A positive electrode material and its preparation method, a positive electrode sheet and a battery
By employing a structural design of lithium iron phosphate inner layer and lithium-rich manganese-based outer layer in lithium-rich manganese-based cathode material, combined with carbon source coating, the problem of low initial charge-discharge efficiency of lithium-rich manganese-based cathode material was solved, achieving high energy density and stable lithium-ion transport, and improving the cycle performance of the battery.
Patent Information
- Application Number
- CN202311600369.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-24
AI Technical Summary
The low initial charge-discharge efficiency of lithium-rich manganese-based cathode materials leads to an increase in irreversible capacity and a decrease in cycle performance.
The material uses lithium iron phosphate as the inner layer and lithium-rich manganese-based material as the outer layer. The coating structure is formed by dry mixing and heat treatment, and combined with carbon source coating, the conductivity and stability of the material are improved.
This improved the energy density and cycle performance of the cathode material, reduced voltage decay, enhanced lithium-ion transport stability, and improved the electrochemical performance of the material.
Smart Images

Figure CN117423821B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, and in particular to a positive electrode material and its preparation method, a positive electrode sheet, and a battery. Background Technology
[0002] Lithium-ion batteries, characterized by high energy density and long cycle life, are considered an important "green energy source" for future electric and hybrid vehicles. However, the energy density of lithium-ion batteries is currently insufficient to meet the demands of pure electric vehicles. Developing lithium-ion batteries with high specific capacity, high energy density, high cycle performance, and low degradation is crucial for their future development.
[0003] Currently, lithium-rich manganese-based cathode materials have attracted widespread attention due to their high specific capacity (greater than 200 mAh / g). These materials are solid solutions formed from layered Li₂MnO₃ and LiMO₂ (M = Mn, Ni, Co) in varying proportions, and their chemical formula can be written as xLi₂MnO₃·(1-x)LiMeO₂ or Li[Li x / 3 Me 1-x Mn 2x / 3 Although lithium-rich manganese-based cathode materials have high specific capacity, they also have some problems, such as very low initial charge-discharge efficiency. The reason for the low initial charge-discharge efficiency is that when the material is first charged to 4.5V, Li in the transition metal layer in its layered structure is net extracted from the structure as Li2O, accompanied by the generation of O2 and structural rearrangement. This net extracted Li2O cannot return to the crystal lattice, resulting in a large irreversible capacity and low initial charge-discharge efficiency. Summary of the Invention
[0004] The purpose of this invention is to overcome the problem of low initial charge-discharge efficiency of lithium-rich manganese-based cathode materials in the prior art, and to provide a cathode material, its preparation method, cathode sheet, and battery.
[0005] A first aspect of this invention provides a cathode material, comprising an inner layer material and an outer layer material coating the inner layer material; the inner layer material is a lithium iron phosphate material, and the outer layer material is a lithium-rich manganese-based material, wherein the chemical formula of the lithium-rich manganese-based material is Li. x Ni y Mn z O2, where 1.5>x>1.2, 0.3>y>0.1, 0.8>z>0.2.
[0006] In the cathode material provided by the embodiments of the present invention, lithium iron phosphate material is used as the inner layer material and lithium-rich manganese-based material is used as the outer layer material. This can effectively improve the compaction density and specific capacity of the cathode material, thereby improving the energy density and cycle performance of the cathode material and reducing voltage decay during the cycle process. This makes the lithium iron phosphate material have both high performance and high efficiency. Furthermore, during the charge and discharge process, the lithium-rich manganese-based material, as a lithium-rich material, can also act as a lithium replenishing agent to provide lithium ions to the lithium iron phosphate material, reducing the loss of active lithium in the early stage of the lithium iron phosphate material.
[0007] The cathode material provided by this invention is supplied with lithium iron phosphate by an outer layer of lithium-rich manganese-based material in the direction of lithium ion transport. Since the structure of the lithium-rich manganese-based material is unstable after lithium ions are released, this invention adopts a structure attached to lithium iron phosphate, which can support the material framework, improve the stability of lithium ion transport, and thus improve the electrochemical performance of the material.
[0008] However, if a structure with lithium-rich manganese-based material in the inner layer and lithium iron phosphate in the outer layer is used, the material structure may collapse, preventing lithium ions from returning to the material structure and reducing the material's cycle performance.
[0009] In a preferred embodiment, the cathode material further includes a coating on at least a portion of the surface of the outer layer material, the coating containing carbon.
[0010] In this embodiment, the carbon-containing coating can effectively improve the conductivity of the cathode material.
[0011] In a preferred embodiment, the lithium iron phosphate material has the chemical formula LiFePO4.
[0012] In a preferred embodiment, the lithium iron phosphate material accounts for more than 60% and less than 85% by mass in the cathode material.
[0013] In a preferred embodiment, the lithium-rich manganese-based material accounts for more than 15% and less than 40% by mass in the cathode material.
[0014] A second aspect of this invention provides a method for preparing a cathode material, comprising the following steps:
[0015] Lithium iron phosphate material and lithium-rich manganese-based material are dry-mixed to obtain a mixture.
[0016] The mixture is heat-treated to obtain the cathode material;
[0017] The lithium iron phosphate has a D50 of 1 μm to 2 μm, and the lithium-rich manganese-based material has a D50 of 0.1 μm to 0.2 μm.
[0018] The chemical formula of the lithium-rich manganese-based material is Lix Ni y Mn z O2, where 1.5>x>1.2, 0.3>y>0.1, 0.8>z>0.2.
[0019] The electrical and physical properties of lithium iron phosphate materials and lithium-rich manganese-based materials prepared by dry mixing are the best under the above particle size conditions. If the particle size is too large, the electrical properties of the material will deteriorate, and if it is too small, the physical properties, compaction and vibration indicators of the material will not meet the standards.
[0020] This invention employs a dry mixing method, and the chemical formula of the lithium-rich manganese-based material used is Li. x Ni y Mn z O2, where 1.5>x>1.2, 0.3>y>0.1, 0.8>z>0.2, has a single molecular mass lower than that of LiFePO4 (157). Therefore, the two materials used in this invention, with their lighter single molecular mass, are more likely to float on the outer layer. Thus, during dry stirring and rotation, they will float to the outer layer. Subsequently, due to the combined action of intermolecular forces and electrostatic forces, the lithium-rich manganese-based material adheres to the surface of the lithium iron phosphate material, which is impossible to achieve in wet synthesis.
[0021] Furthermore, the preparation method provided in this embodiment is an in-situ one-step formation, with a simple process flow that is easy to industrialize.
[0022] In a preferred embodiment, the lithium iron phosphate material has the chemical formula LiFePO4.
[0023] In a preferred embodiment, the heat treatment temperature is above 300°C and below 500°C, and the heat treatment time is above 4 hours and below 7 hours.
[0024] In a preferred embodiment, the dry mixing method is vortex mixing.
[0025] It is worth noting that, reference Figure 2The dry mixing granulator used in this invention can achieve vortex mixing. The granulation cylinder of the equipment rotates, and the rotor is mounted eccentrically on a granulation disc located inside the granulation cylinder. The granulation disc is also equipped with fixed scrapers that push the material towards the mixing tool, achieving thorough mixing. The granulation disc and rotor rotate together, thereby significantly improving the coating effect and efficiency of the lithium-rich manganese-based material. The maximum rotational speed is 2500 rpm, and the maximum revolution speed is 500 rpm. It should be noted that the rotational speed refers to the speed of the internal mixing paddle, and the revolution speed refers to the speed of the external container. Compared with conventional mixing, this invention preferably uses an eccentric rotor and vortex mixing, which has the following advantages: 1. Optimal material mixing uniformity; 2. Shortest mixing time; 3. Less wear; 4. Enables batch or continuous operation.
[0026] In a preferred embodiment, the preparation method further includes: adding a carbon source to form a carbon-containing coating on the surface of the cathode material; preferably, the carbon source accounts for less than 10% of the mass percentage of the cathode material.
[0027] In the preferred embodiment of the present invention, the preparation method involves physically mixing lithium iron phosphate, lithium-rich manganese-based material, and carbon source. During the mixing process, friction and collision occur, causing the lithium-rich manganese-based material to be uniformly dispersed and adsorbed onto the surface of lithium iron phosphate to form a coating layer. The mixing process generates eddies. Since the particle sizes of lithium iron phosphate, lithium-rich manganese-based material, and carbon source are different, and the carbon source, being lighter, floats on the outer layer when eddies are generated, while the lithium-rich manganese-based material, being smaller in particle size, is adsorbed onto the surface of lithium iron phosphate, thus forming a structure with lithium iron phosphate as the inner layer and lithium-rich manganese-based material as the outer layer.
[0028] In a preferred embodiment, the carbon source is an organic carbon source, preferably glucose, sucrose, PEG, etc.
[0029] It should be noted that the inventors discovered through research that when carbon coating is performed on the cathode material provided by this invention, using an organic carbon source can achieve a better coating effect during the coating and sintering process, while the adhesion of an inorganic carbon source is weaker and may detach from the surface of the cathode material, resulting in reduced conductivity.
[0030] A third aspect of the present invention provides a positive electrode sheet, characterized in that it uses the positive electrode material as described above or the positive electrode material prepared by the preparation method as described above as the positive electrode active material.
[0031] A fourth aspect of this invention provides a battery, characterized in that: the battery comprises a positive electrode as described above. Other features and beneficial effects of the invention will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other beneficial effects of the invention can be realized and obtained by means of the structures particularly pointed out in the description, claims, and drawings. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Unless otherwise specified, the positional relationships shown in the drawings in the following description are based on the direction in which the components are drawn in the figure.
[0033] Figure 1 This is a SEM image of the cathode material prepared in Example 3 of the present invention;
[0034] Figure 2 This is a schematic diagram of the internal mixing flow field of the dry mixing granulator of the present invention;
[0035] Figure 3 The first charge-discharge curve of a lithium battery prepared by combining the positive electrode material obtained in Example 3 of this invention with a negative electrode sheet. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. The technical features designed in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0037] The technical solution of the present invention will be further illustrated and described below through specific embodiments. However, the scope of protection of the present invention is not limited thereto.
[0038] Example 1
[0039] This embodiment provides a cathode material, the cathode material being composed of 60% lithium iron phosphate material by mass and 40% lithium-rich manganese-based material by mass;
[0040] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.25 μm;
[0041] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, the D50 of the lithium-rich manganese-based material is 0.12 μm;
[0042] The method for preparing the cathode material includes the following steps:
[0043] (1) Weigh out lithium iron phosphate material and lithium-rich manganese-based material according to the proportion;
[0044] (2) Add to a dry mixing granulator for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 500 rpm.
[0045] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 4.5 hours at a temperature of 400°C to obtain the positive electrode material.
[0046] Example 2
[0047] This embodiment provides a cathode material, the cathode material being composed of 70% lithium iron phosphate material by mass, 30% lithium-rich manganese-based material by mass, and 0% carbon source by mass.
[0048] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.25 μm;
[0049] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, the D50 of the lithium-rich manganese-based material is 0.12 μm;
[0050] The carbon source is glucose;
[0051] The method for preparing the cathode material includes the following steps:
[0052] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0053] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 500 rpm.
[0054] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 4.5 hours at a temperature of 400°C to obtain the positive electrode material.
[0055] Example 3
[0056] This embodiment provides a cathode material, the cathode material being composed of 60% lithium iron phosphate material by mass, 30% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0057] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.25 μm;
[0058] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, the D50 of the lithium-rich manganese-based material is 0.12 μm;
[0059] The carbon source is glucose;
[0060] The method for preparing the cathode material includes the following steps:
[0061] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0062] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 500 rpm.
[0063] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 4.5 hours at a temperature of 450°C to obtain the positive electrode material.
[0064] The obtained cathode material can be observed under an electron microscope to obtain the following results: Figure 1 The SEM image shown indicates that it includes an inner layer material and an outer layer material covering the inner layer material; the inner layer material is lithium iron phosphate, and the outer layer material is lithium-rich manganese-based; and the first charge-discharge curve of the lithium battery prepared by combining the positive electrode material with the negative electrode sheet in this embodiment is shown in the figure. Figure 3 As shown.
[0065] Example 4
[0066] This embodiment provides a cathode material, the cathode material being composed of 60% lithium iron phosphate material by mass, 30% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0067] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.3 μm;
[0068] The lithium-rich manganese-based material is Li 1.25 Ni0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0069] The carbon source is glucose;
[0070] The method for preparing the cathode material includes the following steps:
[0071] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0072] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 500 rpm.
[0073] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 4.5 hours at a temperature of 450°C to obtain the positive electrode material.
[0074] Example 5
[0075] This embodiment provides a cathode material, the cathode material being composed of 60% lithium iron phosphate material by mass, 30% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0076] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.3 μm;
[0077] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0078] The carbon source is glucose;
[0079] The method for preparing the cathode material includes the following steps:
[0080] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0081] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1500 rpm and the revolution speed is 400 rpm.
[0082] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 4.5 hours at a temperature of 500°C to obtain the positive electrode material.
[0083] Example 6
[0084] This embodiment provides a cathode material, the cathode material being composed of 60% lithium iron phosphate material by mass, 30% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0085] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.3 μm;
[0086] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0087] The carbon source is glucose;
[0088] The method for preparing the cathode material includes the following steps:
[0089] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0090] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 500 rpm.
[0091] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 6 hours at a temperature of 500°C to obtain the positive electrode material.
[0092] Example 7
[0093] This embodiment provides a cathode material, the cathode material being composed of 63% lithium iron phosphate material by mass, 25% lithium-rich manganese-based material by mass, and 12% carbon source by mass.
[0094] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.35 μm;
[0095] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.16 μm;
[0096] The carbon source is glucose;
[0097] The method for preparing the cathode material includes the following steps:
[0098] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0099] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1500 rpm and the revolution speed is 300 rpm.
[0100] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 6 hours at a temperature of 450°C to obtain the positive electrode material.
[0101] Example 8
[0102] This embodiment provides a cathode material, the cathode material being composed of 80% lithium iron phosphate material by mass, 10% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0103] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.4 μm;
[0104] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0105] The carbon source is glucose;
[0106] The method for preparing the cathode material includes the following steps:
[0107] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0108] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1600 rpm and the revolution speed is 500 rpm.
[0109] (3) The mixture is added to a square notched crucible and heat-treated in air for 5 hours at a temperature of 500°C to obtain the positive electrode material.
[0110] Example 9
[0111] This embodiment provides a cathode material, the cathode material being composed of 70% lithium iron phosphate material by mass, 20% lithium-rich manganese-based material by mass, and 10% carbon source by mass.
[0112] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.5 μm;
[0113] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0114] The carbon source is glucose;
[0115] The method for preparing the cathode material includes the following steps:
[0116] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0117] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1800 rpm and the revolution speed is 400 rpm.
[0118] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 6 hours at a temperature of 500°C to obtain the positive electrode material.
[0119] Example 10
[0120] This embodiment provides a cathode material, the cathode material being composed of 65% lithium iron phosphate material by mass, 20% lithium-rich manganese-based material by mass, and 15% carbon source by mass.
[0121] The lithium iron phosphate material is LiFePO4, and the D50 of the lithium iron phosphate material is 1.6 μm;
[0122] The lithium-rich manganese-based material is Li 1.25 Ni 0.15 Mn 0.4 O2, wherein the D50 of the lithium-rich manganese-based material is 0.15 μm;
[0123] The carbon source is glucose;
[0124] The method for preparing the cathode material includes the following steps:
[0125] (1) Weigh out the lithium iron phosphate material, lithium-rich manganese-based material and carbon source according to the proportion;
[0126] (2) Add to a high-speed mixer for vortex mixing to obtain a mixture. During the mixing process, the rotation speed is 1500 rpm and the revolution speed is 400 rpm.
[0127] (3) The mixture is added to a square notched crucible and heat-treated in air atmosphere for 6 hours at a temperature of 400°C to obtain the positive electrode material.
[0128] Comparative Example 1
[0129] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 0.8 μm.
[0130] Comparative Example 2
[0131] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 2.1 μm.
[0132] Comparative Example 3
[0133] The rest is the same as in Example 3, except that the D50 of the lithium-rich manganese-based material used in this comparative example is 0.08 μm.
[0134] Comparative Example 4
[0135] The rest is the same as in Example 3, except that the D50 of the lithium-rich manganese-based material used in this comparative example is 0.21 μm.
[0136] Comparative Example 5
[0137] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 0.8 μm and the D50 of the lithium-rich manganese-based material is 0.08 μm.
[0138] Comparative Example 6
[0139] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 0.8 μm and the D50 of the lithium-rich manganese-based material is 0.21 μm.
[0140] Comparative Example 7
[0141] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 2.1 μm and the D50 of the lithium-rich manganese-based material is 0.08 μm.
[0142] Comparative Example 8
[0143] The rest is the same as in Example 3, except that the D50 of the lithium iron phosphate material used in this comparative example is 2.1 μm and the D50 of the lithium-rich manganese-based material is 0.21 μm.
[0144] Comparative Example 9
[0145] The rest is the same as in Example 3, except that: the preparation method of this comparative example first mixes lithium iron phosphate material and lithium-rich manganese-based material and then sintersects them to obtain an intermediate material, and then mixes the intermediate material with a carbon source and calcines it to obtain the cathode material.
[0146] Comparative Example 10
[0147] The rest is the same as in Example 3, except that the lithium-rich manganese-based material used in this comparative example has the chemical formula LiNi. 0.8 Mn 1.2 O2 has a relative molecular mass of 153 g / mol.
[0148] Comparative Example 11
[0149] The rest is the same as in Example 3, except that the lithium-rich manganese-based material used in this comparative example has the chemical formula LiNi. 0.5 Mn 1.5 O4 has a relative molecular mass of 184 g / mol.
[0150] Test case
[0151] A lithium-ion battery was prepared by combining the positive electrode sheet made from the positive electrode material obtained in Examples 1-10 and Comparative Examples 1-11 with a negative electrode sheet.
[0152] The lithium-ion batteries prepared above were tested as follows:
[0153] 1. Clamp the button cell battery in the battery testing cabinet.
[0154] 2. Adjust the test steps (voltage range 2-4.8V, test 0.1C cycle 3 times and 1C cycle 100 times), select the charge / discharge capacity and the number of cycles.
[0155] 3. Click Start
[0156] Table 1 Electrochemical performance of batteries in examples and comparative examples
[0157]
[0158]
[0159]
[0160] From the above test data, it can be seen that, compared with Comparative Example 1, the smaller particle size of lithium iron phosphate in Example 3 makes it difficult to distinguish the inner and outer layers of the mixed material, resulting in a non-uniquely determined electron transport direction and a decrease in the material's discharge specific capacity. Compared with Comparative Example 2, the larger particle size of lithium iron phosphate in Example 3 leads to a lack of the lithium-rich manganese-based material required for coating, preventing complete coating of lithium iron phosphate and reducing the material's cycle performance. Compared with Comparative Example 3, the smaller particle size of the lithium-rich manganese-based material results in a lack of the required lithium-rich manganese-based material for coating, preventing complete coating of lithium iron phosphate and reducing the material's cycle performance. Compared with Comparative Example 4, the larger particle size of the lithium-rich manganese-based material reduces the material's discharge specific capacity and deteriorates its electrical performance. Compared with Comparative Example 5, the particle sizes of both lithium iron phosphate and lithium-rich manganese-based materials are smaller than the specified range, leading to a decrease in material compaction density and substandard physical properties. Compared with Comparative Example 6, the smaller particle size of lithium iron phosphate material and the larger particle size of lithium-rich manganese-based material easily leads to... The unstable lithium-ion transport direction in the material leads to a deterioration in the battery's discharge capacity and cycle performance. A comparison of Example 3 and Comparative Example 7 shows that when the particle size of the lithium iron phosphate material is larger than the specified range and the particle size of the lithium-rich manganese-based material is smaller than the specified range, the unstable lithium-ion transport direction in the material easily leads to a deterioration in the battery's discharge capacity and cycle performance. A comparison of Example 3 and Comparative Example 8 shows that when the lithium particle size of the lithium iron phosphate material and the lithium-rich manganese-based material are larger than the specified range, the discharge capacity of the material decreases, and the electrical performance deteriorates. A comparison of Example 3 and Comparative Example 8 shows that the cathode material prepared by two-step sintering easily forms carbon agglomerates, resulting in poor coating effect and poor material conductivity. A comparison of Example 3 and Comparative Examples 10 and 11 shows that the proportion of elements in the lithium-rich manganese-based material significantly affects the first-cycle efficiency of the cathode material. Furthermore, when the mass content of the lithium iron phosphate material and the lithium-rich manganese-based material exceeds the specified range, the voltage plateau becomes unstable, and the maximum discharge capacity of the mixed material cannot be utilized during the charge and discharge process, ultimately resulting in poor battery performance.
[0161] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a positive electrode material, characterized in that, It includes the following steps: (1) Add lithium iron phosphate material and lithium-rich manganese-based material to a dry mixing granulator and mix them by vortex stirring to obtain a mixture; The vortex mixer has a rotation speed of 1500 rpm-1800 rpm and a revolution speed of 300 rpm-500 rpm; the D50 of the lithium iron phosphate material is above 1 μm and below 2 μm, and the D50 of the lithium-rich manganese-based material is above 0.1 μm and below 0.2 μm. The lithium-rich manganese-based material has a chemical formula of Li x Ni y Mn z O2, wherein 1.5 > x > 1.2, 0.3 > y > 0.1, and 0.8 > z > 0.
2. (2) The mixture is heat-treated to obtain the positive electrode material.
2. The method for preparing the cathode material according to claim 1, characterized in that: The heat treatment temperature is above 300℃ and below 500℃, and the heat treatment time is above 4h and below 7h.
3. The method for preparing the cathode material according to claim 1, characterized in that, The preparation method further includes: adding a carbon source to form a carbon-containing coating on the surface of the cathode material.
4. The method for preparing the cathode material according to claim 3, characterized in that: The carbon source is an organic carbon source.
5. A positive electrode material, characterized in that, The cathode material is prepared by the cathode material preparation method as described in claim 1; In the cathode material, the lithium iron phosphate material accounts for more than 60% and less than 85% by mass, and the lithium-rich manganese-based material accounts for more than 15% and less than 40% by mass.
6. The cathode material according to claim 5, characterized in that: The preparation method further includes: adding a carbon source during the preparation of the cathode material; the cathode material further includes a coating material located on at least a portion of the surface of the outer layer material, the coating material containing carbon.
7. A positive electrode sheet, characterized in that, It uses the positive electrode material as described in claim 5 or 6 as the positive electrode active material.
8. A battery, characterized in that: The battery includes the positive electrode as described in claim 7.
Citation Information
Patent Citations
Lithium manganese iron phosphate-lithium-rich manganese-based composite positive electrode material, preparation method and application