Optical products that improve visual comfort
By designing an interference multilayer coating with alternating layers of high and low refractive index materials on optical products, the problem of mirror coatings reflecting light into the eye at high incident angles has been solved. This achieves a balance between low reflection at high incident angles and high reflection at low incident angles, thus improving the wearer's visual comfort.
Patent Information
- Application Number
- CN202280036740.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-04-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-04-12
AI Technical Summary
Existing mirror coatings reflect light into the wearer's eyes at high incident angles, causing visual discomfort, while at low incident angles, they reflect insufficient light, affecting the wearer's visual comfort.
Design an optical article having an interference multilayer coating on the front or back, comprising alternating layers of high and low refractive index materials, to ensure a reflectance coefficient of less than 2.5% at high incident angles and a reflectance coefficient of more than 2.5% at low incident angles, in order to reduce back reflection and maintain high forward reflection.
It improves the wearer's visual comfort while maintaining the stylish effect of the mirror coating, and ensures high reflectivity at low incident angles by reducing back reflection at high incident angles.
Smart Images

Figure CN117377891B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to an optical product that provides improved visual comfort.
[0002] More specifically, this disclosure relates to an optical article having an interference “mirror” coating that provides improved visual comfort in terms of visible light reflection while maintaining the stylish aspect of a “mirror” coating. In this disclosure, a coating is referred to as a “mirror” coating if its average visible light reflectance Rv is greater than 2.5%, wherein the average visible light reflectance Rv is defined as follows:
[0003]
[0004] Where R(λ) is the reflectance at wavelength λ, V(λ) is the eye sensitivity function in the color space defined by the CIE (Commission on Illumination, French "Commission Internationale de l'Eclairage") in 1931, and D 65 (λ) is the daylight source defined in the CIE S005 / E-1998 standard.
[0005] As a non-limiting example, this disclosure can be applied to the field of sunglasses. Background Technology
[0006] Stylish mirror coatings are widely used on sunglasses. For mirror coatings, high forward reflection of visible light (i.e., visible light reflected from the wearer's eyes onto the surface of the sunglasses lens located on the side of the scene seen by the wearer) is desirable.
[0007] However, conventional mirror coatings also typically exhibit high retroreflectivity of visible light, meaning that visible light from the wearer's side is reflected through the substrate and then through the mirror coating on the front surface toward the wearer's eyes. Therefore, retroreflectivity of visible light is undesirable for the wearer, especially when using mirrors with high to very high reflectivity.
[0008] High back reflection of visible light at low incident angles (i.e., low angles relative to the perpendicular of the lens's surface of consideration) is not a major problem for the wearer, as light from the rear will be blocked by the wearer's head.
[0009] It is also expected that the specular coating will maintain high forward reflectivity of visible light at low incident angles.
[0010] On the other hand, at high incident angles (e.g., 35°–55°), light from the rear may be reflected into the wearer's eyes, which is a problem.
[0011] EP 3 118 658 discloses an optical article comprising a substrate defining a front main surface and a rear main surface, wherein at least one main surface is coated with an interference multilayer coating that defines high reflectivity when the article is viewed from the front and antireflectivity when the article is viewed from the rear.
[0012] To this end, this document teaches the provision of an absorptive asymmetric specular coating on the front of an optical article, the coating consisting of one or two absorptive metal layers (Cr, Ta, Nb, Ti, or Zr) added to an interference stack, and a conventional antireflective coating that transmits visible light behind it.
[0013] Compared to high forward reflection, the metal-containing absorptive asymmetric specular coating can have much lower backward reflection, which can effectively reduce light from the back of the optical article that passes through the substrate and is then reflected from the specular coating on the front surface toward the wearer's eyes.
[0014] However, due to the extremely strong light absorption properties of the metallic materials used, only a very thin metal layer of a few nanometers thickness is used in this type of optical product to ensure minimal light transmission into the wearer's eyes. However, such a low metal layer thickness is difficult or even impossible to achieve, or requires specific methods and / or is not easily controlled.
[0015] Therefore, the unmet need is to provide an optical article that improves the wearer's visual comfort by having reduced back reflection of visible light at high incident angles and high forward reflection of visible light at low incident angles, which involves conventional manufacturing methods. Summary of the Invention
[0016] The purpose of this disclosure is to overcome at least some of the limitations of the prior art described above.
[0017] To this end, this disclosure provides an optical article having a back side on the wearer's eye side and a front side opposite to the back side, wherein the optical article has an interference multilayer coating on at least one of the front and back sides, the interference multilayer coating comprising at least one layer of a high refractive index material with a refractive index greater than 1.55 and at least one layer of a low refractive index material with a refractive index of 1.55 or lower, the refractive index being expressed for a wavelength of 550 nm, the optical article being designed such that it has high reflectivity at low incident angles when viewed from its front or back side, and antireflectivity at high incident angles when viewed from its front or back side.
[0018] When the angle of incidence relative to the perpendicular line from the front or back is greater than or equal to 35° and less than or equal to 55°, the coating has an average visible light reflectance Rv of less than or equal to 2.5% for visible light incident on the front or back; and
[0019] With an incident angle greater than or equal to 0° and less than or equal to 15° relative to the perpendicular line from the front or back, the coating has an average visible light reflectance Rv greater than or equal to 2.5% for visible light irradiated to the front or back.
[0020] Therefore, this optics provides low back reflection of visible light that may reach the wearer's eyes at high incident angles. This improves the wearer's visual comfort while maintaining the stylish aspect of the mirror coating.
[0021] In a specific embodiment, when the incident angle is greater than or equal to 35° and less than or equal to 50°, the average visible light reflectance coefficient Rv is less than or equal to 2%, more preferably less than or equal to 1.5%.
[0022] In a specific embodiment, when the incident angle is greater than or equal to 0° and less than or equal to 10°, the average visible light reflectance coefficient Rv is greater than or equal to 3.5%.
[0023] In a specific embodiment, the ratio between the Rv value Rv(0°) at the incident angle perpendicular to the front or back surface and the minimum Rv value Rvmin(35°-50°) at the incident angle with a perpendicular line to the front or back surface greater than or equal to 35° and less than or equal to 50° is greater than 3, preferably greater than 4, and more preferably greater than 5.
[0024] In a specific embodiment, the ratio between the Rv value Rv(10°) at an angle of incidence equal to 10° relative to the front or back surface and the minimum Rv value Rvmin(35°-50°) at an angle of incidence greater than or equal to 35° and less than or equal to 50° relative to the front or back surface is greater than 3, preferably greater than 4, and more preferably greater than 5.
[0025] In a specific embodiment, the coating comprises alternating layers of high-refractive-index materials and low-refractive-index materials.
[0026] In this disclosure, a “high refractive index” or “HI” material or layer is typically a material or layer having a refractive index greater than or equal to 1.5, and a “low refractive index” or “LI” material or layer is typically a material having a refractive index less than 1.5.
[0027] In a specific embodiment, the alternating layers from the innermost layer to the outermost layer include:
[0028] A first high-refractive-index material layer H1 has a physical thickness ranging from 15 to 50 nm and a relative optical thickness ranging from 0.05 to 0.20, wherein the relative optical thickness is defined as ROT = PT × n 550 / 550, where PT is the physical thickness, and n 550 It is the refractive index at 550 nm;
[0029] A first low-refractive-index material layer L1 has a physical thickness ranging from 0 to 80 nm and a relative optical thickness ranging from 0.04 to 0.20.
[0030] The second high-refractive-index material layer H2 has a physical thickness ranging from 40 nm to 100 nm and a relative optical thickness ranging from 0.10 to 0.50.
[0031] The second low-refractive-index material layer L2 has a physical thickness ranging from 180 nm to 300 nm and a relative optical thickness ranging from 0.40 to 0.90.
[0032] The third high-refractive-index material layer H3 has a physical thickness ranging from 50 nm to 120 nm and a relative optical thickness ranging from 0.15 to 0.50.
[0033] The third low-refractive-index material layer L3 has a physical thickness ranging from 80 nm to 150 nm and a relative optical thickness ranging from 0.20 to 0.40.
[0034] In a specific embodiment:
[0035] The physical thickness ratio between the third low-refractive-index material layer L3 and the second low-refractive-index material layer L2 is less than 0.5, and the relative optical thickness ratio between the third low-refractive-index material layer L3 and the second low-refractive-index material layer L2 is less than 0.5.
[0036] The physical thickness ratio between the third low-refractive-index material layer L3 and the first high-refractive-index material layer H1 is greater than 3, and the relative optical thickness ratio between the third low-refractive-index material layer L3 and the first high-refractive-index material layer H1 is greater than 2.2.
[0037] The product of the physical thicknesses of the third low-refractive-index material layer L3 and the first high-refractive-index material layer H1 is less than 5000, and the product of the relative optical thicknesses of the third low-refractive-index material layer L3 and the first high-refractive-index material layer H1 is less than 0.05.
[0038] In specific embodiments, the aforementioned high refractive index materials are SiN, TiO2, PrTiO3, LaTiO3, ZrO2, Ta2O5, Y2O3, Ce2O3, La2O3, Dy2O5, Nb2O5, HfO2, Sc2O3, Pr2O3, Al2O3, or Si3N4, and the aforementioned low refractive index materials are SiO2, MgF2, ZrF4, Al2O3, AlF3, and Na3[Al3F] cryolite. 14 The material contains cryolite Na3[AlF6], or any mixture thereof, preferably SiO2 or SiO2 doped with Al2O3, wherein the Al2O3 doped SiO2 contains 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer).
[0039] In such specific embodiments, the high refractive index material may be ZrO2, Ta2O5, Nb2O5, SiN or TiO2, and the low refractive index material may be SiO2 or Al2O3-doped SiO2 having 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer).
[0040] In such specific embodiments, the coating may comprise alternating layers of high-refractive-index and low-refractive-index materials, the alternating layers comprising, from the innermost to the outermost layer:
[0041] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 20-40 nm;
[0042] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer having a thickness of 10-80 nm).
[0043] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 46-95 nm;
[0044] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer having a thickness of 180-300 nm).
[0045] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, wherein the layer has a thickness of 50-120 nm;
[0046] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer having a thickness of 80-150 nm).
[0047] In specific embodiments, the optical article may be an ophthalmic lens, a device having a safety wall intended to face the wearer's eye, a filter, or an optical film or patch intended to be fixed to a substrate.
[0048] This disclosure also provides sunglasses, wherein these sunglasses include at least one optical element as briefly described above.
[0049] Since the sunglasses disclosed herein have the same specific features and advantages as optical products, they will not be repeated here. Attached Figure Description
[0050] To gain a more complete understanding of the descriptions and advantages provided herein, please refer now to the following brief description in conjunction with the accompanying drawings and detailed description, wherein the same reference numerals denote the same parts.
[0051] Figure 1 This is a schematic diagram showing the layer structure of a first comparative example of a mirror coating in an optical article according to the prior art and a first non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0052] Figure 2 It is a graph showing the variation of the average visible light reflectance Rv as a function of the incident angle in a first comparative example according to the prior art and a first non-limiting example according to this disclosure.
[0053] Figure 3 This is a schematic diagram showing the layer structure of a second comparative example of a mirror coating in an optical article according to the prior art and a second non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0054] Figure 4 It is a graph showing the average visible light reflectance Rv as a function of the incident angle in a second comparative example according to the prior art and a second non-limiting example according to this disclosure.
[0055] Figure 5 This is a schematic diagram showing the layer structure of a third comparative example of a mirror coating in an optical article according to the prior art and a third non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0056] Figure 6 It is a graph showing the variation of the average visible light reflectance Rv as a function of the incident angle in the third comparative example according to the prior art and the third non-limiting example according to this disclosure.
[0057] Figure 7 This is a schematic diagram showing the layer structure of a fourth comparative example of a mirror coating in an optical article according to the prior art and a fourth non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0058] Figure 8 It is a graph showing the variation of the average visible light reflectance Rv as a function of the incident angle in the fourth comparative example according to the prior art and the fourth non-limiting example according to this disclosure.
[0059] Figure 9 This is a schematic diagram illustrating the layer structure of a fifth non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0060] Figure 10 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the fifth non-limiting example of this disclosure.
[0061] Figure 11 This is a schematic diagram illustrating the layer structure of a sixth non-limiting example of a mirror coating in an optical article according to this disclosure.
[0062] Figure 12 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the sixth non-limiting example of this disclosure.
[0063] Figure 13 This is a schematic diagram illustrating the layer structure of a seventh non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0064] Figure 14 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the seventh non-limiting example of this disclosure.
[0065] Figure 15 This is a schematic diagram illustrating the layer structure of an eighth non-limiting example of a mirror coating in an optical article according to this disclosure.
[0066] Figure 16 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the eighth non-limiting example of this disclosure.
[0067] Figure 17 This is a schematic diagram illustrating the layer structure of a ninth non-limiting example of a mirror coating in an optical article according to the present disclosure.
[0068] Figure 18 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the ninth non-limiting example of this disclosure.
[0069] Figure 19 This is a schematic diagram illustrating the layer structure of a tenth non-limiting example of a mirror coating in an optical article according to this disclosure.
[0070] Figure 20 This is a graph showing how the average visible light reflectance Rv varies as a function of the incident angle according to the tenth non-limiting example of this disclosure.
[0071] Figure 21 It is a chart that collects the range of values for the relative optical thickness and physical thickness of the layers for all non-restricted instances, as well as some layer ratios and products.
[0072] Figure 22 It is a chart that collects the range of values for the relative optical thickness and physical thickness of the layers for all comparative examples, as well as some layer ratios and products. Detailed Implementation
[0073] In the following description, the accompanying drawings are not necessarily drawn to scale, and some features may be shown in a generalized or schematic form for clarity and brevity or for informational purposes. Furthermore, although various embodiments of manufacture and use are discussed in detail below, it should be understood that many inventive concepts, as described herein, can be embodied in a variety of contexts. The embodiments discussed herein are merely representative and do not limit the scope of this disclosure. It will also be apparent to those skilled in the art that all technical features defined in relation to the process can be transposed individually or in combination to the device, and conversely, all technical features associated with the device can be transposed individually or in combination to the process, and that technical features of different embodiments can be exchanged or combined with features of other embodiments.
[0074] The terms “comprise” (and any of its grammatical variations, such as “comprises” and “comprising”), “have” (and any of its grammatical variations, such as “has” and “having”), “contain” (and any of its grammatical variations, such as “contains” and “containing”), and “include” (and any of its grammatical variations, such as “includes” and “including”) are open-ended connecting verbs. They are used to indicate the presence of a feature, whole, step, or component or group thereof, but do not exclude the presence or inclusion of one or more other features, wholes, steps, or components or groups thereof. Therefore, a method or a step in a method that “comprises,” “has,” “contains,” or “includes” one or more steps or elements possesses, but is not limited to, possessing only those steps or elements.
[0075] Unless otherwise specified, all figures or expressions relating to quantities of ingredients, ranges, reaction conditions, etc., used herein should be understood to be modified by the term “about” in all cases.
[0076] Furthermore, unless otherwise specified, the indication of a value range “from X to Y” or “between X and Y” in this disclosure means to include the values of X and Y.
[0077] In this disclosure, when an optical article includes one or more coatings on its surface, the expression “depositing a layer or coating onto the article” is intended to mean depositing a layer or coating onto the outer (exposed) surface of the outer coating of the article (i.e., the coating furthest from the substrate).
[0078] A coating that is claimed to be “on” or deposited on a substrate is defined as a coating that (i) is positioned above the substrate, (ii) is not necessarily in contact with the substrate, i.e., one or more intermediate coatings may be arranged between the substrate and the coating in question, and (iii) does not necessarily completely cover the substrate.
[0079] In a specific embodiment, the coating on or deposited onto the substrate is in direct contact with the substrate.
[0080] As used herein, the “back” or “rear” or “inner” side of an optical article is intended to refer to the side closest to the wearer’s eyes when the optical article is in use. Such a back or rear or inner side is typically concave. Conversely, the front of the substrate is the side furthest from the wearer’s eyes when the optical article is in use. It is typically convex.
[0081] Furthermore, the "angle of incidence (symbol θ)" is the angle formed by the light ray incident on the surface of the ophthalmic lens and the normal to the surface at the point of incidence. The light ray is, for example, a light source that emits light, such as the standard illuminator D65 as defined in the CIE L*a*b* international colorimetric standard. Generally, the angle of incidence varies from 0° (normal incidence) to 90° (grazing incidence). The general range of the angle of incidence is from 0° to 75°.
[0082] The colorimetric coefficients of the optical articles disclosed herein, in the international colorimetric system CIE L*a*b*, are calculated between 380 nm and 780 nm (considering a standard light source D65 and an observer (at an angle of 10°)). The observer is as shown in the international colorimetric system CIE L*a*b*. * a * b * The "standard observer" as defined in [the text].
[0083] The expression "natural light" or "visible light" includes any type of natural light, especially sunlight or direct sunlight. Sunlight has bright emission across the entire visible spectrum, particularly in the wavelength range of 550 nm to 620 nm. In some embodiments, the expression "natural light" or "visible light" also includes artificial light with a broad spectrum, such as light emitted by some LED devices that mimic the sun.
[0084] In this invention, the term "absorbing / absorption" of a device within a certain wavelength range refers to the situation where the average emission value of the device within that wavelength range is less than 50% of the average emission value of the device in each adjacent 40 nm wavelength range.
[0085] Generally, the interference coating (which, depending on the described configuration, will be referred to as a "reflective (or specular) coating") of the optical articles according to this disclosure can be deposited on any substrate, and is preferably deposited on an organic lens substrate, such as a thermoplastic or thermosetting plastic material. Thermoplastic plastics can be selected from, for example: polyamides; polyimides; polysulfones; polycarbonates and copolymers thereof; poly(ethylene terephthalate) and polymethyl methacrylate (PMMA).
[0086] Thermosetting materials can be selected from, for example: cyclic olefin copolymers, such as ethylene / norbornene or ethylene / cyclopentadiene copolymers; homopolymers and copolymers of allyl carbonates of linear or branched aliphatic or aromatic polyols, such as homopolymers of diethylene glycol bis(allyl carbonate) (CR). (); homopolymers and copolymers of (meth)acrylic acid and its esters that may be derived from bisphenol A; polymers and copolymers of thio(meth)acrylic acid and its esters, polymers and copolymers of allyl esters that may be derived from bisphenol A or phthalic acid and allyl aromatic hydrocarbons such as styrene, polymers and copolymers of urethane and thiourethane, polymers and copolymers of epoxy resins, and polymers and copolymers of sulfides, disulfides and cyclic sulfides, and combinations thereof.
[0087] As used herein, (co)polymer is intended to mean copolymer or polymer. As used herein, (meth)acrylate is intended to mean acrylate or methacrylate. As used herein, polycarbonate (PC) is intended to mean homopolymer or copolymer and block copolymer.
[0088] Diethylene glycol bis(allyl carbonate) homopolymer (CR) Allyl and (meth)acrylic acid copolymers (having a refractive index between 1.54 and 1.58), polymers and copolymers of thiourethane, and polycarbonate are preferred.
[0089] Prior to depositing the antireflective or specular coating disclosed herein, the substrate may be coated with one or more functional coatings. These functional coatings, commonly used in optical devices, may be, but are not limited to, impact-resistant primers, abrasion-resistant coatings and / or scratch-resistant coatings, polarizing coatings, photochromic coatings, or coloring coatings. Hereinafter, substrate means bare substrate or such coated substrate.
[0090] Prior to depositing a specular coating, the surface of the substrate is typically subjected to a physical or chemical surface activation treatment to enhance the adhesion of the antireflective or specular coating. This pretreatment is usually performed under vacuum. It can be bombardment with high-energy and / or reactive substances, such as ion beams (“ion pre-cleaning” or “IPC”) or electron beams, corona discharge treatment, ion spallation treatment, ultraviolet radiation treatment, or vacuum plasma-mediated treatment (typically using oxygen or argon plasma). It can also be an acidic or alkaline treatment and / or a solvent-based treatment (water, hydrogen peroxide, or any organic solvent).
[0091] Optical articles according to this disclosure include at least one ophthalmic lens or filter or optical glass or optical material suitable for human vision, such as at least one ophthalmic lens or filter, or optical film or patch intended to be fixed on a substrate, or optical glass, or optical material intended for use in ophthalmic instruments (e.g. for determining a subject's visual acuity and / or refractive error), or any kind of safety device (including safety glass or safety barriers intended to face an individual's eyes, such as protective devices (e.g., safety lenses or masks or shields)).
[0092] Optical articles can be implemented as eyeglass devices having a frame that at least partially surrounds one or more ophthalmic lenses. As non-limiting examples, optical articles can be eyeglasses, sunglasses, safety goggles, sports goggles, contact lenses, intraocular implants, active lenses with amplitude modulation (such as polarized lenses), or active lenses with phase modulation (such as autofocus lenses), etc.
[0093] At least one ophthalmic lens or optical glass or optical material suitable for human vision can provide optical functionality to the user (i.e., the wearer of the lens).
[0094] For example, an ophthalmic lens can be a corrective lens, that is, a spherical, cylindrical, and / or sub-light lens for users with refractive errors to treat myopia, hyperopia, astigmatism, and / or presbyopia. The lens can have a constant power, allowing it to provide power like a single-vision lens, or it can be a progressive lens with variable power.
[0095] The optical article disclosed herein has a back side on the side of the wearer's eye and a front side opposite to the back side. Furthermore, the optical article has an interference multilayer coating on the front, or on the back, or on both sides, the interference multilayer coating comprising at least one layer of a high refractive index material with a refractive index greater than 1.55 and at least one layer of a low refractive index material with a refractive index of 1.55 or less, the refractive index being expressed relative to a wavelength of 550 nm.
[0096] This optical product (also known as a specular coating) is designed such that it exhibits high reflectivity at low angles of incidence when viewed from its front or back, and antireflective properties at high angles of incidence when viewed from its front or back.
[0097] According to this disclosure:
[0098] - As defined in the preamble, at an angle of incidence greater than or equal to 35° and less than or equal to 55° perpendicular to the front or back of the optical article, the coating has an average visible light reflectance Rv of less than or equal to 2.5% for visible light irradiating the front or back of the optical article, and when the angle of incidence is greater than or equal to 35° and less than 50°, the average visible light reflectance Rv is even less than or equal to 2%, more preferably less than or equal to 1.5%; and
[0099] - At an angle of incidence greater than or equal to 0° and less than or equal to 15° relative to the front or back of the optical article, the coating has an average visible light reflectance Rv greater than or equal to 2.5% for visible light illuminating the front of the optical article, and at an angle of incidence greater than or equal to 0° and less than or equal to 10° relative to the front or back of the optical article, the average visible light reflectance Rv is even greater than or equal to 3.5%.
[0100] In the specific embodiments disclosed herein, the ratio between the Rv value Rv(0°) at the incident angle perpendicular to the front or back surface and the minimum Rv value Rvmin(35°-50°) at the incident angle with a perpendicular line to the front or back surface greater than or equal to 35° and less than or equal to 50° is greater than 3, preferably greater than 4, and more preferably greater than 5.
[0101] In the specific embodiments disclosed herein, the ratio between the Rv value Rv(10°) at an angle of incidence equal to 10° relative to the front or back surface and the minimum Rv value Rvmin(35°-50°) at an angle of incidence greater than or equal to 35° and less than or equal to 50° relative to the front or back surface is greater than 3, preferably greater than 4, and more preferably greater than 5.
[0102] In specific embodiments disclosed herein, the proposed mirror coating comprises alternating layers of high refractive index or "HI" material (typically having a refractive index greater than or equal to 1.5) and low refractive index or "LI" material (typically having a refractive index less than 1.5).
[0103] The mirror coating can be applied directly to the substrate or base material. Alternatively, at least one layer, such as a hard coating, can exist between the substrate and the mirror coating.
[0104] Alternating HI and LI layers can be arranged from the innermost to the outermost layer as follows:
[0105] - A first high-refractive-index material layer H1 has a physical thickness ranging from 15 to 50 nm and a relative optical thickness ranging from 0.05 to 0.20, which is defined as ROT = PT × n 550 / 550, where PT is the physical thickness, and n 550 It is the refractive index at 550 nm;
[0106] - A first low-refractive-index material layer L1, having a physical thickness ranging from 0 to 80 nm and a relative optical thickness ranging from 0.04 to 0.20;
[0107] - A second high-refractive-index material layer H2, having a physical thickness ranging from 40 nm to 100 nm and a relative optical thickness ranging from 0.10 to 0.50;
[0108] - A second low-refractive-index material layer L2, having a physical thickness ranging from 180 nm to 300 nm and a relative optical thickness ranging from 0.40 to 0.90;
[0109] - A third high-refractive-index material layer H3, having a physical thickness ranging from 50 nm to 120 nm and a relative optical thickness ranging from 0.15 to 0.50; and
[0110] - A third low-refractive-index material layer L3, having a physical thickness ranging from 80 nm to 150 nm and a relative optical thickness ranging from 0.20 to 0.40.
[0111] Furthermore, in the above embodiments:
[0112] - The physical thickness ratio between L3 and L2 is less than 0.5, and the relative optical thickness ratio between L3 and L2 is less than 0.5;
[0113] - The physical thickness ratio between L3 and H1 is greater than 3, and the relative optical thickness ratio between L3 and H1 is greater than 2.2;
[0114] The product of the physical thicknesses of L3 and H1 is less than 5000, and the product of the relative optical thicknesses of L3 and H1 is less than 0.05.
[0115] Figure 1 The left side shows the layer structure of a first comparative example of a prior art specular coating, and the right side shows the structure of a first non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure (the specular coating having low retroreflection and high forward reflection). The left column for both layer structures gives the material of the layer under consideration, and the right column gives its physical thickness.
[0116] Figure 1 The two mirror coatings shown consist of alternating Ta2O5 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0117] Table 1 below shows the optical properties h*, C*, and Rv of the mirror coating reflecting back at the normal angle of incidence of light (i.e., light illuminating the surface of the optical article perpendicular to the surface under consideration), which are summarized in Table 1 as “@0°”.
[0118] h*@0° C*@0° Rv@0°(%) Comparison with existing technology example 1 295 69 3.84 According to Example 1 of this disclosure 286 74 3.93
[0119] Table 1
[0120] Figure 2 The graph shows two curves, which give... Figure 1 The variation of Rv for the two mirror coatings under different incident angles θ is shown. For the prior art mirror coating, when θ ≤ 40°, Rv varies slightly between 3% and 4%. When θ > 40°, Rv increases rapidly.
[0121] In contrast, for the mirror coating according to this disclosure, the Rv is comparable to that of prior art mirror coatings only at low incident angles (θ ≤ 10°). In the incident angle range of 25° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2%.
[0122] Within the range of 35°≤θ≤50°, the Rv of the mirror coating according to this disclosure is even about 1% or less.
[0123] This feature of the proposed mirror coating can effectively minimize back-reflected light that may potentially reach the wearer's eyes.
[0124] Figure 3 The left side shows the layer structure of a second comparative example of a prior art specular coating, and the right side shows the structure of a second non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure (the specular coating having low reflection at high incident angles and high reflection at low incident angles). Figure 1 In the diagram, the left column for both layer structures indicates the material of the layer under consideration, and the right column indicates its physical thickness.
[0125] Figure 3 The two mirror coatings shown consist of alternating ZrO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0126] Figure 4 The graph shows two curves, which give... Figure 3 The variation of Rv for the two mirror coatings under different incident angles θ.
[0127] like Figure 4 As shown, Figure 3 The optical properties of the mirror coating are similar to Figure 1 and Figure 2 The optical properties of the first example are as follows: Specifically, for prior art specular coatings, Rv varies slightly between 2.9% and 4% when θ ≤ 40°. Rv increases rapidly when θ > 40°. In contrast, for the specular coating according to this disclosure, Rv is comparable to that of prior art specular coatings only at low incident angles (θ ≤ 10°). In the incident angle range of 25° ≤ θ ≤ 55°, the Rv of the specular coating according to this disclosure is always less than or equal to 2%. In the range of 35° ≤ θ ≤ 50°, the Rv of the specular coating according to this disclosure is even about 1% or less.
[0128] Other types of optical materials can also be used to design similar mirror coatings.
[0129] The HI layer may include, but is not limited to, one or more inorganic oxides, such as SiN, TiO2, PrTiO3, LaTiO3, ZrO2, Ta2O5, Y2O3, Ce2O3, La2O3, Dy2O5, Nb2O5, HfO2, Sc2O3, Pr2O3, Al2O3, or Si3N4.
[0130] Among the materials suitable for the LI layer, examples include, but are not limited to, SiO2, MgF2, ZrF4, Al2O3, AlF3, and cone cryolite (Na3[Al3F4]). 14 The LI layer preferably contains cryolite (Na3[Al2O3]), or any mixture thereof, preferably SiO2 or SiO2 doped with Al2O3 (which helps to increase the critical temperature of the stack). When using a SiO2 / Al2O3 mixture, the LI layer preferably contains 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 + Al2O3 in the LI layer).
[0131] In a preferred embodiment, the HI material is ZrO2, Ta2O5, Nb2O5, SiN, or TiO2, and the LI material is SiO2 or SiO2 doped with Al2O3, wherein the Al2O3-doped SiO2 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 + Al2O3 in the LI layer).
[0132] In such embodiments, the coating may comprise alternating layers of HI and LI refractive index materials, the alternating layers comprising, from the innermost to the outermost layer:
[0133] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 20-40 nm;
[0134] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the LI layer having a thickness of 10-80 nm).
[0135] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 46-95 nm;
[0136] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the LI layer having a thickness of 180-300 nm).
[0137] A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, wherein the layer has a thickness of 50-120 nm;
[0138] A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% by weight, more preferably 1% to 8% by weight of Al2O3 (relative to the total weight of SiO2 and Al2O3 in the LI layer having a thickness of 80-150 nm).
[0139] Figure 5 The left side shows the layer structure of a third comparative example of a prior art specular coating, and the right side shows the structure of a third non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure (the specular coating having low reflection at high incident angles and high reflection at low incident angles). Figure 1 In the diagram, the left column for both layer structures indicates the material of the layer under consideration, and the right column indicates its physical thickness.
[0140] As in the second example, Figure 5 The two mirror coatings shown consist of alternating ZrO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0141] Figure 6 The graph shows two curves, which give... Figure 5 The variation of Rv for the two mirror coatings under different incident angles θ.
[0142] like Figure 6 As shown, compared with the two examples above, the third example has a higher Rv at low incident angles, approximately 5.5% at 0°, compared with both the prior art mirror coating and the mirror coating according to this disclosure.
[0143] For prior art mirror coatings, Rv varies slightly between 4.6% and 5.5% when θ ≤ 30°. Rv increases rapidly when θ ≥ 35°. In contrast, for the mirror coating according to this disclosure, Rv is comparable to that of prior art mirror coatings only at low incident angles (θ ≤ 10°). In the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2%. In the range of 35° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even about 1.5% or less. Compared to the second example, when Rv@0° increases from 4% to 5.5%, the minimum Rv at high incident angles increases slightly from 0.09% to 1.12%.
[0144] Figure 7The left side shows the layer structure of a fourth comparative example of a prior art specular coating, and the right side shows the structure of a fourth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure (the specular coating having low reflection at high incident angles and high reflection at low incident angles). Figure 1 In the diagram, the left column for both layer structures indicates the material of the layer under consideration, and the right column indicates its physical thickness.
[0145] As in the second example, Figure 5 The two mirror coatings shown consist of alternating ZrO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0146] Figure 8 The graph shows two curves, which give... Figure 7 The variation of Rv for the two mirror coatings under different incident angles θ.
[0147] like Figure 8 As shown, for both the prior art mirror coating and the mirror coating according to this disclosure, compared with the above three examples, the fourth example has a higher Rv at low incident angles, approximately 8% at 0°.
[0148] For prior art mirror coatings, when θ ≤ 30°, Rv varies slightly between 7.9% and 8.2%. When θ ≥ 35°, Rv increases rapidly. In contrast, for the mirror coating according to this disclosure, the Rv is comparable to that of prior art mirror coatings only at low incident angles (θ ≤ 10°). In the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2.5%. In the range of 40° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even less than 1.9%.
[0149] Figure 9 A fifth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown, the structure of which (the specular coating has low reflection at high incident angles and high reflection at low incident angles) is illustrated. Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0150] Figure 9 The mirror coating shown consists of alternating TiO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0151] Figure 10 The graph shows the given Figure 9 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0152] like Figure 10 The fifth example shown has a higher Rv at low incident angles, approximately 4.5% at 0°.
[0153] Within the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2.5%. Within the range of 35° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even about 1.5% or less.
[0154] Figure 11 A sixth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown (the specular coating having low reflection at high incident angles and high reflection at low incident angles). As in Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0155] Figure 11 The mirror coating shown consists of alternating TiO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0156] Figure 12 The graph shows the given Figure 11 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0157] like Figure 12 The sixth example shown has a higher Rv at low incident angles, approximately 8% at 0°.
[0158] Within the incident angle range of 35°≤θ≤55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2.5%.
[0159] Figure 13 A seventh non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown (the specular coating having low reflection at high incident angles and high reflection at low incident angles). As in Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0160] Figure 13 The mirror coating shown consists of alternating TiO2 (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0161] Figure 14 The graph shows the given Figure 13 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0162] like Figure 14 The seventh example shown has a higher Rv at low incident angles, approximately 6% at 0°.
[0163] Within the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2.5%. Within the range of 35° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even about 1.5% or less.
[0164] Figure 15 An eighth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown (the specular coating having low reflection at high incident angles and high reflection at low incident angles). As in Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0165] Figure 15 The mirror coating shown consists of alternating layers of Ta2O5 (HI material) and SiO2 (LI material), forming a stack arranged on a hard coating (“HC”).
[0166] Figure 16 The graph shows the given Figure 15 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0167] like Figure 16 The eighth example shown has a higher Rv at low incident angles, approximately 8% at 0°.
[0168] Within the incident angle range of 35°≤θ≤55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2.5%.
[0169] Figure 17 A ninth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown (the specular coating having low reflection at high incident angles and high reflection at low incident angles). As shown in Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0170] Figure 17 The mirror coating shown consists of alternating SiN (HI material) layers and SiO2 (LI material) layers, forming a stack arranged on a hard coating (“HC”).
[0171] Figure 18 The graph shows the given Figure 17 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0172] like Figure 18 As shown, the ninth example has a higher Rv at low incident angles, approximately 5% at 0°.
[0173] Within the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2%. Within the range of 35° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even about 1.5% or less.
[0174] Figure 19 A tenth non-limiting example of a specular coating applied to the surface of an optical article according to this disclosure is shown (the specular coating having low reflection at high incident angles and high reflection at low incident angles). As shown in Figure 1 In the diagram, the left column of the layer structure gives the material of the layer under consideration, and the right column gives its physical thickness.
[0175] Figure 19 The mirror coating shown consists of alternating layers of Nb2O5 (HI material) and SiO2 (LI material), forming a stack arranged on a hard coating (“HC”).
[0176] Figure 20 The graph shows the given Figure 19 The curves showing the variation of Rv of the mirror coating under different incident angles θ.
[0177] like Figure 20 The tenth example shown has a higher Rv at low incident angles, approximately 5.5% at 0°.
[0178] Within the incident angle range of 35° ≤ θ ≤ 55°, the Rv of the mirror coating according to this disclosure is always less than or equal to 2%. Within the range of 35° ≤ θ ≤ 50°, the Rv of the mirror coating according to this disclosure is even about 1.5% or less.
[0179] Figure 21 The table provides the range of ROT and PT values for the first to the tenth instances, as well as a summary of the ratios L3 / L2 and L3 / H1 of ROT and PT, and the range of values for the product L3 x H1.
[0180] Figure 22 The table provides a similar summary of the first through fourth comparative examples.
[0181] In an embodiment, the coating according to this disclosure may be a colored mirror coating, that is, the mirror coating has a predetermined color.
[0182] Sunglasses according to this disclosure may have one or more (usually two) lenses having the optical features described above.
[0183] Although representative optical articles and sunglasses have been described in detail herein, those skilled in the art will recognize that various substitutions and modifications can be made without departing from the scope described and defined by the appended claims.
Claims
1. An optical article having a back side on the side of a wearer's eye and a front side opposite to the back side, wherein the optical article has an interference multilayer coating on at least one of the front and back sides, the interference multilayer coating comprising at least one layer of a high refractive index material with a refractive index greater than 1.55 and at least one layer of a low refractive index material with a refractive index of 1.55 or lower, the refractive index being expressed with respect to a wavelength of 550 nm, the optical article being designed such that it has high reflectivity at low angles of incidence when viewed from its front or back side, and antireflectivity at high angles of incidence when viewed from its front or back side. When the angle of incidence relative to the perpendicular line of the front or back surface is greater than or equal to 35° and less than or equal to 55°, the coating has an average visible light reflectance Rv of less than or equal to 2.5% for visible light irradiated onto the front or back surface; and With an incident angle greater than or equal to 0° and less than or equal to 15° relative to the perpendicular line of the front or back, the coating has an average visible light reflectance Rv greater than or equal to 2.5% for visible light irradiated onto the front or back.
2. The optical article according to claim 1, wherein, When the incident angle is greater than or equal to 35° and less than or equal to 50°, the average visible light reflectance coefficient Rv for back reflection is less than or equal to 2%.
3. The optical article according to claim 2, wherein, For back reflection, the average visible light reflectance Rv is less than or equal to 1.5%.
4. The optical article according to any one of claims 1 to 3, wherein, When the incident angle is greater than or equal to 0° and less than or equal to 10°, the average visible light reflectance Rv is greater than or equal to 3.5%.
5. The optical article according to any one of claims 1 to 3, wherein, The ratio between the Rv value Rv(0°) at the angle of incidence perpendicular to the front or back and the minimum Rv value Rvmin(35°-50°) at the angle of incidence relative to the front or back that is greater than or equal to 35° and less than or equal to 50° is greater than 3.
6. The optical article according to claim 5, wherein, The ratio between Rv (0°) and Rvmin (35°-50°) is greater than 4.
7. The optical article according to claim 6, wherein, The ratio between Rv (0°) and Rvmin (35°-50°) is greater than 5.
8. The optical article according to any one of claims 1 to 3, wherein, The ratio between the Rv value Rv(10°) at an angle of incidence equal to 10° relative to the front or back and the minimum Rv value Rvmin(35°-50°) at an angle of incidence greater than or equal to 35° and less than or equal to 50° relative to the front or back is greater than 3.
9. The optical article according to claim 8, wherein, The ratio between Rv (10°) and Rvmin (35°-50°) is greater than 4.
10. The optical article according to claim 9, wherein, The ratio between Rv (10°) and Rvmin (35°-50°) is greater than 5.
11. The optical article according to any one of claims 1 to 3, wherein, The coating comprises alternating layers of high-refractive-index and low-refractive-index materials, the alternating layers comprising, from the innermost to the outermost layer: A first high-refractive-index material layer (H1) has a physical thickness ranging from 15 to 50 nm and a relative optical thickness ranging from 0.05 to 0.20, wherein the relative optical thickness is defined as ROT = PT × n 550 / 550, where PT is the physical thickness, and n 550 It is the refractive index at 550 nm; A first low-refractive-index material layer (L1) has a physical thickness ranging from 10 to 80 nm and a relative optical thickness ranging from 0.04 to 0.
20. The second high-refractive-index material layer (H2) has a physical thickness ranging from 40 nm to 100 nm and a relative optical thickness ranging from 0.10 to 0.
50. The second low-refractive-index material layer (L2) has a physical thickness ranging from 180 nm to 300 nm and a relative optical thickness ranging from 0.40 to 0.
90. A third high-refractive-index material layer (H3) has a physical thickness ranging from 50 nm to 120 nm and a relative optical thickness ranging from 0.15 to 0.50; and The third low-refractive-index material layer (L3) has a physical thickness ranging from 80 nm to 150 nm and a relative optical thickness ranging from 0.20 to 0.
40.
12. The optical article according to claim 11, wherein: The physical thickness ratio between the third low-refractive-index material layer (L3) and the second low-refractive-index material layer (L2) is less than 0.5, and the relative optical thickness ratio between the third low-refractive-index material layer (L3) and the second low-refractive-index material layer (L2) is less than 0.5; The physical thickness ratio between the third low-refractive-index material layer (L3) and the first high-refractive-index material layer (H1) is greater than 3, and the relative optical thickness ratio between the third low-refractive-index material layer (L3) and the first high-refractive-index material layer (H1) is greater than 2.2; The product of the physical thickness of the third low-refractive-index material layer (L3) and the first high-refractive-index material layer (H1) is less than 5000, and the product of the relative optical thickness of the third low-refractive-index material layer (L3) and the first high-refractive-index material layer (H1) is less than 0.
05.
13. The optical article according to any one of claims 1 to 3, wherein, The high refractive index material is SiN, TiO2, PrTiO3, LaTiO3, ZrO2, Ta2O5, Y2O3, Ce2O3, La2O3, Dy2O5, Nb2O5, HfO2, Sc2O3, Pr2O3, Al2O3, or Si3N4, and the low refractive index material is SiO2, MgF2, ZrF4, Al2O3, AlF3, or Na3[Al3F] cryolite. 14 ], cryolite Na3[AlF6], or any mixture thereof.
14. The optical article according to claim 13, wherein, The low-refractive-index material is SiO2 or SiO2 doped with Al2O3, wherein the Al2O3 doped SiO2 contains 1% to 10% Al2O3 by weight relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer.
15. The optical article according to claim 14, wherein, The SiO2 doped with Al2O3 has 1% to 8% Al2O3 by weight, relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer.
16. The optical article according to claim 13, wherein, The high refractive index material is ZrO2, Ta2O5, Nb2O5, SiN or TiO2, and the low refractive index material is SiO2 or Al2O3-doped SiO2, wherein the Al2O3-doped SiO2 has 1% to 10% Al2O3 by weight relative to the total weight of SiO2 and Al2O3 in the low refractive index material layer.
17. The optical article according to claim 16, wherein, The SiO2 doped with Al2O3 has 1% to 8% Al2O3 by weight, relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer.
18. The optical article according to claim 16, wherein, The coating comprises alternating layers of high-refractive-index and low-refractive-index materials, the alternating layers comprising, from the innermost to the outermost layer: A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 20-40 nm; A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% Al2O3 by weight, relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer having a thickness of 10-80 nm. A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 46-95 nm; A layer of SiO2 or SiO2 doped with Al2O3, wherein the SiO2 doped with Al2O3 has 1% to 10% Al2O3 by weight relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer having a thickness of 180-300 nm. A layer of ZrO2, Ta2O5, Nb2O5, SiN or TiO2, the layer having a thickness of 50-120 nm; A layer of SiO2 or SiO2 doped with Al2O3, wherein the Al2O3 doped SiO2 contains 1% to 10% Al2O3 by weight, relative to the total weight of SiO2 and Al2O3 in the low-refractive-index material layer having a thickness of 80-150 nm.
19. The optical article according to claim 18, wherein, At least one of the low-refractive-index material layers in the alternating layers is: an Al2O3-doped SiO2 layer having Al2O3 comprising 1% to 8% by weight of the total weight of SiO2 and Al2O3.
20. The optical article according to any one of claims 1 to 3, wherein, The optical article is an ophthalmic lens, a device having a safety barrier intended to face the wearer's eye, a filter, or an optical film or patch intended to be fixed to a substrate.
21. A type of sunglasses, wherein, The sunglasses include at least one optical article according to any one of claims 1 to 20.
Citation Information
Patent Citations
Mirror-coated lens
EP3118658A1
Mirror-coated lens
CN106104312A
An OPTICAL LENS COMPRISING AN ANTIREFLECTIVE COATING WITH MULTIANGULAR EFFICIENCY
CN109791219A