A high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder and its preparation method
By preparing Y-BaCeO3@Y-CeO2 core-shell structured nanoparticles, the problem of low grain boundary conductivity in CeO2-based electrolytes was solved, enabling the application of CeO2-based electrolyte materials with high conductivity.
Patent Information
- Application Number
- CN202311271145.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-28
AI Technical Summary
The low grain boundary conductivity of CeO2-doped electrolytes limits their ability to improve conductivity and their widespread application. Existing technologies struggle to effectively improve grain boundary conductivity.
Y-BaCeO3@Y-CeO2 core-shell structured nanopowder is used. By wrapping the CeO2 core with a BaCeO3 shell, a high-conductivity core-shell structure is formed. The high-conductivity interface between the CeO2/BaCeO3 phases is utilized to improve the conductivity of the multiphase ceramic.
The prepared core-shell structured nanopowder has small grain size and large grain boundary area, which significantly improves the grain boundary conductivity of the CeO2-based electrolyte and realizes a CeO2-based electrolyte material with high conductivity.
Smart Images

Figure HDA0004475589020000011 
Figure HDA0004475589020000012 
Figure HDA0004475589020000021
Abstract
Description
Technical Field
[0001] This invention discloses a high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder and its preparation method, belonging to the field of solid electrolyte technology. Background Technology
[0002] Solid-state ionic conductors are solid materials that use ions as charge carriers and exhibit high conductivity over a wide operating temperature range. They are widely used in fuel cells, electrochromic devices, gas separation devices, sensors, oxygen pumps, and other fields. Doped CeO2 is an important oxygen ion conductor solid electrolyte with even higher ionic conductivity, allowing it to operate at lower temperatures and making it a promising electrolyte material for solid oxide fuel cells. However, the main factor limiting the improvement of the conductivity of CeO2-based solid electrolytes is not from the grain interior, but from the grain boundaries. Numerous experiments have shown that the grain boundary conductivity of doped CeO2-based electrolytes is 2 to 3 orders of magnitude lower than that of the grain interior, becoming the biggest obstacle to improving its conductivity and its widespread application.
[0003] Previous studies have shown that introducing another suitable conductive phase into the CeO2 matrix can form a two-phase interface with high ionic conductivity, thereby greatly improving the grain boundary conductivity of the doped CeO2-based electrolyte. Proton conductors have the advantages of small transport ion radius and relatively high conductivity; while doped BaCeO3 is a typical proton conductor with high conductivity, high melting point, and stable structure. Introducing doped BaCeO3 as a second phase into the CeO2 matrix to form a core-shell structure can greatly increase the two-phase interface area, thereby improving the conductivity of the CeO2-based electrolyte. Summary of the Invention
[0004] The purpose of this invention is to provide a core-shell structure with the chemical formula Y-BaCeO3@Y-CeO2, wherein yttrium-doped cerium dioxide (Y-CeO2) is used as the core and yttrium-doped barium cerate (Y-BaCeO3) is used as the shell; the average grain size of the core-shell nanoparticles is 61.8 nm to 70.5 nm.
[0005] Another object of the present invention is to provide a method for preparing the high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder, specifically including the following steps:
[0006] (1) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in water to prepare solution A. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) is 1:(0.1~0.5):(0.5~1).
[0007] (2) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in water to prepare solution B. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) is 1:1:0.1~0.5:0.5~1mol / L.
[0008] (3) Dissolve the surfactant in water and stir at 60-65℃ for 15-20 min to obtain solution C, wherein the concentration of the surfactant solution is 0.1-0.5 mol / L.
[0009] (4) Ammonia water is slowly added to solution A to adjust the pH value to 8-10 and a co-precipitation reaction is carried out. Then, Y-CeO2 powder is obtained by filtration, repeated washing with ethanol, drying, calcination and grinding.
[0010] (5) Take a certain amount of Y-CeO2 powder obtained in step (4) and add it to water for ultrasonic dispersion to prepare Y-CeO2 core suspension. The concentration of Y-CeO2 powder in the suspension is 0.2-0.5 mol / L. Add the C solution obtained in step (3) to the core suspension (the volume ratio of C solution to suspension does not exceed 1:1) and adjust the pH value to 8-10 with ammonia.
[0011] (6) The core suspension with pH adjusted in step (5) is dropped into solution B obtained in step (2). The molar ratio of cerium ions in the suspension to barium ions in solution B does not exceed 1:1. Ammonia water is added from time to time to keep the pH of solution B stable at 8-10. Co-precipitation reaction is carried out. Then, Y-BaCeO3@Y-CeO2 core-shell nanoparticles are obtained by filtration, repeated washing with ethanol, drying, calcination and grinding.
[0012] Preferably, the concentration of each raw material powder in the aqueous solution in step (1) of the present invention is 0.1 to 1.5 mol / L.
[0013] Preferably, the concentration of each raw material powder in the aqueous solution in step (2) of the present invention is 0.03 to 0.3 mol / L.
[0014] Preferably, the surfactant in step (3) of the present invention is sodium dodecylbenzenesulfonate.
[0015] Preferably, in steps (4), (5) and (6) of the present invention, the pH is 8-10, the co-precipitation reaction is 2-6 hours, the washing is 2-6 times, the drying temperature is 100-200℃, the drying time is 12-48 hours, the calcination is 800-1100℃ for 5-8 hours, and the ultrasonication is 15-30 minutes.
[0016] Preferably, the concentration of Y-CeO2 powder in the aqueous solution in step (5) is 0.2 to 0.5 mol / L.
[0017] In this invention, yttrium-doped barium cerate (Y-BaCeO3) is selected as the second phase. BaCeO3 is a good proton conductor in hydrogen or humid air. Due to its small H+ radius and low migration activation energy, it is expected to enable CeO2-based electrolytes to achieve high conductivity.
[0018] The core-shell structured nanopowder prepared in this invention can prevent the isolated existence of the second-phase grains. If the second-phase grains are isolated, the two-phase interfaces cannot connect to form a network. Although the introduced two-phase interface has high conductivity, it is still blocked by the low-conductivity CeO2 grains, and the overall conductivity of the multiphase ceramic cannot be significantly improved. Furthermore, microscopic agglomeration of the second phase or uneven dispersion in different regions macroscopically exacerbates the blockage of transport pathways, thus greatly limiting the improvement of the conductivity of the CeO2-based multiphase electrolyte. Therefore, by preparing a core-shell structured second-phase@CeO2 nanopowder with CeO2 as the core and a second phase (doped BaCeO3 proton conductor phase) as the nano-thick outer shell, the problem of interface separation, isolation, and discontinuity after introducing the BaCeO3 second phase is solved. Simultaneously, the high conductivity interface between the CeO2 / BaCeO3 phases can be used to improve the conductivity of the multiphase ceramic.
[0019] Beneficial effects of the present invention
[0020] (1) The core-shell structured nanopowder prepared by this invention has simple production equipment and process methods and low economic cost.
[0021] (2) The average grain size of the core-shell structured nanopowder prepared by the present invention is between 61.8 and 70.5 nm. The grain size is relatively small and the grain boundary area is relatively large, which is more conducive to improving the grain boundary conductivity of the CeO2-based electrolyte. Attached Figure Description
[0022] Figure 1 The image shows the XRD pattern of the core-shell structure Y-BaCeO3@Y-CeO2 nanopowder from Example 1 after calcination.
[0023] Figure 2 The image shows the SEM image of the core-shell structure Y-BaCeO3@Y-CeO2 nanopowder of Example 1 after calcination.
[0024] Figure 3 The image shows a statistical diagram of the grain size of the core-shell structure Y-BaCeO3@Y-CeO2 nanopowder after calcination, as described in Example 1.
[0025] Figure 4 The image shows the TEM image of the core-shell structure Y-BaCeO3@Y-CeO2 nanopowder of Example 1 after calcination. Detailed Implementation
[0026] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited to the content described.
[0027] Example 1
[0028] A method for preparing Y-BaCeO3@Y-CeO2 core-shell structured nanopowder, the specific steps of which are as follows:
[0029] (1) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 30 ml of water to prepare solution A. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) is 1:0.2:0.5.
[0030] (2) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 100 ml of water to prepare solution B. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) is 1:1:0.2:0.5.
[0031] (3) Dissolve 2.09g of surfactant sodium dodecylbenzenesulfonate in 20ml of water and stir at 60℃ for 20min to obtain solution C, wherein the concentration of surfactant solution is 0.3mol / L.
[0032] (4) Ammonia water was slowly added to solution A to adjust its pH to 9.2. Co-precipitation reaction was carried out for 3 hours. Then, the solution was filtered, washed twice with ethanol, dried in an oven at 110°C for 24 hours, calcined at 900°C for 6 hours, and ground to obtain Y-CeO2 powder.
[0033] (5) Take 1.03g of Y-CeO2 powder obtained in step (4) and add it to 20ml of water and sonicate for 20min to disperse it, so as to obtain a 0.3mol / L Y-CeO2 core suspension. Add the C solution obtained in step (3) to the core suspension and adjust the pH to 9.2 with ammonia.
[0034] (6) The core suspension with pH adjusted in step (5) was added dropwise to the B solution obtained in step (2), and ammonia was added from time to time to keep the pH of the B solution at 9.2. The co-precipitation reaction was carried out for 5 hours, and then the Y-BaCeO3@Y-CeO2 core-shell nanopowder was obtained by filtration, repeated washing with ethanol 3 times, drying in an oven at 110℃ for 48 hours, calcining at 1000℃ for 8 hours and grinding.
[0035] Figure 1 The XRD pattern of the core-shell structured nanopowder prepared in Example 1 shows that no other impurity phases appeared in the synthesized core-shell structured powder, indicating that Y-BaCeO3@Y-CeO2 nanopowder was initially synthesized.
[0036] Figure 2 , Figure 3 The image shows the SEM image and corresponding grain size statistics of the core-shell structured nanopowder prepared in Example 1. As can be seen from the image, the synthesized powder is at the nanoscale, and the powder has good dispersibility, uniform particle size, and an average grain size between 61.8 and 70.5 nm.
[0037] Figure 4 The image shows the TEM spectrum of the core-shell structured nanopowder prepared in Example 1. The core-shell structure can be clearly seen from the image. Combined with the EDS spectrum, it can better prove that the prepared powder is Y-BaCeO3@Y-CeO2 nanopowder.
[0038] Example 2
[0039] A method for preparing Y-BaCeO3@Y-CeO2 core-shell structured nanopowder, the specific steps of which are as follows:
[0040] (1) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 30 ml of water to prepare solution A. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) is 1:0.5:1.
[0041] (2) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 100 ml of water to prepare solution B. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) is 1:1:0.5:1.
[0042] (3) Dissolve 3.48g of surfactant sodium dodecylbenzenesulfonate in 20ml of water and stir at 62℃ for 18min to obtain solution C, wherein the concentration of surfactant solution is 0.5mol / L.
[0043] (4) Ammonia water was slowly added to solution A to adjust its pH to 10 and co-precipitation reaction was carried out for 6 hours. Then, it was filtered, washed repeatedly with ethanol 6 times, dried in an oven at 200℃ for 48 hours, calcined at 1100℃ for 8 hours and ground to obtain Y-CeO2 powder.
[0044] (5) Take 1.72g of Y-CeO2 powder obtained in step (4) and add it to 20ml of water and sonicate for 30min to disperse it, so as to prepare a 0.5mol / L Y-CeO2 core suspension. Add the C solution obtained in step (3) to the core suspension and adjust the pH to 10 with ammonia.
[0045] (6) The core suspension with pH adjusted in step (5) was added dropwise to the B solution obtained in step (2), and ammonia was added from time to time to keep the pH of the B solution at 10. The co-precipitation reaction was carried out for 6 hours. Then, the solution was filtered, washed repeatedly with ethanol 6 times, dried in an oven at 200℃ for 48 hours, calcined at 1100℃ for 6 hours, and ground to obtain Y-BaCeO3@Y-CeO2 core-shell nanopowder.
[0046] The Y-BaCeO3@Y-CeO2 core-shell nanopowder prepared in this embodiment has a similar structure and properties to those in Example 1.
[0047] Example 3
[0048] A method for preparing Y-BaCeO3@Y-CeO2 core-shell structured nanopowder, the specific steps of which are as follows:
[0049] (1) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 30 ml of water to prepare solution A, wherein the molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3) and dispersant (citric acid C6H8O7) is 1:0.1:0.8.
[0050] (2) Weigh cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) according to the stoichiometric ratio and dissolve them in 100 ml of water to prepare solution B. The molar ratio of cerium nitrate (Ce(NO3)3), yttrium nitrate (Y(NO3)3), barium nitrate (Ba(NO3)2) and dispersant (citric acid C6H8O7) is 1:1:0.1:0.9.
[0051] (3) Dissolve 0.34g of surfactant sodium dodecylbenzenesulfonate in 20ml of water and stir at 65℃ for 15min to obtain solution C, wherein the concentration of surfactant solution is 0.1mol / L.
[0052] (4) Ammonia water was slowly added to solution A to adjust its pH to 8 and co-precipitation reaction was carried out for 2 hours. Then, the solution was filtered, washed repeatedly with ethanol 4 times, dried in an oven at 100℃ for 12 hours, calcined at 800℃ for 5 hours, and ground to obtain Y-CeO2 powder.
[0053] (5) Take 0.69g of Y-CeO2 powder obtained in step (4) and add it to 20ml of water and sonicate for 15min to disperse it, so as to prepare a 0.2mol / L Y-CeO2 core suspension. Add the C solution obtained in step (3) to the core suspension and adjust the pH to 8 with ammonia.
[0054] (6) The core suspension with pH adjusted in step (5) was added dropwise to the B solution obtained in step (2), and ammonia was added from time to time to keep the pH of the B solution at 8. The co-precipitation reaction was carried out for 2 hours. Then, the solution was filtered, washed twice with ethanol, dried in an oven at 100°C for 12 hours, calcined at 800°C for 5 hours, and ground to obtain Y-BaCeO3@Y-CeO2 core-shell nanopowder.
[0055] The Y-BaCeO3@Y-CeO2 core-shell nanopowder prepared in this embodiment has a similar structure and properties to those in Example 1.
Claims
1. A high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder, characterized in that: The core-shell structured nanopowder has a yttrium-doped cerium dioxide (Y-CeO2) core and a yttrium-doped barium cerate (Y-BaCeO3) shell, and the average grain size of the core-shell structured nanopowder is 61.8 nm to 70.5 nm. The preparation method of the high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder specifically includes the following steps: (1) Weigh cerium nitrate, yttrium nitrate and dispersant citric acid according to the stoichiometric ratio and dissolve them in water to prepare solution A, wherein the molar ratio of cerium nitrate, yttrium nitrate and citric acid is 1:(0.1~0.5):(0.5~1); (2) Weigh cerium nitrate, yttrium nitrate, barium nitrate and dispersant citric acid according to the stoichiometric ratio and dissolve them in water to prepare solution B; (3) Dissolve the surfactant in water and stir at 60~65℃ for 15~20min to obtain solution C, wherein the concentration of the surfactant solution is 0.1~0.5mol / L; (4) Ammonia water is slowly added to solution A to adjust the pH value to 8~10, and a co-precipitation reaction is carried out. Then, Y-CeO2 powder is obtained by filtration, repeated washing with ethanol, drying, calcination and grinding. (5) Take a certain amount of Y-CeO2 powder obtained in step (4) and add it to water for ultrasonic dispersion to prepare Y-CeO2 core suspension. The concentration of Y-CeO2 powder in the suspension is 0.2~0.5mol / L. Add the C solution obtained in step (3) to the core suspension and adjust the pH value to 8~10 with ammonia. (6) The core suspension with pH adjusted in step (5) is dropped into solution B obtained in step (2). The molar ratio of cerium ions in the suspension to barium ions in solution B does not exceed 1:
1. Ammonia water is added from time to time to keep the pH of solution B stable at 8~10. Co-precipitation reaction is carried out. Then, Y-BaCeO3@Y-CeO2 core-shell nanopowder is obtained by filtration, repeated washing with ethanol, drying, calcination and grinding.
2. The method for preparing the high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 1, characterized in that, Specifically, the following steps are included: (1) Weigh cerium nitrate, yttrium nitrate and dispersant citric acid according to the stoichiometric ratio and dissolve them in water to prepare solution A, wherein the molar ratio of cerium nitrate, yttrium nitrate and citric acid is 1:(0.1~0.5):(0.5~1); (2) Weigh cerium nitrate, yttrium nitrate, barium nitrate and dispersant citric acid according to the stoichiometric ratio and dissolve them in water to prepare solution B; (3) Dissolve the surfactant in water and stir at 60~65℃ for 15~20min to obtain solution C, wherein the concentration of the surfactant solution is 0.1~0.5mol / L; (4) Ammonia water is slowly added to solution A to adjust the pH value to 8~10, and a co-precipitation reaction is carried out. Then, Y-CeO2 powder is obtained by filtration, repeated washing with ethanol, drying, calcination and grinding. (5) Take a certain amount of Y-CeO2 powder obtained in step (4) and add it to water for ultrasonic dispersion to prepare Y-CeO2 core suspension. The concentration of Y-CeO2 powder in the core suspension is 0.2~0.5mol / L. Add the C solution obtained in step (3) to the core suspension and adjust the pH value to 8~10 with ammonia. (6) The core suspension with pH adjusted in step (5) is dropped into solution B obtained in step (2). The molar ratio of cerium ions in the suspension to barium ions in solution B does not exceed 1:
1. Ammonia water is added from time to time to keep the pH of solution B stable at 8~10. Co-precipitation reaction is carried out. Then, Y-BaCeO3@Y-CeO2 core-shell nanopowder is obtained by filtration, repeated washing with ethanol, drying, calcination and grinding.
3. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: In step (1), the concentration of each raw material powder in the aqueous solution is 0.1~1.5 mol / L.
4. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: In step (2), the concentration of each raw material powder in the aqueous solution is 0.03~0.3 mol / L.
5. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: The surfactant in step (3) is sodium dodecylbenzenesulfonate.
6. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: Step (6) Co-precipitation reaction for 2-6 hours, followed by washing 2-6 times.
7. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: In step (6), the drying temperature is 100~200℃ and the drying time is 12~48h.
8. The method for preparing high-conductivity Y-BaCeO3@Y-CeO2 core-shell structured nanopowder according to claim 2, characterized in that: In step (6), calcination is carried out at 800~1100℃ for 5~8 hours.
Citation Information
Patent Citations
Method for preparing cerium oxide nano powder
CN101070180A
Lithium ion solid electrolyte material with composite core-shell structure and preparation method thereof