the above range; no limitation is made here. The peak intensity I of the D band... D With the peak intensity I of the G-band G Controlling the ratio between them within the above range is beneficial for obtaining anode materials with low surface defect rate, few surface functional groups, and suitable microscopic order. When I D / I G When the ratio is less than 1.1, the surface defect rate of the negative electrode material is large, and there are many surface functional groups; when I D / I G When the ratio is greater than 1.7, the pore structure of the negative electrode material collapses, and the sodium storage capacity decreases. Preferably, I D / I G It is 1.3 to 1.5.

[0098] This application also provides a method for preparing the above-mentioned negative electrode material, such as... Figure 2 As shown, it includes the following steps:

[0099] Step S100: After mixing the carbon source and the modifying additive, a first heat treatment is performed to obtain a first precursor, wherein the modifying additive includes RM compound, wherein R includes an organic functional group and M includes a metal element.

[0100] Step S200: The first precursor is pre-carbonized to obtain the second precursor.

[0101] Step S300: The second precursor is acid-washed and subjected to a second heat treatment to obtain the negative electrode material.

[0102] In the above scheme, a modified additive containing organic functional group R and metal element M is mixed with a carbon source and then subjected to a first heat treatment to obtain a first precursor with a "rigid structure". The metal element is highly dispersed within the first precursor and its position is fixed, exhibiting strong chemical bonding with adjacent groups. This characteristic provides favorable conditions for increasing the microscopic disorder of the negative electrode and constructing a large number of highly dispersed nanopores. The first precursor is then pre-carbonized to obtain a second precursor. Metal elements in similar positions within the material are transformed into nano-metal oxide microcrystals, and the carbon-containing components are transformed into graphite microcrystalline units. The nano-metal oxide microcrystals hinder the ordered arrangement of graphite microcrystals, increasing the microscopic disorder of the negative electrode and causing the graphite microcrystalline units to be highly disordered. This results in a large number of highly dispersed nanoporous structures within the material, providing favorable conditions for sodium storage. Finally, the second precursor is acid-washed to remove the nano-metal oxide microcrystals, resulting in a large number of highly dispersed nano-sized pore structures inside the material, providing favorable conditions for sodium storage. After a second heat treatment, the structural defects (dangling bonds, free radicals, etc.) of the negative electrode material are burned off, improving the powder conductivity, reducing polarization, and improving the electrical contact environment of the nanopores. This increases the sodium storage electrochemical activity of the negative electrode pore structure, significantly improving the sodium storage capacity and cycle performance, ultimately obtaining a high-capacity, fast-chargeable, and long-life negative electrode material for sodium-ion batteries.

[0103] like Figure 3 As shown, the preparation method of this application is described in detail below with reference to the embodiments:

[0104] Step S100: After mixing the carbon source and the modifying additive, a first heat treatment is performed to obtain the first precursor.

[0105] In some embodiments, the modifying additive includes an organometallic salt, which may be abbreviated as RM compound, wherein R includes an organic functional group and M includes a metal element.

[0106] In some embodiments, the organic functional group R includes a carbonyl functional group or a combination of a carbonyl functional group and a heteroatom functional group; wherein, the carbonyl functional group includes at least one of alkyl, alkenyl, alkynyl, phenyl and carbon chains containing benzene rings, and the heteroatom functional group includes at least one of hydroxyl, aldehyde, carboxyl, amino, acyl, amide, nitro, carbonyl, carboxylate and sulfonate groups; preferably, the organic functional group includes a combination of a carbonyl functional group and a heteroatom functional group, and more preferably, the organic functional group includes a combination of a carbonyl functional group and a heteroatom functional group, and the heteroatom functional group includes at least one of hydroxyl, carboxyl and amino groups.

[0107] In some embodiments, the metal element M includes at least one selected from lithium, sodium, magnesium, potassium, calcium, zinc, copper, and tin.

[0108] In some embodiments, the RM compound includes R′(OH). x (COO) y M 1 / z ] i , where x, y, z, i are positive integers, R′ includes organic functional groups, and M includes metallic elements.

[0109] In some embodiments, the RM compound includes at least one of lithium tartrate, sodium tartrate, magnesium tartrate, potassium tartrate, calcium tartrate, zinc tartrate, copper tartrate, lithium maleate, sodium maleate, magnesium maleate, potassium maleate, calcium maleate, zinc maleate, copper maleate, lithium citrate, sodium citrate, magnesium citrate, potassium citrate, calcium citrate, zinc citrate, copper citrate, lithium glycolate, sodium glycolate, magnesium glycolate, potassium glycolate, calcium glycolate, zinc glycolate, copper glycolate, lithium salicylate, sodium salicylate, magnesium salicylate, potassium salicylate, calcium salicylate, zinc salicylate, and copper salicylate.

[0110] This application synthesizes a class of highly dispersed first precursors that are "organic and inorganic composites at the molecular level" by selecting specific modifying additives. The organic functional groups can connect hydroxyl groups and carboxylic acid groups, which can undergo addition reactions with carbon sources, thereby adding the modifying additives to the carbon source molecules. The metal elements form nano-metal oxides in the first heat treatment. The nano-metal oxides are highly dispersed inside the material, which hinders the orderly arrangement of graphite microcrystals in the negative electrode material, increases the microscopic disorder, and provides favorable conditions for constructing highly dispersed nanopores.

[0111] In some implementations, the carbon source includes a first carbon source and a second carbon source:

[0112] The first carbon source includes at least one of glucose, fructose, maltose, sucrose, thermoplastic phenolic resin, starch, cellulose, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt, and asphalt.

[0113] The second carbon source includes at least one of starch, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt, lignin, coconut shell, almond shell, walnut shell, peach kernel shell, peanut shell, pistachio shell, hazelnut shell, sawdust, and straw.

[0114] In some embodiments, when the carbon source is a first carbon source, the process of mixing the carbon source with a modifying additive and then performing a first heat treatment to obtain the first precursor specifically includes: mixing the first carbon source with the modifying additive and then sequentially performing a first addition reaction and a first curing reaction to obtain the first precursor. In some embodiments, the mass ratio of the first carbon source to the modifying additive is (40:60) to (99:1). The mass ratio of the first carbon source to the modifying additive can be 99:1, 90:10, 80:20, 70:30, 60:40, 50:50, 40:60, etc., and of course, other values ​​within the above range are also possible and are not limited here. Controlling the mass ratio of the modifying additive to the first carbon source within the above range is beneficial to improving the disorder of the graphite microcrystal arrangement in the negative electrode and constructing a large number of dispersed nanopores.

[0115] In some embodiments, the temperature of the first addition reaction is 80°C to 160°C. For example, the temperature of the first addition reaction can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C and 160°C, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0116] In some embodiments, the time for the first addition reaction is 0.5h to 24h. For example, the time for the first addition reaction can be 0.5h, 1h, 2h, 5h, 8h, 10h, 12h, 16h, 18h, 20h, 22h and 24h, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0117] In some embodiments, before the first curing reaction, the step of mixing the reaction product of the first carbon source and the modified additive with the curing agent is further included. Specifically, step S100 includes: mixing the first carbon source and the modified additive to carry out an addition reaction, and then mixing the material obtained from the addition reaction with the first curing agent to carry out a curing reaction to obtain the first precursor.

[0118] In some embodiments, the first curing agent includes at least one selected from ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate.

[0119] In some embodiments, the mass ratio of the first carbon source to the first curing agent is (60:40) to (95:5). The mass ratio of the first carbon source to the curing agent can be 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, 65:35, and 60:40, etc., or other values ​​within the above range, which are not limited here.

[0120] In some embodiments, when the carbon source is a second carbon source, the first precursor is obtained by mixing the second carbon source, the modifying additive, and the second curing agent and then performing a first heat treatment. Specifically, this includes mixing the second carbon source, the modifying additive, and the second curing agent and then simultaneously performing a second addition reaction and a second curing reaction to obtain the first precursor.

[0121] In some embodiments, the temperatures at which the second addition reaction and the second curing reaction occur simultaneously can be, for example, 80°C, 90°C, 100°C, 120°C, 150°C, 170°C, 200°C, 230°C, 250°C, 280°C, and 300°C, or other values ​​within the above ranges, without limitation. Temperatures above 300°C result in uneven curing, numerous defect sites and pores in the target product, and accompanying side reactions, leading to material expansion and unsuitability for industrial production. Temperatures below 80°C result in slow curing rates and incomplete reactions, failing to obtain a first precursor with a rigid cross-linked structure, making it difficult to fix the positions of metal elements, resulting in metal oxides transformed from metal elements, low structural order in the obtained negative electrode material, small number and volume of nanopores, and decreased sodium storage capacity.

[0122] In some embodiments, the time for the simultaneous second addition reaction and the second curing reaction is 0.5h to 24h. The time for the simultaneous second addition reaction and the second curing reaction can be, for example, 0.5h, 1h, 2h, 5h, 8h, 10h, 12h, 16h, 18h, 20h, 22h and 24h, etc. Of course, other values ​​within the above range are also possible and are not limited here.

[0123] In some embodiments, the second curing agent includes at least one selected from ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate.

[0124] In some embodiments, the mass ratio of the second carbon source to the second curing agent is (60:40) to (100:0) (inclusive). The mass ratio of the second carbon source to the curing agent can be 100:0, 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, 65:35, and 60:40, etc., and of course, other values ​​within the above range are also possible, without limitation. It is understood that when the second carbon source is used as a raw material, the second carbon source and the modified additive undergo an addition reaction under the second heat treatment conditions. Since the second carbon source is a thermosetting raw material, after the addition reaction, no further curing agent needs to be added for the curing reaction to proceed. Of course, a second curing agent can also be used to increase the efficiency of the curing reaction.

[0125] In some embodiments, the first carbon source, the second carbon source, and the modifying additive all need to be pulverized and sieved before use. Specifically, before mixing the first carbon source and the modifying additive, the process further includes a first pulverization and a first sieve of the first carbon source and the modifying additive; or before mixing the second carbon source and the modifying additive, the process further includes a second pulverization and a second sieve of the second carbon source and the modifying additive.

[0126] In some embodiments, the equipment for the first and / or second pulverization includes at least one of ball milling equipment, air jet milling equipment, and mechanical pulverizing equipment.

[0127] In some embodiments, the median particle size of the material obtained after the first crushing is 3mm to 3μm, for example, it can be 3mm, 10mm, 20mm, 50mm, 100mm, 300mm, 500mm, 800mm, 1μm, 2μm, and 3μm, etc., and of course, it can also be other values ​​within the above range, which are not limited here. The median particle size of the material obtained after the second crushing is 3mm to 3μm, for example, it can be 3mm, 10mm, 20mm, 50mm, 100mm, 300mm, 500mm, 800mm, 1μm, 2μm, and 3μm, etc., and of course, it can also be other values ​​within the above range, which are not limited here.

[0128] In some embodiments, the screen size of the first screening is 10 mesh to 400 mesh. The mesh size of the screen for the first screening can be, for example, 10 mesh, 20 mesh, 30 mesh, 40 mesh, 50 mesh, 60 mesh, 80 mesh, 100 mesh, 152 mesh, 180 mesh, 200 mesh, 350 mesh, 280 mesh, 320 mesh, 360 mesh, 380 mesh, and 400 mesh, etc. Of course, it can also be other values ​​within the above range, which are not limited here. The screen size for the second screening is 10 mesh to 400 mesh. For example, the screen mesh size for the second screening can be 10 mesh, 20 mesh, 30 mesh, 40 mesh, 50 mesh, 60 mesh, 80 mesh, 100 mesh, 152 mesh, 180 mesh, 200 mesh, 350 mesh, 280 mesh, 320 mesh, 360 mesh, 380 mesh, and 400 mesh, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0129] Step S200: The first precursor is pre-carbonized to obtain the second precursor.

[0130] In the above steps, the first precursor after curing does not collapse after pre-carbonization. The metal elements inside the first precursor material are transformed into nano-metal oxides, and the carbon-containing part is transformed into graphite microcrystals. The nano-metal oxides are distributed in the gaps between the graphite microcrystal units.

[0131] In some embodiments, the pre-carbonization treatment is carried out in a first protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon, and krypton.

[0132] In some embodiments, the pre-carbonization temperature is 500℃ to 800℃. For example, the pre-carbonization temperature can be 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, and 800℃, or other values ​​within the above range, which are not limited here. Within the above temperature range, as the pre-carbonization reaction temperature increases, locally adjacent nano-metal oxides merge, and the particle size increases. Therefore, the particle size and distribution of the nano-metal oxides can be controlled by the pre-carbonization temperature. When the pre-carbonization temperature is higher than 800℃, the metal oxide particle size is too large, ultimately leading to phase separation between the carbon matrix and the metal oxide. The metal oxide cannot improve the microscopic disorder of the carbon matrix, and the carbon matrix structure generates a large number of structural defects. When the pre-carbonization temperature is lower than 500℃, metal oxides are not generated, or the metal oxide particle size is too small to hinder the orderly growth of graphite crystals, and cannot provide favorable conditions for constructing a large number of highly dispersed nanopores.

[0133] In some embodiments, the pre-carbonization treatment time is 0.5h to 24h. The pre-carbonization treatment time can be, for example, 0.5h, 1h, 2h, 5h, 8h, 10h, 12h, 16h, 18h, 20h, 22h and 24h, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0134] In some embodiments, the equipment for pre-carbonization treatment includes at least one of a tube furnace, a box furnace, a pusher kiln, and a calcining kiln.

[0135] In some embodiments, after obtaining the second precursor through pre-carbonization treatment, the process further includes a third crushing and a third sieving step on the second precursor.

[0136] In some embodiments, the median particle size of the material obtained from the third crushing can be, for example, 3 mm, 10 mm, 20 mm, 50 mm, 100 mm, 300 mm, 500 mm, 800 mm, 1 μm, 2 μm, and 3 μm, or other values ​​within the above range, which are not limited here.

[0137] In some embodiments, the screen size of the third screening is 10 mesh to 400 mesh. The mesh size of the screen gear of the third screening can be, for example, 10 mesh, 20 mesh, 30 mesh, 40 mesh, 50 mesh, 60 mesh, 80 mesh, 100 mesh, 152 mesh, 180 mesh, 200 mesh, 350 mesh, 280 mesh, 320 mesh, 360 mesh, 380 mesh and 400 mesh, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0138] Step S300: The second precursor is acid-washed and subjected to a second heat treatment to obtain the negative electrode material.

[0139] In some embodiments, the acid solution used for pickling includes a solution of at least one selected from hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, acetic acid, oxalic acid, benzoic acid, hydrosulfuric acid, hydrobromic acid, and hydroiodic acid.

[0140] In some embodiments, the mass ratio of the second precursor to the pickling acid is 1:(3-15). Specifically, the mass ratio of the second precursor to the pickling acid can be, for example, 1:3, 1:5, 1:7, 1:9, 1:12 and 1:15, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0141] In some embodiments, the mass concentration of the pickling acid solution is 10% to 50%. Specifically, the mass concentration of the pickling acid solution can be, for example, 10%, 20%, 30%, 40%, and 50%, or other values ​​within the above range, which are not limited here.

[0142] In some embodiments, pickling further includes steps of impregnation, solid-liquid separation, washing, and drying of the pickled material.

[0143] In some embodiments, the immersion treatment time is 1 hour to 24 hours. The immersion treatment time can be, for example, 1 hour, 2 hours, 5 hours, 8 hours, 10 hours, 12 hours, 16 hours, 18 hours, 20 hours, 22 hours and 24 hours, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0144] In some embodiments, the solid-liquid separation method includes at least one of centrifugation and filtration.

[0145] In some embodiments, the pH of the material obtained after washing is 4 to 7.

[0146] In some embodiments, the drying equipment is at least one of an oven, a double cone dryer, a pusher kiln, a box furnace, and a spray dryer.

[0147] In some embodiments, the second heat treatment is carried out in a second protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon, and krypton.

[0148] In some embodiments, the temperature of the second heat treatment is 900℃ to 1800℃. For example, the temperature can be 900℃, 1000℃, 1100℃, 1200℃, 1300℃, 1400℃, 1500℃, 1600℃, 1700℃, and 1800℃, or other values ​​within the above range, which are not limited here. Preferably, the temperature of the second heat treatment is 1200℃ to 1700℃. When the second heat treatment temperature is below 900℃, the oxidation content on the surface of the nanopores of the negative electrode is too high, the powder conductivity is low, the sodium storage activity of the nanopores is low, and there are many electrochemical side reactions, resulting in low capacity and initial efficiency. When the second heat treatment temperature is above 1800℃, the microscopic disorder of the negative electrode decreases, the pore volume and interstitial space of the nanopores decrease, and the sodium storage capacity decreases.

[0149] In some embodiments, the equipment for the second heat treatment includes at least one of a tube furnace, a box furnace, a pusher kiln, a graphitization furnace, and a calcining kiln.

[0150] In some embodiments, this application provides a sodium-ion battery comprising a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The negative electrode includes a current collector and a negative active material layer. The negative active material layer includes a negative active material, a conductive agent, and a binder. The positive active material layer may include a positive active material, a conductive agent, and a binder. The positive current collector may be Al foil, or other positive current collectors commonly used in the art. The negative active material includes the aforementioned negative electrode material.

[0151] In some embodiments, the current collector of the negative electrode may include at least one of copper foil, aluminum foil, nickel foil, or fluorocarbon current collector. The binder may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinylpyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, polystyrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin, or polyfluorene.

[0152] In some embodiments, the binder in the positive electrode sheet may include at least one of polyvinylidene fluoride, a copolymer of polyvinylidene fluoride and hexafluoropropylene, a styrene-acrylate copolymer, a styrene-butadiene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene. The positive electrode active material includes, but is not limited to, at least one of sodium-transition metal oxides, sodium-transition metal phosphates and variants, sodium-transition metal sulfates, and sodium-transition metal Prussian blue compounds; these positive electrode active materials may be doped or coated.

[0153] In some embodiments, the separator includes at least one selected from polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, aramid, or glass fiber. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene. In some embodiments, the thickness of the separator is in the range of about 5 μm to 500 μm.

[0154] In some embodiments, the sodium-ion battery may further include an electrolyte. In some embodiments, the electrolyte is composed of a sodium salt (NaClO4, NaPF6, etc.) and a solvent, the solvent including but not limited to at least two of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC), propylene carbonate (PC), and propyl propionate (PP). Furthermore, the electrolyte may additionally include at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), or a dinitrile compound as an electrolyte additive.

[0155] A sodium-ion battery is made by sequentially winding or stacking positive electrode sheets, separator membrane, and negative electrode sheets into an electrode assembly, then encapsulating it in an aluminum-plastic film, injecting electrolyte, forming, and sealing.

[0156] The present application will be further described below through specific embodiments.

[0157] Example 1

[0158] S100: After crushing, thermoplastic phenolic resin and sodium tartrate are sieved through a 30-mesh sieve and mixed at a mass ratio of 50:50. The mixture is heated to 150°C in a forced-air oven and kept at that temperature for 3 hours. After cooling, it is crushed and sieved through a 30-mesh sieve. The resulting material is mixed with crushed and sieved hexamethylenetetramine at a mass ratio of 90:10. The mixture is then transferred to a forced-air oven and heat-treated at 150°C for 2 hours. After cooling and crushing, the first precursor is obtained.

[0159] S200: The first precursor is put into a box furnace and heat-treated at 600°C for 3 hours under a nitrogen atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0160] S300: Mix the second precursor, hydrochloric acid and deionized water in a mass ratio of 1:1:3, stir for 2 hours, centrifuge, wash until pH=4-6, dry in a double cone dryer, and pulverize in an airflow to a median particle size of about 10μm. Transfer the obtained material to a box furnace and sinter at 1300℃ for 3 hours under a nitrogen atmosphere. Cool, mix with VC, and sieve through a 325 mesh to obtain the negative electrode material.

[0161] like Figure 4The image shown is a SEM image of the negative electrode material prepared in this embodiment. This negative electrode material includes a carbon matrix composed of graphite microcrystalline structural units. Pores are distributed between the graphite microcrystalline structural units. The microscopic disorder S, carbon interlayer spacing, and Raman spectroscopy of the negative electrode material are also shown. D / I G The results of peak intensity ratio, oxygen content, oil absorption value and median particle size test are shown in Table 1.

[0162] Example 2

[0163] Unlike Example 1, step S100 is adjusted as follows: the crushed and sieved thermoplastic phenolic resin, sodium tartrate, and hexamethylenetetramine are mixed in a mass ratio of 45:45:10, treated in a forced-air drying oven at 150°C for 5 hours, cooled, crushed, and sieved using a 30-mesh screen to obtain the first precursor.

[0164] Example 3

[0165] S100: Thermosetting phenolic resin and sodium citrate are crushed and sieved through a 30-mesh screen, and mixed at a mass ratio of 60:40. The resulting mixture is heated to 100°C in a forced-air drying oven and kept at that temperature for 2 hours. After cooling, it is crushed and sieved through a 100-mesh screen. The resulting mixture is then mixed with melamine at a mass ratio of 80:20. The mixture is then transferred to a box furnace and heat-treated at 170°C for 1 hour. After cooling and crushing, the first precursor is obtained.

[0166] S200: The first precursor is put into a box furnace and heat-treated at 700°C for 2 hours under a nitrogen atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0167] S300: The second precursor, 90% sulfuric acid, and deionized water are mixed in a mass ratio of 1:1.5:5, stirred for 2 hours, centrifuged, washed until pH=4-6, dried in a forced-air oven, mechanically pulverized to a median particle size of about 30μm, and the resulting material is transferred to a tube furnace and sintered at 1200℃ for 5 hours under an argon atmosphere. After cooling, VC is mixed and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0168] Example 4

[0169] Unlike Example 3, S100 is adjusted to: no curing agent (melamine) is added during the curing process. That is, the thermosetting phenolic resin and sodium citrate are crushed, sieved through a 30-mesh sieve, mixed in a mass ratio of 60:40, heated to 100°C in a forced-air oven, kept at that temperature for 2 hours, cooled, crushed, sieved through a 100-mesh sieve, and the resulting material is transferred to a box furnace for heat treatment at 170°C for 1 hour, cooled, crushed, and the first precursor is obtained.

[0170] Example 5

[0171] S100: Corn starch and zinc salicylate are crushed and sieved through a 30-mesh sieve, and mixed at a mass ratio of 70:30. The resulting mixture is heated to 120°C in a forced-air drying oven and kept at that temperature for 4 hours. After cooling, it is crushed and sieved through a 30-mesh sieve to obtain the first precursor. The obtained material is mixed with ammonium chloride sieved through a 30-mesh sieve at a mass ratio of 85:15. The mixture is then transferred to a box furnace and heat-treated at 300°C for 24 hours. After cooling, it is crushed to obtain the first precursor.

[0172] S200: The first precursor is put into a box furnace and heat-treated at 650°C for 5 hours in a krypton atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0173] S300: The second precursor, phosphoric acid, and deionized water are mixed in a mass ratio of 1:3:10, stirred for 2 hours, centrifuged, washed until pH=4-6, dried in a box furnace, and pulverized by air jet milling to a median particle size of about 6μm. The resulting material is transferred to a box furnace and sintered at 1500℃ for 24 hours under a helium atmosphere. After cooling, VC is mixed and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0174] Example 6

[0175] S100: Sucrose and copper glycolate are crushed and sieved through a 30-mesh sieve, mixed in a mass ratio of 85:15, heated to 180°C in a forced-air oven, kept at that temperature for 3 hours, cooled, crushed, and sieved through a 30-mesh sieve. The resulting material and melamine are added to a 20% formaldehyde ethanol solution and heated to 75°C with stirring. The mass ratio of the resulting material, melamine, and 20% formaldehyde ethanol solution is 7:1:2. Stirring is continued for 1 hour, and the solvent is further evaporated with stirring to obtain a solid block. The solid block is transferred to a forced-air oven and heat-treated at 170°C for 3 hours, cooled, and crushed to obtain the first precursor.

[0176] S200: The first precursor is put into a box furnace and heat-treated at 600°C for 4 hours in a xenon atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0177] S300: The second precursor, sulfuric acid, and deionized water are mixed in a mass ratio of 1:0.5:5, stirred for 2 hours, centrifuged, washed until pH=4-6, dried in a double cone dryer, ball-milled to a median particle size of about 8μm, and the resulting material is transferred to a tube furnace and sintered at 1700℃ for 1 hour under an argon atmosphere. After cooling, VC is mixed and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0178] Example 7

[0179] S100: Walnut shells are crushed using a crusher and screened with a 3mm sieve to obtain walnut shell powder. The walnut shell powder and magnesium maleate are mixed in a mass ratio of 40:60, heated to 140℃ in a forced-air drying oven, kept at that temperature for 24 hours, cooled, crushed, and screened with a 30-mesh sieve. The resulting material is then transferred to a box furnace for heat treatment at 300℃ for 1 hour, cooled, and crushed to obtain the first precursor.

[0180] S200: The first precursor is put into a box furnace and heat-treated at 900°C for 2 hours in a neon atmosphere. After cooling, crushing, and sieving with a 30-mesh sieve, the second precursor is obtained.

[0181] S300: The second precursor, hydrochloric acid and deionized water are mixed in a mass ratio of 1:2:4, stirred for 2 hours, centrifuged, washed until pH=4-6, dried in a box furnace, and air-jet pulverized to a median particle size of about 6μm. The resulting material is transferred to a roller kiln and sintered at 1400℃ for 3 hours under a nitrogen atmosphere. After cooling, VC is mixed and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0182] Example 8

[0183] S100: High-temperature asphalt is fed into a rotary kiln, air is introduced, the temperature is raised to 230℃ and held for 2 hours, then cooled to obtain oxidized asphalt. The oxidized asphalt and calcium citrate are crushed and sieved through a 30-mesh screen, and mixed at a mass ratio of 80:20. The mixture is then kept at 140℃ for 6 hours in a forced-air drying oven, cooled, crushed, and sieved through a 30-mesh screen. The resulting mixture is then mixed with crushed and sieved ammonium carbonate at a mass ratio of 90:10, transferred to a forced-air drying oven, heat-treated at 180℃ for 2 hours, cooled, and crushed to obtain the first precursor.

[0184] S200: The first precursor is put into a box furnace and heat-treated at 500°C for 3 hours under a nitrogen atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0185] S300: The second precursor, hydrobromic acid, and deionized water are mixed in a mass ratio of 1:1:3, stirred for 2 hours, centrifuged, washed until pH=4-6, dried in a forced-air drying oven, and air-jet pulverized to a median particle size of about 8μm. The resulting material is transferred to a box furnace and sintered at 900℃ for 3 hours under an argon atmosphere. After cooling, VC is mixed and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0186] Example 9

[0187] Unlike Example 1, the pre-carbonization temperature in S200 is 400°C. That is, in S200, the first precursor is put into a box furnace and heat-treated at 400°C for 3 hours in a nitrogen atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0188] Example 10

[0189] Unlike Example 1, the pre-carbonization temperature in S200 is 900°C. That is, in S200, the first precursor is put into a box furnace and heat-treated at 900°C for 3 hours under a nitrogen atmosphere. After cooling, crushing, and sieving through a 30-mesh sieve, the second precursor is obtained.

[0190] Example 11

[0191] Unlike Example 1, the second heat treatment temperature in S300 is 850°C. That is, S300 is as follows: the second precursor, hydrobromic acid and deionized water are mixed in a mass ratio of 1:1:3, stirred for 2 hours, centrifuged, dried in a forced-air drying oven, pulverized by airflow to a median particle size of about 8 μm, transferred to a box furnace and sintered at 850°C for 3 hours under a nitrogen atmosphere, cooled, mixed with VC, and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0192] Example 12

[0193] Unlike Example 1, the second heat treatment temperature in S300 is 1850℃. That is, S300 is as follows: the second precursor, hydrobromic acid and deionized water are mixed in a mass ratio of 1:1:3, stirred for 2 hours, centrifuged, dried in a forced-air drying oven, air-jet pulverized to a median particle size of about 8μm, transferred to a box furnace and sintered at 1850℃ for 3 hours under a nitrogen atmosphere, cooled, mixed with VC, and sieved through a 325-mesh sieve to obtain the negative electrode material.

[0194] Example 13

[0195] Unlike Example 1, no curing agent (hexamethylenetetramine) was added in S100. That is, S100 is made by crushing and screening thermoplastic phenolic resin and sodium tartrate, mixing them in a mass ratio of 50:50, heating them to 150°C in a forced-air oven, holding them at that temperature for 3 hours, cooling them, crushing them, screening them in a 30-mesh sieve, transferring the resulting material to a forced-air oven for heat treatment at 150°C for 2 hours, cooling them, crushing them, and obtaining the first precursor.

[0196] Comparative Example 1

[0197] Unlike Example 1, no modifying additive (sodium tartrate) was added in S100. That is, S100 is as follows: thermoplastic phenolic resin is crushed, sieved through a 30-mesh sieve, heated to 150°C in a forced-air oven, kept at that temperature for 3 hours, cooled, crushed, and sieved through a 30-mesh sieve. The resulting material is mixed with crushed and sieved hexamethylenetetramine at a mass ratio of 90:10, transferred to a forced-air oven for heat treatment at 150°C for 2 hours, cooled, crushed, and the first precursor is obtained.

[0198] Performance testing

[0199] (1) SEM images of the negative electrode material were obtained using a Hitachi S4800 scanning electron microscope.

[0200] (2) XRD data were obtained using a Panalytical X'Pert PRO MPD instrument with Kα rays (wavelength λ = 0.1541 nm) from a Cu target as the light source, within the 2Theta range of 10°–90°. The carbon interlayer spacing was calculated using the (002) diffraction angle of the XRD and substituted into the Scherrer formula. To characterize the microstructure of the anode material, such as... Figure 5 As shown, the microstructural disorder S is defined as follows:

[0201] Microscopic disorder S = (A / B) * 100% (I)

[0202] In the formula, A is the ordinate value of the valley of the XRD curve of the negative electrode between 2Theta = 10° and 20°, formed by connecting the baseline with the 002 diffraction peak curve, and B is the ordinate value of the peak value of the 002 diffraction peak of the negative electrode XRD. Disorder is used to characterize the degree of disorder in the microstructure of the negative electrode material. When the microstructure of the negative electrode is non-porous and highly crystalline (e.g., the negative electrode is graphite), A is much smaller than B, and its disorder is close to 0. When the microstructure of the negative electrode is highly porous and the graphite crystals are arranged in a highly disordered manner, A ≈ B, and its disorder is close to 100%.

[0203] (3) Raman spectra were measured using a Raman spectrometer. The test conditions were: He-Ne laser (wavelength 532 nm), 10% filter, 500 μm aperture, 100 μm slit, 1800 gr / mm grating, 60 s exposure time, 2 exposures, 50XLwd microscope objective, and 800 cm² test range. -1 ~2000cm -1 The D peak is at 1350 cm. -1 Nearby, G peak is at 1600cm -1 Nearby. Randomly select 20 points to test Raman IF. D / I G The peak intensity ratio (i.e., the ratio of the peak value of D to the peak value of G on the ordinate), taken as the average value, is the I of the negative electrode material. D / I G Peak intensity ratio.

[0204] (4) Nitrogen adsorption tests were performed at 77 K using a McMeter meter (model ASAP2460) to obtain the specific surface area and pore volume. The specific surface area was calculated using the BET formula (unit: m³). 2 / g), pore volume V 孔 This represents the total pore volume of single-point adsorption (unit: cm³ / g).

[0205] (5) The true density ρ was tested using a Bestech 3H-2000TD tester, using helium gas. The unit is cm³. 3 / g; To characterize the pore structure features of the negative electrode material provided in this application, the porosity W is defined as:

[0206] W = V 孔 / (V 孔 +1 / ρ)*100% (II)

[0207] In the above formula, V 孔 ρ is the pore volume, i.e., the total pore volume of adsorption at a single point, expressed in cm³ / g; ρ is the true density, expressed in cm³ / g. 3 / g; The physical meaning of porosity is the average ratio between the pore volume contained in the negative electrode material particles and the total volume of the particles (pore volume + carbon matrix volume), where the volume of the carbon matrix = 1 / ρ.

[0208] (5) Powder conductivity was tested using a Mitsubishi Chemical MCP-PD51 powder resistivity tester. Test conditions: A certain amount of powder material was placed in the sample cell, and the powder conductivity was measured under a pressure of 20 kN. The unit is S / cm.

[0209] (6) The oil absorption value was tested using the Japanese ASAHI S500. The test method was to add 20g of powder sample to the sample cell, add linseed oil, start the test, and the oil absorption value data was obtained, with the unit being mL / 100g.

[0210] (7) Oxygen content test. The oxygen content in the sample was tested using an ONH-2000 elemental analyzer by burning method.

[0211] (8) The specific button cell negative electrode sheet is prepared using a method known in the art: the negative electrode material, conductive agent, and binder are mixed in a mass percentage ratio of 91:3:6, adjusted to a solid content of 50% with deionized water, and then uniformly mixed. The mixture is coated onto a copper foil current collector, vacuum dried, and sliced ​​to obtain the negative electrode sheet. The electrode sheet has a diameter of 14 mm and an areal density of 5.5 ± 0.5 mg / cm³. 2 ;

[0212] Button cell fabrication: A sodium sheet is used as the counter electrode, 1 mol / L NaPF6 / DIGLYME (100 Vol%) is used as the electrolyte, glass fiber filter paper is used as the separator, and a 2032 button cell casing is used for the outer shell. The negative electrode, counter electrode, electrolyte, separator and battery casing are assembled to obtain the button cell.

[0213] The sodium storage specific capacity and initial efficiency of the materials obtained in Examples 1-13 and Comparative Example 1 were tested under the following conditions: at room temperature, on the ARBIN battery testing system, first charged at a constant current of 0.1C to 5mV, and then charged at a constant voltage of 5mV to a current density of 3.5*10. -6 A. Charging cut-off; after standing, discharge again at 0.1C with a cut-off voltage of 2V. The test results are shown in Table 2. Specific capacity (mAh / g) is the initial discharge capacity divided by the weight of the negative electrode material contained in the negative electrode sheet. The nominal specific capacity is 350mAh / g. The initial efficiency is the ratio of the initial discharge capacity to the initial charge capacity.

[0214] 1C / 1C@80-cycle retention: At room temperature, coin cells that had undergone initial performance testing (specific capacity and initial efficiency) at 0.1C / 0.1C (CC+CV) were tested on the LAND battery testing system of Wuhan Jinno Electronics Co., Ltd. 1C / 1C constant current charge-discharge cycle testing was performed. The percentage of the discharge capacity at 80th week of 1C / 1C cycle divided by the discharge capacity at the first week of 1C / 1C cycle is the 1C / 1C@80-cycle retention rate. The test results are shown in Table 1.

[0215] Table 1. Parameter test results for each embodiment and comparative example

[0216]

[0217] As shown in Table 1, the specific surface area, oxygen content, oil absorption value, and microstructure disorder of the negative electrode material in Comparative Example 1 are all lower than those in Example 1. This is because the use of modified additives in S100 of Example 1 increases the microstructure disorder of the negative electrode material, thereby giving the negative electrode material a large number of dispersed nanopores. Specifically, S100 uses a carbon source and modified additives for the first heat treatment, where they undergo addition and curing reactions, followed by pre-carbonization. The carbon-containing portion of the resulting product is converted into graphite microcrystals, and the metal elements are converted into nano-metal oxides. The nano-metal oxide microcrystals hinder the orderly arrangement of graphite microcrystals, thereby increasing the microstructure disorder of the negative electrode. After acid washing and sintering, the nano-metal oxides and defects (dangling bonds, free radicals) are removed, but the disordered arrangement structure of the graphite microcrystals is still retained. Therefore, a large number of dispersed nanopores exist in the gaps between the graphite microcrystals. In addition, the oxygen-containing functional groups of the modified additives can dope the negative electrode material with oxygen, which is beneficial to improving the electrolyte wettability of the negative electrode material, thereby improving the sodium storage capacity and cycle performance. In contrast, S100 of Comparative Example 1 did not use any modifying additives, resulting in a lower degree of disorder in the arrangement of graphite microcrystals in the negative electrode material. The pore volume and number of nanopores in the interstitial spaces between the graphite microcrystals were less than those in Example 1 (e.g., ...). Figure 6 ).

[0218] The specific surface area, oil absorption value, and microstructure disorder of the negative electrode material prepared in Example 4 were lower than those in Example 3. Both examples used thermosetting raw materials and could be cured without a curing agent in S100. However, Example 3 used a curing agent, while Example 4 did not. This indicates that for thermosetting carbon sources, the curing agent in S100 can enhance the curing effect, thereby further enhancing the efficacy of the modified additives (i.e., increasing the microstructure disorder of the negative electrode material and increasing its nanoporous structure).

[0219] The specific surface area, oil absorption value, and microstructure disorder of the anode materials prepared in Examples 9 and 10 were significantly lower than those in Example 1. This is because the pre-carbonization temperature (400°C) in S200 of Example 9 was too low, resulting in only a small portion of the metal elements being converted into nano-metal oxides. Consequently, the effectiveness of the modifying additives (i.e., improving the microstructure disorder of the anode material and increasing its nanoporous structure) was weak, and the resulting anode had fewer nanopores and lower pore volume. In addition, the pre-carbonization temperature (900°C) in S200 of Example 10 was too high. During this process, most of the nano-metal oxides generated fused together, eventually resulting in the separation of the metal oxide phase and the carbon-based phase. This also weakened the effectiveness of the modifying additives (i.e., improving the microstructure disorder of the anode material and increasing its nanoporous structure), resulting in a cathode with fewer nanopores and lower sodium storage activity. As can be seen from Examples 9 and 10, both excessively high and excessively low pre-carbonization temperatures will weaken the effectiveness of the modified additives (i.e., increasing the microscopic disorder of the anode material and increasing its nanoporous structure). This indicates that controlling the pre-carbonization temperature within a certain range is necessary for preparing anode materials with high microscopic disorder and a large number of highly dispersed nanopores.

[0220] The negative electrode material prepared in Example 11 has a greater specific surface area, oxygen content, microstructure disorder, and oil absorption value than that of Example 1, while Raman spectroscopy shows that... D / I G The peak intensity ratio and powder conductivity are lower than those of Example 1. This is because the second heat treatment temperature (850°C) in S300 of Example 11 is too low, lower than that of Example 1 (1300°C), resulting in most of the defective structures (dangling bonds, free radicals, etc.) in the second precursor not being burned off during the second heat treatment, and the resulting anode material has an overly loose graphite microcrystal arrangement. Therefore, the microstructure disorder, oxygen content, and oil absorption value are relatively high, and the Raman spectroscopy results are poor. D / I G The peak intensity ratio and powder conductivity are relatively low. This indicates that an excessively low second heat treatment temperature leads to a higher degree of disorder and defect rate in the resulting anode material, while the powder conductivity is lower, which is detrimental to the sodium storage capacity of the anode material.

[0221] The negative electrode material prepared in Example 12 has lower specific surface area, carbon interlayer spacing, oxygen content, microstructure disorder, and oil absorption value than that of Example 1. Its powder conductivity and Raman spectroscopy performance are also lower. D / IG The peak intensity ratio was higher than that of Example 1. This is because the second heat treatment temperature (1850°C) in S300 of Example 12 was too high, exceeding that of Example 1 (1300°C). This caused the graphite microcrystals in the second precursor to become more ordered after the second heat treatment, resulting in a decrease in the carbon interlayer spacing. Defect structures (dangling bonds, free radicals, etc.) and most of the nanopores were burned off, thus reducing the pore volume of the nanopores. This indicates that an excessively high second heat treatment temperature leads to a lower degree of disorder in the resulting anode material, with some nanopores collapsing and a lower pore volume, which is detrimental to the sodium storage capacity of the anode material.

[0222] The specific surface area, oil absorption value, and microstructure disorder of the negative electrode material prepared in Example 13 were lower than those in Example 1. Since no curing agent (hexamethylenetetramine) was used in the preparation method of Example 3, the first precursor molecules obtained after the curing reaction did not form a fully cross-linked rigid structure. During the pre-carbonization reaction, the carbon-containing portion of the first precursor could not effectively confine the metal elements within a certain range, leading to thermal migration of the latter. This resulted in the inability to obtain a large amount of highly dispersed nano-metal oxides between the graphite microcrystals, thus limiting the effect of preventing the ordered arrangement of graphite microcrystals. This indicates that the curing agent in S100 plays a crucial role in enhancing the effectiveness of the modified additives (i.e., improving the microstructure disorder of the negative electrode material and increasing its nanoporous structure).

[0223] Table 2. Performance determination of the anode materials prepared in each example and comparative example

[0224]

[0225]

[0226] As shown in Table 2 and Figure 7 As shown, the anode materials prepared in Examples 1-8 have a specific capacity of 311-452 mAh / g, an initial efficiency of 86.1%-94.3%, and a 1C / 1C@80-cycle retention rate of 85%-91%, exhibiting excellent electrochemical performance. This indicates that the anode materials provided by the present invention have excellent characteristics such as high capacity, high initial efficiency, and good cycle performance.

[0227] The sodium storage specific capacity and initial efficiency of Example 1 are both higher than those of Comparative Example 1. This is because the graphite microcrystal arrangement of the negative electrode material obtained in Example 1 has a high degree of microscopic disorder, and the interstices of the graphite microcrystals have a large number of dispersed nanopore structures, which have sodium storage activity. In contrast, Comparative Example 1 did not use any modifying additives in S100, resulting in low microscopic disorder and a small number and volume of nanopores with active sodium storage activity. Therefore, its sodium storage capacity is lower than that of Example 1. The main improvement of reversible capacity in Example 1 is achieved by increasing sodium storage through nanopores. Moreover, this mechanism of sodium storage has high reversibility and has little or no effect on the irreversible capacity of SEI film formation. Therefore, its initial efficiency is higher than that of Comparative Example 1.

[0228] The specific capacity and initial efficiency of the anode material in Example 1 were higher than those in Examples 9 and 10. This is because the pre-carbonization temperatures in Examples 9 and 10 were either too high or too low, resulting in lower microscopic disorder, fewer nanopores, and more defect structures in the anode materials. Consequently, their sodium storage specific capacity, initial efficiency, and 1C / 1C@80 cycle retention were lower. This indicates that controlling the pre-carbonization temperature within a certain range is necessary for preparing anode materials with high microscopic disorder and a large number of highly dispersed nanopores.

[0229] The sodium storage specific capacity, initial efficiency, and 1C / 1C@80 cycle retention rate of the anode material in Example 1 were all higher than those in Examples 11 and 12. This is because the second heat treatment temperature (S300) in Example 11 was too low. A low second heat treatment temperature leads to higher disorder and defect rate in the resulting anode material, and lower powder conductivity, resulting in a decrease in sodium storage specific capacity, initial efficiency, and 1C / 1C@80 cycle retention rate compared to Example 1. The specific capacity and initial efficiency of the anode material in Example 1 were higher than those in Example 12. This may be because the second heat treatment temperature (S300) in Example 12 was too high, causing most of the nanopores generated in S100-S200 to collapse during the sintering process in S300, resulting in decreased microscopic disorder and a smaller number and volume of nanopores compared to Example 1. Therefore, the sodium storage specific capacity and initial efficiency of Example 12 also decreased. In addition, the second heat treatment temperature in Example 12 was too high, which reduced the carbon interlayer spacing and decreased the cycling stability of the carbon structure. Therefore, the 1C / 1C@80 cycle retention rate was lower than that in Example 1.

[0230] The 1C / 1C@80-cycle retention rate of the negative electrode of Example 1 is higher than that of Example 13. This is because the sodium storage capacity contributed by the nanopores of the negative electrode of Example 1 is highly reversible. The specific capacity, initial efficiency, and 1C / 1C@80-cycle retention rate of the negative electrode material of Example 1 are all higher than those of Example 13. This is because, compared with Example 1, no curing agent was used in step S100 of Example 13, resulting in lower microscopic disorder of the pre-carbonized negative electrode material, smaller number and pore volume of nanopores. Therefore, the specific capacity and initial efficiency of Example 13 show a significant decrease compared with Example 1. The 1C / 1C@80-cycle retention rate of Example 13 is lower because, during the second heat treatment in S300, the metal oxide and carbon-based phases separate, which leads to the generation of a large number of defect structures (such as free radicals) in the carbon structure. These structures undergo side reactions with the electrolyte during cycling, resulting in capacity decay.

[0231] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A negative electrode material, characterized in that, The negative electrode material comprises a carbon matrix, the carbon matrix comprising graphite microcrystalline structural units, and porous structures distributed between the graphite microcrystalline structural units. The microscopic disorder S of the negative electrode material is 67.76%~80%, wherein: S=(A / B) 100%(I) In the above formula, A is the ordinate value of the peak and valley formed by connecting the baseline and the 002 diffraction peak curve of the XRD curve of the negative electrode material between 2 Theta = 10° and 20°, and B is the ordinate value of the peak value of the 002 diffraction peak in the XRD curve of the negative electrode material.

2. The negative electrode material according to claim 1, characterized in that, The negative electrode material includes at least one of the following features (1) to (5): (1) The negative electrode material includes soft carbon and hard carbon; (2) The carbon interlayer spacing of the negative electrode material is 0.34 nm to 0.40 nm; (3) The pore volume V of the negative electrode material 孔 It is 0.05cm 3 / g~0.35cm 3 / g; (4) The true density ρ of the negative electrode material is 1.2 g / cm³. 3 ~2.2 g / cm 3 ; (5) The porosity W of the negative electrode material is 10%~40%, wherein: W=V 孔 / (V 孔 +1 / p) 100% (II) In the above formula, ρ is the true density, with units of g / cm³. 3 V 孔 The volume of the pore is in cm³. 3 / g; where the volume of the carbon matrix = 1 / ρ.

3. The negative electrode material according to claim 1, characterized in that, The negative electrode material includes at least one of the following features (1) to (6): (1) The median particle size of the negative electrode material is 1 μm to 40 μm; (2) The specific surface area SA of the negative electrode material is: 5 m² 2 / g<SA≤250m 2 / g; (3) The powder conductivity of the negative electrode material is 30 S / cm ~ 55 S / cm; (4) The oxygen content of the negative electrode material is 0.1%~1.0%; (5) The oil absorption value of the negative electrode material is 45 mL / 100g to 90 mL / 100g; (6) The negative electrode material is shown in the Raman spectrum obtained by Raman spectroscopy using a measuring light source with a wavelength of 532 nm. At 1000 cm⁻¹ -1 Up to 1400cm -1 G-band was observed at 1500 cm. -1 Up to 2000cm -1 The D band was observed, and the peak intensity I of the D band was... D With the peak intensity I of the G-band G The ratio between I D / I G It ranges from 1.1 to 1.

7.

4. A method for preparing the negative electrode material according to any one of claims 1 to 3, characterized in that, Includes the following steps: A first precursor is obtained by subjecting a mixture containing a carbon source and a modifying additive to a first heat treatment, wherein the modifying additive includes an RM compound, wherein R includes an organic functional group and M includes a metal element. The first precursor is pre-carbonized to obtain the second precursor, wherein the pre-carbonization temperature is 500℃~800℃. The second precursor is subjected to acid washing and a second heat treatment to obtain the negative electrode material. The temperature of the second heat treatment is 900℃~1800℃.

5. The preparation method according to claim 4, characterized in that, The method includes at least one of the following features (1) to (6): (1) The organic functional group includes a carbon-based functional group or a combination of a carbon-based functional group and a heteroatom functional group; (2) The organic functional group includes a carbon-based functional group or a combination of a carbon-based functional group and a heteroatom functional group, wherein the carbon-based functional group includes at least one of alkyl, alkenyl, alkynyl, phenyl and carbon chain containing a benzene ring; (3) The organic functional group includes a carbonyl functional group or a combination of a carbonyl functional group and a heteroatom functional group, wherein the heteroatom functional group includes at least one of hydroxyl, aldehyde, carboxyl, amino, acyl, amide, nitro, carbonyl, carboxylate and sulfonate groups; (4) The metallic element includes at least one of lithium, sodium, magnesium, potassium, calcium, zinc, copper and tin; (5) The RM compound includes R'(OH) x (COO) y M 1 / z ] i , where x, y, z, and i are positive integers, and R' includes organic functional groups; (6) The RM compound includes at least one of lithium tartrate, sodium tartrate, magnesium tartrate, potassium tartrate, calcium tartrate, zinc tartrate, copper tartrate, lithium maleate, sodium maleate, magnesium maleate, potassium maleate, calcium maleate, zinc maleate, copper maleate, lithium citrate, sodium citrate, magnesium citrate, potassium citrate, calcium citrate, zinc citrate, copper citrate, lithium glycolate, sodium glycolate, magnesium glycolate, potassium glycolate, calcium glycolate, zinc glycolate, copper glycolate, lithium salicylate, sodium salicylate, magnesium salicylate, potassium salicylate, calcium salicylate, zinc salicylate, and copper salicylate.

6. The preparation method according to claim 4, characterized in that, The carbon source includes a first carbon source, and the first heat treatment of the mixture containing the first carbon source and the modifying additive to obtain the first precursor includes: mixing the first carbon source and the modifying additive and then performing a first addition reaction and a first curing reaction sequentially to obtain the first precursor; the method includes at least one of the following features (1) to (10): (1) The first carbon source includes at least one of glucose, fructose, maltose, sucrose, thermoplastic phenolic resin, starch, cellulose, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt and asphalt; (2) The mass ratio of the first carbon source to the modified additive is (40:60) to (99:1). (3) The temperature of the first addition reaction is 80℃~160℃; (4) The time for the first addition reaction is 0.5 h ~ 24 h; (5) The first curing reaction is preceded by a step of adding a first curing agent to the reaction product of the first carbon source and the modified additive; (6) Before the first curing reaction, the step of adding a first curing agent to the reaction product of the first carbon source and the modified additive is further included, wherein the mass ratio of the first carbon source to the first curing agent is (60:40) to (95:5). (7) Before the first curing reaction, the step of adding a first curing agent to the reaction product of the first carbon source and the modified additive is further included. The first curing agent includes at least one of ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium sulfate. (8) The temperature of the first curing reaction is 80℃~300℃; (9) The time for the first curing reaction is 0.5 h ~ 24 h; (10) Before the first carbon source is mixed with the modified additive, the first carbon source and the modified additive are further subjected to a first crushing and a first sieving step.

7. The preparation method according to claim 4, characterized in that, The carbon source includes a second carbon source, and the first heat treatment of the mixture containing the second carbon source and the modifying additive to obtain the first precursor includes: mixing the second carbon source, the modifying additive and the second curing agent and simultaneously carrying out a second addition reaction and a second curing reaction to obtain the first precursor, and the method includes at least one of the following features (1) to (7): (1) The second carbon source includes at least one of starch, thermosetting phenolic resin, epoxy resin, melamine resin, furfural resin, urea-formaldehyde resin, oxidized asphalt, lignin, cellulose, coconut shell, almond shell, walnut shell, peach kernel shell, peanut shell, pistachio shell, hazelnut shell, sawdust and straw. (2) The mass ratio of the second carbon source to the modified additive is (40:60) to (99:1); (3) The temperature at which the second addition reaction and the second curing reaction are carried out simultaneously is 80℃~300℃; (4) The time for the simultaneous second addition reaction and second curing reaction is 0.5 h to 24 h; (5) The mass ratio of the second carbon source to the second curing agent is (60:40) to (100:0) (inclusive of 0); (6) The second curing agent includes at least one of ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium sulfide, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium oxalate, ammonium acetate, melamine, hexamethylenetetramine, formaldehyde, p-benzaldehyde, ammonium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium sulfate; (7) Before mixing the second carbon source, the modified additive and the second curing agent, the process further includes a second crushing and a second sieving step of the second carbon source, the modified additive and the second curing agent.

8. The preparation method according to claim 4, characterized in that, The method includes at least one of the following features (1) to (7): (1) The pre-carbonization treatment is carried out in a first protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon and krypton; (2) The pre-carbonization time is 0.5 h ~ 24 h; (3) The pre-carbonization equipment includes at least one of tube furnace, box furnace, pusher kiln and roasting kiln; (4) After obtaining the second precursor through pre-carbonization, the process further includes a third crushing and a third sieving step on the second precursor; (5) The acid solution used for pickling includes at least one of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, acetic acid, oxalic acid, benzoic acid, hydrosulfuric acid, hydrobromic acid and hydroiodic acid. (6) The mass ratio of the second precursor to the pickling acid is 1:(3~15); (7) The mass concentration of the acid solution used for pickling is 10%~50%.

9. The preparation method according to claim 4, characterized in that, The method includes at least one of the following features (1) to (3): (1) The second heat treatment time is 1h~24h; (2) The second heat treatment is carried out in a second protective atmosphere, which includes at least one of nitrogen, argon, neon, helium, xenon and krypton; (3) The second heat treatment also includes a fourth screening step of the obtained material, wherein the screen size of the fourth screening is 200 mesh to 325 mesh.

10. A sodium-ion battery, characterized in that, The sodium-ion battery includes the negative electrode material according to any one of claims 1 to 3 or the negative electrode material prepared by the preparation method of the negative electrode material according to any one of claims 4 to 9.

Citation Information

Patent Citations

  • A carbon-based negative electrode material with high ramp capacity and a preparation method and use thereof

    CN109148884A