Methods to improve the resistance stability of thin films

By measuring the thickness of the implantation barrier layer, adjusting the ion implantation dose, and employing a low-power etching process, the problem of thin-film resistance stability was solved, and resistance uniformity and lattice structure were improved.

CN117393448BActive Publication Date: 2026-11-17SHANGHAI HUAHONG GRACE SEMICON MFG CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311188970.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-14
Publication Date
2026-11-17
Estimated Expiration
2043-09-14

AI Technical Summary

Technical Problem

In the semiconductor integrated circuit manufacturing process, the stability of thin-film resistors is affected by the thickness of the implantation barrier layer and the dry etching process, resulting in fluctuations in resistance uniformity and damage to the crystal structure, which are difficult to effectively improve with existing technologies.

Method used

By measuring the thickness of the implantation barrier layer, adjusting the ion implantation dose, and using a low-power etching process to remove the sacrificial oxide layer, a new ion implantation dose value is formed, reducing batch-to-batch variations and mitigating etching damage to the crystal lattice.

Benefits of technology

This improves the stability and in-plane uniformity of thin-film resistors, reduces resistance differences between batches, and improves the overall performance of thin-film resistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117393448B_ABST
    Figure CN117393448B_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the resistance stability of thin films: forming a sacrificial oxide layer as an implantation barrier layer for ion implantation; measuring the thickness T of the sacrificial oxide layer; opening an ion implantation window for ion implantation, adjusting and compensating the implantation dose based on the measured thickness T of the sacrificial oxide layer to obtain a compensated ion implantation dose D; performing ion implantation at the ion implantation window using the ion implantation dose D; after implantation, removing the photoresist and performing annealing activation; removing the sacrificial oxide layer using a low-power etching process to reduce plasma damage from etching. This invention calculates ion implantation compensation for different batches by analyzing the correlation between the ion implantation dose, the thickness of the implantation barrier layer, and lattice damage, reducing batch-to-batch differences after ion implantation; the low-power etching process improves in-plane uniformity and enhances the resistance stability of the thin film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor integrated circuit manufacturing processes, and in particular to a method for improving the resistance stability of thin films after implantation. Background Technology

[0002] As the size of integrated circuit components manufactured by the semiconductor industry becomes smaller and smaller, the requirements for the performance of various semiconductor devices are becoming higher and higher. As an important parameter characterizing the performance of semiconductor devices, the stability of thin-film resistors is particularly important.

[0003] In the process of integrated circuit manufacturing, a sacrificial oxide layer is typically grown before the doping of thin-film resistors. This layer acts as an implantation barrier, and its thickness (T) affects subsequent doping processes, thus affecting the thin-film resistor. When this oxide layer is removed by dry etching, the introduction of plasma causes high-energy particles to collide with atoms in the crystal lattice, resulting in the displacement of some lattice atoms. Impurity atoms that were originally in their replacement positions are scattered to interstitial positions, which also leads to changes in the thin-film resistor.

[0004] Analyzing from the perspective of the thickness of the injection barrier layer: The test data shows that the sheet resistance is directly proportional to the thickness of the injection barrier layer and inversely proportional to the injection dose. Therefore, compensating for the subsequent injection dose based on the thickness of the injection barrier layer can effectively reduce the impact of injection barrier layer thickness fluctuations on the sheet resistance.

[0005] From the perspective of reducing lattice damage: In traditional implantation processes, the implantation dose is fixed for different implantation barrier layer thicknesses, and high-power plasma etching is used to remove the barrier layer during subsequent dry etching.

[0006] If the injection barrier layer is removed by dry etching, a large number of high-energy particles will damage the lattice structure of the thin-film resistor when the plasma contacts the interface of the thin-film resistor, affecting the in-plane uniformity of the thin-film resistor.

[0007] Studies have found that the etching power of the dry etching process used to remove the implantation barrier layer has a significant impact on the lattice structure of the thin-film resistor. Comparative tests were conducted on two batches of products using different etching powers. The results showed that lower power etching significantly reduced the uniformity fluctuations in resistance, as shown in the table below: Summary of the Invention

[0008] The technical problem to be solved by the present invention is to provide a method for improving the resistance stability of a thin film after injection.

[0009] To address the above problems, the present invention provides a method for improving the resistance stability of a thin film after injection, comprising: A semiconductor substrate is provided, and a sacrificial oxide layer is formed on the semiconductor substrate, the sacrificial oxide layer serving as an implantation barrier layer for ion implantation; The thickness of the sacrificial oxide layer on the semiconductor substrate is measured to obtain the thickness measurement value T; Coating photoresist and performing photolithography to open the ion implantation window of the photoresist; Ion implantation is performed on the opened ion implantation window, and the implanted ions penetrate the sacrificial oxide layer and enter the semiconductor substrate; the implantation dose is adjusted and compensated according to the thickness measurement value T of the sacrificial oxide layer to obtain the compensated ion implantation dose D, and ion implantation is performed on the ion implantation window with the ion implantation dose D; After the injection is completed, the photoresist is removed, and annealing and activation are performed. To remove the sacrificial oxide layer, a low-power etching process with an etching power of no more than 150W is used to reduce plasma damage during etching.

[0010] Furthermore, the semiconductor substrate includes a silicon substrate, a germanium silicon substrate, a gallium arsenide substrate, a gallium nitride substrate, and a silicon carbide substrate.

[0011] Furthermore, ion implantation is performed on the opened ion implantation window. The ion implantation dose is automatically compensated proportionally based on the thickness T of the sacrificial oxide layer measured before each batch of implantation. The center value of the film thickness fluctuation of the sacrificial oxide layer is T0.

[0012] Furthermore, the ion implantation process also includes: The influence factors K1 and K2 of the thickness of the sacrificial oxide layer on the resistance of the product wafer; the injection dose D0 in the existing process without adjustment; The ion implantation dose is D, where D = D0 + K1 / K2 * (T - T0).

[0013] Furthermore, the removal of the sacrificial oxide layer is performed using a low-power plasma dry etching process.

[0014] The method for improving the resistance stability of thin films after implantation, as described in this invention, reduces batch-to-batch differences by measuring the thickness of the implantation barrier layer and lattice damage, and by calculating ion implantation compensation based on the thickness differences of the implantation barrier layer in different batches. Furthermore, the use of a low-power etching process to remove the implantation barrier layer can further reduce interface structure damage, improve in-plane uniformity, and enhance the resistance stability of the thin films. Attached Figure Description

[0015] Figure 1 This is a flowchart of the process steps of the present invention. Implementation

[0016] The following detailed description, in conjunction with the accompanying drawings, provides specific embodiments of the present invention and clearly and completely describes the technical solutions of the present invention. However, the present invention is not limited to the following embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The advantages and features of the present invention will become clearer from the following description and claims. It should be noted that the accompanying drawings are all in a very simplified form and use non-precise ratios, and are only used for the purpose of conveniently and clearly illustrating the embodiments of the present invention. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] This invention can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the invention to those skilled in the art. In the drawings, for clarity, the dimensions and relative dimensions of layers and regions may be exaggerated, and the same reference numerals denote the same elements throughout. In the description of this application, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," "outer," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0018] The method for improving the resistance stability of a thin film after implantation according to the present invention comprises: A semiconductor substrate is provided, comprising, but not limited to, any one of silicon, germanium-silicon, gallium arsenide, gallium nitride, and silicon carbide substrates. Widely used semiconductor materials in the industry are acceptable. Taking a silicon substrate as an example, a sacrificial oxide layer is first formed on the silicon substrate, which serves as an implantation barrier layer for subsequent ion implantation. In the production line, the thickness of the implantation barrier layer formed in different batches (lots) of wafers varies and fluctuates within a certain range. Therefore, after the implantation barrier layer is formed, the thickness of the sacrificial oxide layer on the semiconductor substrate is measured to obtain the current thickness measurement value T of the implantation barrier layer.

[0019] Photoresist is coated and solidified and photolithographic processes are performed to pattern the photoresist. Ion implantation windows in the corresponding areas of the photoresist are opened to expose the implantation barrier layer on the silicon substrate within the window.

[0020] Ion implantation is performed through the opened ion implantation window, with the implanted ions penetrating the sacrificial oxide layer and entering the semiconductor substrate. The implantation dose is automatically adjusted and compensated proportionally based on the measured thickness T of the sacrificial oxide layer, resulting in a compensated ion implantation dose value D. Ion implantation is then performed on the ion implantation window using this dose value D. This process involves two important parameters: the influence factor K1 of the sacrificial oxide layer thickness on the film resistance, which is a linear relationship coefficient between film resistance and sacrificial oxide layer thickness; and the influence factor K2 of the implantation dose on the film resistance, which is also a linear relationship coefficient between film resistance and implantation dose. These two parameters, K1 and K2, can be obtained through a limited number of experimental tests. Additionally, the film thickness fluctuation center value of the sacrificial oxide layer is T0. A new compensated ion implantation dose D is calculated based on the existing ion implantation dose D0, as follows: D = D0 + K1 / K2 * (T - T0).

[0021] Ion implantation is performed on the opened ion implantation window using the newly calculated compensated ion implantation dose D. Compensating the subsequent implantation dose based on the thickness of the implantation barrier layer can effectively reduce the impact of the barrier layer thickness on the average resistivity of the sheet.

[0022] After ion implantation, the photoresist is removed, and the impurities are annealed and activated.

[0023] The sacrificial oxide layer is removed. A low-power etching process with an etching power not exceeding 150W is used to remove the sacrificial oxide layer. This low-power plasma etching process reduces the bombardment intensity of the plasma on the interface of the thin-film resistor, mitigating the impact of high-power plasma etching on the lattice structure and the in-plane uniformity of the thin-film resistor.

[0024] The method for improving the resistance stability of a thin film after implantation, as described in this invention, establishes a new ion implantation dose value D by measuring the thickness of the implantation barrier layer and lattice damage, and calculating ion implantation compensation based on the thickness differences of the implantation barrier layer in different batches. Compared with the fixed ion implantation dose D0 in traditional processes, this method can select a more suitable ion implantation dose value based on the current film thickness, reducing batch-to-batch differences after ion implantation. Furthermore, the use of a low-power etching process to remove the implantation barrier layer can further reduce interface structure damage, improve in-plane uniformity, and enhance the stability of the thin film resistance.

[0025] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for improving the resistance stability of a thin film, characterized in that: A semiconductor substrate is provided, and a sacrificial oxide layer is formed on the semiconductor substrate, the sacrificial oxide layer serving as an implantation barrier layer in an ion implantation process; The thickness of the sacrificial oxide layer formed on the semiconductor substrate is measured to obtain the current thickness measurement value T of the sacrificial oxide layer; Coating photoresist and performing photolithography to open the ion implantation window of the photoresist; The sacrificial oxide layer is exposed within the ion implantation window, while the sacrificial oxide layer in the unopened area remains covered by the photoresist. Ion implantation is performed through the opened ion implantation window, and the implanted ions penetrate the sacrificial oxide layer and enter the semiconductor substrate; The implanted dose is calculated by compensating for the thickness measurement T of the sacrificial oxide layer to obtain the compensated ion implantation dose D, and ion implantation is performed on the ion implantation window with the ion implantation dose D. After the ion implantation is completed, the photoresist is removed, and an annealing activation process is performed to activate impurities and repair the lattice damage caused by ion implantation. The sacrificial oxide layer is removed, and etching is performed using a low etching power that minimizes damage to the thin-film resistive lattice structure.

2. The method for improving the resistance stability of a thin film as described in claim 1, characterized in that: The semiconductor substrates include silicon substrates, germanium-silicon substrates, gallium arsenide substrates, gallium nitride substrates, and silicon carbide substrates.

3. The method for improving the resistance stability of a thin film as described in claim 1, characterized in that: Ion implantation is performed through the opened ion implantation window. The ion implantation dose is automatically compensated proportionally based on the thickness T of the sacrificial oxide layer measured before each batch of implantation. The center value of the film thickness fluctuation of the sacrificial oxide layer is T0.

4. The method for improving the resistance stability of a thin film as described in claim 3, characterized in that: The ion implantation process also includes: The influence factor K1 of the thickness of the sacrificial oxide layer on the sheet resistance of the product, wherein the influence factor K1 is the linear relationship coefficient between the sheet resistance and the thickness of the sacrificial oxide layer; the influence factor K2 of the implantation dose on the sheet resistance, wherein the influence factor K2 is the linear relationship coefficient between the sheet resistance and the implantation dose; and the implantation dose D0 in the unadjusted existing process; The compensated ion implantation dose D is then calculated as D0 + K1 / K2 * (T - T0).

5. The method for improving the resistance stability of a thin film as described in claim 1, characterized in that: The removal of the sacrificial oxide layer is achieved by using a low-power plasma dry etching process.

6. The method for improving the resistance stability of a thin film as described in claim 1, characterized in that: The sacrificial oxide layer is formed by thermal oxidation or deposition on the semiconductor substrate to a predetermined thickness.

7. The method for improving the resistance stability of a thin film as described in claim 1, characterized in that: The etching power for removing the sacrificial oxide layer is no higher than 150W.

Citation Information

Patent Citations

  • Manufacturing method of gate oxidation films

    CN101131961A

  • Preparation method of semiconductor device

    CN104425282A