Mg and Ti ion composite doped lithium iron phosphate positive electrode material, lithium battery as well as preparation method and application of lithium battery
Through the composite doping of Mg and Ti ions to modify the lithium iron phosphate positive electrode material, the problem of poor magnification and low-temperature performance of lithium iron phosphate materials in lithium batteries is solved, the lithium ion mobility and electronic conductivity are improved, and the material efficiency is achieved Cycling performance and low cost production.
Patent Information
- Application Number
- CN202411234451.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
Due to the low lithium ion mobility and electronic conductivity of lithium iron phosphate, lithium batteries have poor rate performance and low temperature performance, which cannot meet the requirements of high rate and low temperature resistance.
Through the composite doping of Mg and Ti ions to modify the lithium iron phosphate positive electrode material, the electron conductivity and lithium ion migration rate are improved, structural stability is enhanced, and the high-energy ball mill grinding and sintering process is adopted, combined with carbon source material for coating, to improve the material cyclicity and conductivity.
The electrochemical performance of lithium iron phosphate positive electrode material is significantly improved, the diffusion stability and electronic conductivity of lithium ions are enhanced, the magnification and low-temperature performance are improved, the preparation process is simplified, energy consumption is saved, and production costs are reduced.
Smart Images

Figure CN118929614A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a Mg and Ti ion composite doped lithium iron phosphate positive electrode material, a lithium battery, and a preparation method and application thereof. Background Art
[0002] Lithium iron phosphate cathode materials have the advantages of good safety performance, long cycle life, wide source of raw materials, and low price, and have broad market prospects in the fields of electric vehicles and smart grids. However, lithium iron phosphate materials have poor electronic and ionic conductivity and low lithium ion migration rate, resulting in poor low temperature and rate performance, which seriously restricts the development of lithium iron phosphate materials. To solve this problem, people have done a lot of research work in the aspects of lithium iron phosphate material structure optimization, surface coating and doping modification, and have made certain progress, making the application of lithium iron phosphate materials move towards a wider field.
[0003] At present, the modified lithium iron phosphate material still cannot meet the performance requirements of lithium iron phosphate positive electrode materials and lithium batteries. Its low lithium ion mobility and conductivity seriously affect the rate performance and low temperature performance of the battery, and cannot meet the requirements of high rate and low temperature resistant lithium iron phosphate system batteries. Therefore, the research and development of new methods and technologies for modifying lithium iron phosphate materials is the focus and difficulty of current research on lithium iron phosphate positive electrode materials. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a Mg and Ti ion composite doped lithium iron phosphate positive electrode material, a lithium battery and a preparation method and application thereof, which increases the structural stability of lithium iron phosphate by composite doping with Mg ions and Ti ions, improves its lithium ion mobility and electronic conductivity, and improves the cyclability of the material. The preparation method is simple and saves energy. The present invention can effectively solve the technical problem that the existing lithium iron phosphate positive electrode material has low lithium ion mobility and electronic conductivity, resulting in poor rate performance and low temperature performance of lithium batteries.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0006] A technical solution of the present invention provides a method for preparing a lithium iron phosphate positive electrode material composite doped with Mg and Ti ions, comprising the following steps:
[0007] (1) mixing a lithium salt, a phosphorus source and an iron source material, grinding them in a high-energy ball mill, and then sintering them under nitrogen protection to obtain a lithium iron phosphate precursor material;
[0008] (2) The lithium iron phosphate precursor material is mixed with a magnesium source material, a titanium source material and a carbon source material, and anhydrous ethanol is used as a dispersion medium. The mixture is placed in a high-energy ball mill for grinding, and then sintered under nitrogen protection. After cooling to room temperature, the mixture is sieved with a molecular sieve to obtain a powdered Mg and Ti ion composite doped lithium iron phosphate positive electrode material.
[0009] In the above technical solution, the modified lithium iron phosphate cathode material is modified by composite doping with Mg and Ti ions, which is beneficial to improving the electronic conductivity, lithium ion migration rate, structural stability and cyclicity of lithium iron phosphate. Due to the presence of Mg and Ti composite ions, the column effect of Ti-O bonds and Mg ions in the preparation process of the material enhances the stability of the lithium iron phosphate structure, which can further reduce the surface side reactions between the material and the electrolyte. The stability of the structure provides a guarantee for the lithium ion channel and transmission stability, which is beneficial to the diffusion of lithium ions, and also increases the number of movable electrons, improves the electronic conductivity of lithium iron phosphate, and thus improves the electrochemical performance of the lithium iron phosphate cathode material.
[0010] In some possible implementations, the lithium salt is lithium carbonate or lithium hydroxide; the iron source and phosphorus source materials are a mixture of diammonium phosphate and ferrous oxalate dihydrate or ferric phosphate.
[0011] Preferably, the lithium salt is lithium carbonate (Li2CO3), the iron source material is ammonium dihydrogen phosphate (NH4H2PO4), and the phosphorus source material is ferrous oxalate dihydrate (FeC2O4·2H2O).
[0012] In some possible implementations, the lithium salt, iron source and phosphorus source materials are lithium carbonate, diammonium phosphate and ferrous oxalate dihydrate, respectively, and the mass ratio of lithium carbonate, diammonium phosphate and ferrous oxalate dihydrate is 3:2:1.
[0013] In some possible implementations, the grinding time in step (1) is 4 to 6 hours, the sintering temperature is 400 to 600° C., and the sintering time is 5 to 8 hours. Exemplarily, the grinding time in step (1) is 4 hours, 4.5 hours, 5 hours or 6 hours, the sintering temperature is 400° C., 500° C. or 600° C., and the sintering time is 5 hours, 6 hours, 7 hours or 8 hours.
[0014] Preferably, in step (1), the grinding time is 4.5 hours, the sintering temperature is 600° C., and the sintering time is 8 hours.
[0015] In some possible implementations, in step (2), the magnesium source material is magnesium acetate tetrahydrate (Mg(CH3COO)2·4H2O); the titanium source material is tetrabutyl titanate (C 16 H 36O4Ti); the carbon source material is sucrose or glucose. Preferably, the carbon source material is sucrose (C 12 H 22 O 11 ), the role of sucrose is to coat the carbon and enhance the conductivity of the material.
[0016] In some possible implementations, in step (2), 95 to 99 parts of precursor material, 1 to 5 parts of magnesium acetate tetrahydrate, 1 to 5 parts of tetrabutyl titanate, and 0.5 to 1 part of sucrose are added by mass.
[0017] Exemplarily, in the step (2), 95 parts of precursor material, 5 parts of magnesium acetate tetrahydrate, 5 parts of tetrabutyl titanate, and 1 part of sucrose are added, by mass; or 96 parts of precursor material, 4 parts of magnesium acetate tetrahydrate, 4 parts of tetrabutyl titanate, and 1 part of sucrose; or 97 parts of precursor material, 3 parts of magnesium acetate tetrahydrate, 3 parts of tetrabutyl titanate, and 1 part of sucrose; or 98 parts of precursor material, 2 parts of magnesium acetate tetrahydrate, 2 parts of tetrabutyl titanate, and 1 part of sucrose; or 99 parts of precursor material, 1 part of magnesium acetate tetrahydrate, 1 part of tetrabutyl titanate, and 1 part of sucrose; or 99 parts of precursor material, 1 part of magnesium acetate tetrahydrate, 1 part of tetrabutyl titanate, and 0.5 part of sucrose.
[0018] In some possible implementations, the mass ratio of magnesium acetate tetrahydrate to tetrabutyl titanate is 1:1.
[0019] In some possible implementations, the grinding time in step (2) is 4 to 6 hours, the sintering temperature is 600 to 800° C., and the sintering time is 10 to 12 hours. Exemplarily, the grinding time in step (2) is 4 hours, 4.5 hours, 5 hours or 6 hours, the sintering temperature is 600° C., 700° C., 750° C. or 800° C., and the sintering time is 10 hours, 10.5 hours, 11 hours or 12 hours.
[0020] Preferably, in step (2), the grinding time is 4 hours, the sintering temperature is 750° C., and the sintering time is 10.5 hours.
[0021] In some possible implementations, the molecular sieve is 200-300 mesh molecular sieve, preferably 300 mesh molecular sieve.
[0022] Another technical solution of the present invention provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the method described in any of the above technical solutions, wherein the chemical formula of the Mg and Ti ion composite doped lithium iron phosphate positive electrode material is (Li x Mg y )(Fe x Ti y)PO4 / C, where 0.95 ≤ x < 1 and 0 < y ≤ 0.05. Exemplarily, the chemical formula of the Mg, Ti ion composite doped lithium iron phosphate cathode material is (Li 0.99 Mg 0.01 )(Fe 0.99 Ti 0.01 )PO4 / C or (Li 0.98 Mg 0.02 )(Fe 0.98 Ti 0.02 )PO4 / C or (Li 0.97 Mg 0.03 )(Fe 0.97 Ti 0.03 )PO4 / C or (Li 0.96 Mg 0.04 )(Fe 0.96 Ti 0.04 )PO4 / C or (Li 0.95 Mg 0.05 )(Fe 0.95 Ti 0.05 )PO4 / C. The D50 particle size of the Mg, Ti ion composite doped lithium iron phosphate cathode material is 1.2 ± 0.15 μm.
[0023] The present invention also provides a positive electrode sheet, which comprises the Mg, Ti ion composite doped lithium iron phosphate cathode material prepared by the method described in any one of the above technical solutions, or the Mg, Ti ion composite doped lithium iron phosphate cathode material described in any one of the above solutions.
[0024] The present invention also provides a method for preparing a positive electrode sheet as described in the above solution, comprising the following steps: mixing the Mg, Ti ion composite doped lithium iron phosphate cathode material, conductive carbon black, and binder polyvinylidene fluoride (PVDF) according to a mass ratio of 93:3:4, using N-methylpyrrolidone (NMP) as a solvent, modulating into a slurry, uniformly coating the surface of the aluminum foil, drying, and then roll-pressing into the required thickness by a roll press to obtain the positive electrode sheet.
[0025] The present invention also provides the application of the Mg, Ti ion composite doped lithium iron phosphate cathode material prepared by the preparation method described in any one of the above technical solutions, or the Mg, Ti ion composite doped lithium iron phosphate cathode material described in any one of the above technical solutions, or the positive electrode sheet described in any one of the above technical solutions, or the positive electrode sheet prepared by the preparation method described in any one of the above technical solutions in a lithium ion battery.
[0026] The present invention also provides a button-type lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet adopts the positive electrode sheet described in any of the above technical solutions or the positive electrode sheet prepared by the preparation method described in any of the above technical solutions. The negative electrode sheet adopts a metal lithium sheet, the separator adopts a Celgard 2400 polypropylene porous membrane, and the electrolyte adopts a LiPF6 / (EC+DEC+DMC) mixed solution with a concentration of 1 mol / L, and the volume ratio of EC, DEC and DMC is 1:1:1.
[0027] The present invention has the following beneficial effects:
[0028] The present invention prepares a lithium iron phosphate positive electrode material doped with Mg ions and Ti ions by a high-temperature solid phase method, and replaces Li in situ and Fe in situ in the lithium iron phosphate material by regulating the content of Mg ions and Ti ions, which is beneficial to improving the structural stability of the lithium iron phosphate material, improving its electronic conductivity and lithium ion mobility, and improving the cycle performance of the material. The preparation method provided by the present invention is simple, the production process is easy to control, energy consumption is saved, the production cost is low, and it is convenient for large-scale production and promotion in the later stage. The lithium iron phosphate positive electrode material doped with Mg ions and Ti ions provided by the present invention is applied to button batteries, which proves that the positive electrode material after doping has a significant improvement in the first effect, capacity and cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0030] Figure 1 It is a flow chart of the preparation process of the lithium iron phosphate positive electrode material composite doped with Mg and Ti ions in the present invention;
[0031] Figure 2 (a) is a particle size distribution diagram of the lithium iron phosphate positive electrode material doped with Mg and Ti ions in Example 3, and (b) is a particle size distribution diagram of the LiFePO4 / C material in the comparative example;
[0032] Figure 3 (a) is a SEM photograph of the lithium iron phosphate positive electrode material doped with Mg and Ti ions in Example 3, and (b) is a SEM photograph of the LiFePO4 / C material in the comparative example;
[0033] Figure 4 It is a 0.1C charge and discharge curve diagram of button-type half-cells in Examples 1 to 5 of the present invention and the comparative example. DETAILED DESCRIPTION
[0034] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, it does not mean that the features of this invention are limited to the implementation.
[0035] The low electronic conductivity and lithium ion migration rate of lithium iron phosphate materials lead to poor low temperature and rate performance, which cannot meet the requirements of high rate and low temperature resistant lithium iron phosphate system batteries, seriously restricting the development of lithium iron phosphate materials. 1-x-y Co x Mn y O2) shows that composite ion doping is an effective method to improve the performance of electrode materials. Therefore, the present invention provides a lithium iron phosphate material modified by composite doping with Mg and Ti ions.
[0036] The present invention provides a method for preparing a lithium iron phosphate positive electrode material compositely doped with Mg and Ti ions, comprising the following steps:
[0037] (1) lithium salt, phosphorus source and iron source materials are weighed and mixed in a mass ratio of 3:2:1, and the mixture is placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4 to 6 hours, and then sintered at 400 to 600° C. for 5 to 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which is cooled and set aside for later use;
[0038] (2) Weigh 95-99 parts of lithium iron phosphate precursor material, 1-5 parts of magnesium source material, 1-5 parts of titanium source material and 0.5-1 part of carbon source material by mass, mix them evenly, use anhydrous ethanol as a dispersion medium, place them in a high-energy ball mill with zirconium oxide beads and grind them for 4-6 hours, then sinter them at 600-800° C. for 10-12 hours under nitrogen protection, cool them to room temperature in the furnace, and sieve out uniform powder with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material.
[0039] The grinding speed of the ball mill can be controlled at 200-600 r / min.
[0040] The above-mentioned lithium salt is lithium carbonate or lithium hydroxide, preferably lithium carbonate; the iron source and phosphorus source materials are a mixture of ammonium dihydrogen phosphate and ferrous oxalate dihydrate or ferric phosphate, the iron source material is preferably ammonium dihydrogen phosphate, and the phosphorus source material is preferably ferrous oxalate dihydrate; the carbon source material is sucrose or glucose, preferably sucrose; the magnesium source material is magnesium acetate tetrahydrate; and the titanium source material is tetrabutyl titanate.
[0041] The present invention also provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the above method, the chemical formula of which is (Lix Mg y )(Fe x Ti y )PO4 / C, where 0.95≤x<1, 0 <y≤0.05。
[0042] The present invention also provides a positive electrode plate, comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material or the Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the above-mentioned method.
[0043] The present invention also provides a method for preparing the above-mentioned positive electrode sheet, comprising the following steps: mixing Mg and Ti ion composite doped lithium iron phosphate positive electrode material, conductive carbon black, and adhesive polyvinylidene fluoride (PVDF) in a mass ratio of 93:3:4, using N-methylpyrrolidone (NMP) as a solvent, preparing a slurry and evenly coating it on the surface of an aluminum foil, drying it at 120°C for 12 hours, and rolling it into a thickness of 90 to 200 μm using a roller press after drying to obtain the desired positive electrode sheet.
[0044] The present invention also provides a button-type lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet adopts the positive electrode sheet or the positive electrode sheet prepared by the above method, the negative electrode sheet adopts a metal lithium sheet, the separator adopts a Celgard 2400 polypropylene porous membrane, and the electrolyte adopts a LiPF6 / (EC+DEC+DMC) mixed solution with a concentration of 1 mol / L, and the volume ratio of EC, DEC and DMC is 1:1:1, and is assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere).
[0045] To make the purpose, technical scheme and advantages of the present invention clearer, the embodiments of the present invention will be described in further detail below in conjunction with the accompanying drawings. In the following examples, unless otherwise specified, the raw materials used are all common commercial products, and the reagents are analytically pure reagents.
[0046] Example 1
[0047] This embodiment provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.99 Mg 0.01 )(Fe 0.99 Ti 0.01 )PO4 / C, and provides a method for preparing the positive electrode material, comprising the following steps:
[0048] (1) lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate were weighed and mixed in a mass ratio of 3:2:1, and the mixture was placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4.5 hours, and then sintered at 600° C. for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which was cooled and used for later use;
[0049] (2) 99 parts of lithium iron phosphate precursor material, 1 part of magnesium acetate tetrahydrate, 1 part of tetrabutyl titanate and 1 part of sucrose were weighed by mass, and the lithium iron phosphate precursor material was mixed with magnesium acetate tetrahydrate, tetrabutyl titanate and sucrose, and anhydrous ethanol was used as a dispersion medium. The mixture was placed in a high-energy ball mill containing zirconium oxide beads and ground and stirred for 4 hours. The mixture was then sintered at 750° C. for 10.5 hours under nitrogen protection. After cooling to room temperature with the furnace, a uniform powder was sieved out with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.99 Mg 0.01 )(Fe 0.99 Ti 0.01 )PO4 / C.
[0050] This embodiment further provides a positive electrode sheet comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material, and provides a method for preparing the positive electrode sheet, comprising the following steps:
[0051] Will (Li 0.99 Mg 0.01 )(Fe 0.99 Ti 0.01 )PO4 / C, conductive carbon black, and binder PVDF are mixed in a mass ratio of 93:3:4, and NMP is used as a solvent. The slurry is evenly coated on the surface of the aluminum foil and dried at 120°C for 12 hours. After drying, a roller press is used to press the slurry into the desired thickness to obtain the desired positive electrode sheet.
[0052] This embodiment also provides the use of the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material and positive electrode plate in lithium ion batteries.
[0053] This embodiment also provides a button-type half-cell, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet is the positive electrode sheet of this embodiment, the negative electrode sheet is a metal lithium sheet, the separator is a Celgard2400 polypropylene porous membrane, and the electrolyte is a mixed solution of LiPF6 / (EC+DEC+DMC) with a concentration of 1 mol / L. The volume ratio of EC, DEC and DMC is 1:1:1. The above materials are assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere). The assembled button-type half-cell was subjected to charge and discharge tests at room temperature and a rate of 0.1C. The test results are shown in Tables 1 and Figure 4 shown.
[0054] Example 2
[0055] This embodiment provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.98 Mg 0.02 )(Fe0.98 Ti 0.02 )PO4 / C, and provides a method for preparing the positive electrode material, comprising the following steps:
[0056] (1) lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate were weighed and mixed in a mass ratio of 3:2:1, and the mixture was placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4.5 hours, and then sintered at 600° C. for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which was cooled and used for later use;
[0057] (2) 98 parts of lithium iron phosphate precursor material, 2 parts of magnesium acetate tetrahydrate, 2 parts of tetrabutyl titanate and 1 part of sucrose were weighed by mass, and the lithium iron phosphate precursor material was mixed with magnesium acetate tetrahydrate, tetrabutyl titanate and sucrose, and anhydrous ethanol was used as a dispersion medium. The mixture was placed in a high-energy ball mill containing zirconium oxide beads and ground and stirred for 4 hours. The mixture was then sintered at 750° C. for 10.5 hours under nitrogen protection. After cooling to room temperature with the furnace, a uniform powder was sieved out with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.98 Mg 0.02 )(Fe 0.98 Ti 0.02 )PO4 / C.
[0058] This embodiment further provides a positive electrode sheet comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material, and provides a method for preparing the positive electrode sheet, comprising the following steps:
[0059] Will (Li 0.98 Mg 0.02 )(Fe 0.98 Ti 0.02 )PO4 / C, conductive carbon black, and binder PVDF are mixed in a mass ratio of 93:3:4, and NMP is used as a solvent. The slurry is evenly coated on the surface of the aluminum foil and dried at 120°C for 12 hours. After drying, a roller press is used to press the slurry into the desired thickness to obtain the desired positive electrode sheet.
[0060] This embodiment also provides the use of the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material and positive electrode plate in lithium ion batteries.
[0061] This embodiment also provides a button-type half-cell, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet is the positive electrode sheet of this embodiment, the negative electrode sheet is a metal lithium sheet, the separator is a Celgard2400 polypropylene porous membrane, and the electrolyte is a mixed solution of LiPF6 / (EC+DEC+DMC) with a concentration of 1 mol / L. The volume ratio of EC, DEC and DMC is 1:1:1. The above materials are assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere). The assembled button-type half-cell was subjected to charge and discharge tests at room temperature and a rate of 0.1C. The test results are shown in Tables 1 and Figure 4 shown.
[0062] Example 3
[0063] This embodiment provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.97 Mg 0.03 )(Fe 0.97 Ti 0.03 )PO4 / C, and provides a method for preparing the positive electrode material, comprising the following steps:
[0064] (1) lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate were weighed and mixed in a mass ratio of 3:2:1, and the mixture was placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4.5 hours, and then sintered at 600° C. for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which was cooled and used for later use;
[0065] (2) 97 parts of lithium iron phosphate precursor material, 3 parts of magnesium acetate tetrahydrate, 3 parts of tetrabutyl titanate and 1 part of sucrose were weighed by mass, and the lithium iron phosphate precursor material was mixed with magnesium acetate tetrahydrate, tetrabutyl titanate and sucrose, and anhydrous ethanol was used as a dispersion medium. The mixture was placed in a high-energy ball mill containing zirconium oxide beads and ground and stirred for 4 hours. The mixture was then sintered at 750° C. for 10.5 hours under nitrogen protection. After cooling to room temperature with the furnace, a uniform powder was sieved out with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.97 Mg 0.03 )(Fe 0.97 Ti 0.03 )PO4 / C.
[0066] This embodiment further provides a positive electrode sheet comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material, and provides a method for preparing the positive electrode sheet, comprising the following steps:
[0067] Will (Li 0.97 Mg 0.03 )(Fe 0.97 Ti 0.03)PO4 / C, conductive carbon black, and binder PVDF are mixed in a mass ratio of 93:3:4, and NMP is used as a solvent. The slurry is evenly coated on the surface of the aluminum foil and dried at 120°C for 12 hours. After drying, a roller press is used to press the slurry into the desired thickness to obtain the desired positive electrode sheet.
[0068] This embodiment also provides the use of the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material and positive electrode plate in lithium ion batteries.
[0069] This embodiment also provides a button-type half-cell, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet is the positive electrode sheet of this embodiment, the negative electrode sheet is a metal lithium sheet, the separator is a Celgard2400 polypropylene porous membrane, and the electrolyte is a mixed solution of LiPF6 / (EC+DEC+DMC) with a concentration of 1 mol / L. The volume ratio of EC, DEC and DMC is 1:1:1. The above materials are assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere). The assembled button-type half-cell was subjected to charge and discharge tests at room temperature and a rate of 0.1C. The test results are shown in Tables 1 and Figure 4 shown.
[0070] Example 4
[0071] This embodiment provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.96 Mg 0.04 )(Fe 0.96 Ti 0.04 )PO4 / C, and provides a method for preparing the positive electrode material, comprising the following steps:
[0072] (1) lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate were weighed and mixed in a mass ratio of 3:2:1, and the mixture was placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4.5 hours, and then sintered at 600° C. for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which was cooled and used for later use;
[0073] (2) 96 parts of lithium iron phosphate precursor material, 4 parts of magnesium acetate tetrahydrate, 4 parts of tetrabutyl titanate and 1 part of sucrose were weighed by mass, and the lithium iron phosphate precursor material was mixed with magnesium acetate tetrahydrate, tetrabutyl titanate and sucrose, and anhydrous ethanol was used as a dispersion medium. The mixture was placed in a high-energy ball mill containing zirconium oxide beads and ground and stirred for 4 hours. The mixture was then sintered at 750° C. for 10.5 hours under nitrogen protection. After cooling to room temperature with the furnace, a uniform powder was sieved out with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.96 Mg 0.04 )(Fe 0.96 Ti 0.04)PO4 / C.
[0074] This embodiment further provides a positive electrode sheet comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material, and provides a method for preparing the positive electrode sheet, comprising the following steps:
[0075] Will (Li 0.96 Mg 0.04 )(Fe 0.96 Ti 0.04 )PO4 / C, conductive carbon black, and binder PVDF are mixed in a mass ratio of 93:3:4, and NMP is used as a solvent. The slurry is evenly coated on the surface of the aluminum foil and dried at 120°C for 12 hours. After drying, a roller press is used to press the slurry into the desired thickness to obtain the desired positive electrode sheet.
[0076] This embodiment also provides the use of the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material and positive electrode plate in lithium ion batteries.
[0077] This embodiment also provides a button-type half-cell, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet is the positive electrode sheet of this embodiment, the negative electrode sheet is a metal lithium sheet, the separator is a Celgard2400 polypropylene porous membrane, and the electrolyte is a mixed solution of LiPF6 / (EC+DEC+DMC) with a concentration of 1 mol / L. The volume ratio of EC, DEC and DMC is 1:1:1. The above materials are assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere). The assembled button-type half-cell was subjected to charge and discharge tests at room temperature and a rate of 0.1C. The test results are shown in Tables 1 and Figure 4 shown.
[0078] Example 5
[0079] This embodiment provides a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.95 Mg 0.05 )(Fe 0.95 Ti 0.05 )PO4 / C, and provides a method for preparing the positive electrode material, comprising the following steps:
[0080] (1) lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate were weighed and mixed in a mass ratio of 3:2:1, and the mixture was placed in a high-energy ball mill containing zirconium oxide beads for grinding for 4.5 hours, and then sintered at 600° C. for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material, which was cooled and used for later use;
[0081] (2) 95 parts of lithium iron phosphate precursor material, 5 parts of magnesium acetate tetrahydrate, 5 parts of tetrabutyl titanate and 1 part of sucrose were weighed by mass, and the lithium iron phosphate precursor material was mixed with magnesium acetate tetrahydrate, tetrabutyl titanate and sucrose, and anhydrous ethanol was used as a dispersion medium. The mixture was placed in a high-energy ball mill containing zirconium oxide beads and ground and stirred for 4 hours, and then sintered at 750°C for 10.5 hours under nitrogen protection. After cooling to room temperature with the furnace, a uniform powder was sieved out with a 300-mesh molecular sieve to obtain a Mg and Ti ion composite doped lithium iron phosphate positive electrode material (Li 0.95 Mg 0.05 )(Fe 0.95 Ti 0.05 )PO4 / C.
[0082] This embodiment further provides a positive electrode sheet comprising the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material, and provides a method for preparing the positive electrode sheet, comprising the following steps:
[0083] Will (Li 0.95 Mg 0.05 )(Fe 0.95 Ti 0.05 )PO4 / C, conductive carbon black, and binder PVDF are mixed in a mass ratio of 93:3:4, and NMP is used as a solvent. The slurry is evenly coated on the surface of the aluminum foil and dried at 120°C for 12 hours. After drying, a roller press is used to press the slurry into the desired thickness to obtain the desired positive electrode sheet.
[0084] This embodiment also provides the use of the above-mentioned Mg and Ti ion composite doped lithium iron phosphate positive electrode material and positive electrode plate in lithium ion batteries.
[0085] This embodiment also provides a button-type half-cell, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet is the positive electrode sheet of this embodiment, the negative electrode sheet is a metal lithium sheet, the separator is a Celgard2400 polypropylene porous membrane, and the electrolyte is a mixed solution of LiPF6 / (EC+DEC+DMC) with a concentration of 1 mol / L. The volume ratio of EC, DEC and DMC is 1:1:1. The above materials are assembled into a CR 2025 button-type half-cell in a glove box (high-purity Ar atmosphere). The assembled button-type half-cell was subjected to charge and discharge tests at room temperature and a rate of 0.1C. The test results are shown in Tables 1 and Figure 4 shown.
[0086] Comparative Example
[0087] In this comparative example, an undoped LiFePO4 / C powder is provided. The preparation method of the positive electrode material is as follows: lithium salt, phosphorus source and iron source materials are weighed and mixed in a mass ratio of 3:2:1, and the mixture is placed in a high-energy ball mill containing zirconium oxide beads and ground for 4.5 hours, and then sintered at 600°C for 8 hours under nitrogen protection to obtain a powdered lithium iron phosphate precursor material. After cooling to room temperature with the furnace, a uniform powder is sieved out with a 300-mesh molecular sieve to obtain an undoped lithium iron phosphate positive electrode material LiFePO4 / C powder.
[0088] The method for preparing the positive electrode sheet using the LiFePO4 / C powder in this comparative example is as follows:
[0089] LiFePO4 / C powder, conductive carbon black and binder PVDF were mixed in a mass ratio of 93:3:4, prepared into slurry using NMP as solvent and evenly coated on the surface of aluminum foil, dried at 120°C for 12 hours, and rolled into the required thickness using a roller press to obtain the required positive electrode sheet.
[0090] Further, the positive electrode sheet was used to make a button half-cell, the positive electrode sheet was used and a metal lithium sheet was used as a negative electrode sheet, a Celgard 2400 polypropylene porous membrane was used as a separator, and a LiPF6 / (EC+DEC+DMC) mixed solution with a concentration of 1 mol / L was used as the electrolyte, and the volume ratio of EC, DEC, and DMC was 1:1:1. The above materials were assembled into a CR 2025 button half-cell in a glove box (high-purity Ar atmosphere). The assembled button half-cell was charged and discharged at room temperature and a rate of 0.1C, and the test results are shown in Table 1.
[0091] Table 1. Test data of button-type half-cell at 0.1C rate charge and discharge in the present invention
[0092]
[0093] Analysis of the data in Table 1 shows that, compared with the comparative example, the lithium iron phosphate positive electrode materials modified by composite doping of Mg ions and Ti ions in Examples 1 to 5 of the present invention can improve the electronic conductivity and ion migration rate of the positive electrode materials, and can significantly improve the initial efficiency, capacity and cycle performance of lithium batteries when applied to lithium batteries. Figure 4 It can be seen from the test data of Examples 1 to 5 in Table 1 that with the increase of the doping content of Mg ions and Ti ions, the battery's 0.1C first discharge specific capacity, coulombic efficiency and capacity retention rate after multiple cycles all show a trend of first increasing and then decreasing, but each performance is still better than the undoped modified lithium iron phosphate positive electrode material in the comparative example. The lithium iron phosphate positive electrode material modified by the doping content of Mg and Ti ions in Example 3 can be preferably used in lithium batteries.
[0094] The particle size and powder morphology of the Mg and Ti ion composite doped lithium iron phosphate positive electrode material of Example 3 and the LiFePO4 / C powder of the comparative example were tested by a particle size analyzer and a scanning electron microscope. Figure 2 and Figure 3 It can be seen that compared with the comparative example, the average particle size of the powder material of the Mg and Ti ion composite doped lithium iron phosphate positive electrode material provided by the present invention does not change much after composite doping modification, and the powder particle size is more uniform and stable, has good dispersibility, and is not easy to agglomerate.
[0095] Although the preferred embodiments of the present invention have been disclosed as above, they are not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solutions of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the contents of the technical solutions of the present invention shall fall within the protection scope of the technical solutions of the present invention.
Claims
1. A method for preparing a Mg and Ti ion composite doped lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: (1) mixing a lithium salt, a phosphorus source and an iron source material, grinding them in a high-energy ball mill, and then sintering them under nitrogen protection to obtain a lithium iron phosphate precursor material; (2) The lithium iron phosphate precursor material is mixed with a magnesium source material, a titanium source material and a carbon source material, and anhydrous ethanol is used as a dispersion medium. The mixture is placed in a high-energy ball mill for grinding, and then sintered under nitrogen protection. After cooling to room temperature, the mixture is sieved with a molecular sieve to obtain a powdered Mg and Ti ion composite doped lithium iron phosphate positive electrode material.
2. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step (1), the lithium salt is lithium carbonate or lithium hydroxide; the iron source and phosphorus source materials are a mixture of ammonium dihydrogen phosphate and ferrous oxalate dihydrate or ferric phosphate.
3. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 2, characterized in that: The lithium salt, iron source and phosphorus source materials are lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate respectively, and the mass ratio of lithium carbonate, ammonium dihydrogen phosphate and ferrous oxalate dihydrate is 3:2:
1.
4. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the grinding time is 4 to 6 hours, the sintering temperature is 400 to 600° C., and the sintering time is 5 to 8 hours.
5. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step (2), the magnesium source material is magnesium acetate tetrahydrate; the titanium source material is tetrabutyl titanate; and the carbon source material is sucrose or glucose.
6. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 5, characterized in that: In the step (2), 95 to 99 parts of precursor material, 1 to 5 parts of magnesium acetate tetrahydrate, 1 to 5 parts of tetrabutyl titanate, and 0.5 to 1 part of sucrose are added by weight.
7. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 6, characterized in that: The mass ratio of the magnesium acetate tetrahydrate to tetrabutyl titanate is 1:
1.
8. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (2), the grinding time is 4 to 6 hours, the sintering temperature is 600 to 800° C., and the sintering time is 10 to 12 hours.
9. The method for preparing the Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 1, characterized in that: The molecular sieve is a 200-300 mesh molecular sieve.
10. A Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the method according to any one of claims 1 to 9, characterized in that: The chemical formula of the Mg and Ti ion composite doped lithium iron phosphate positive electrode material is (Li x Mg y )(Fe x Ti y )PO4 / C, where 0.95≤x<1, 0 <y≤0.05。 11. A positive electrode sheet, characterized in that: It comprises a Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the method according to any one of claims 1 to 9, or a Mg and Ti ion composite doped lithium iron phosphate positive electrode material according to claim 10.
12. A method for preparing a positive electrode sheet as claimed in claim 11, characterized in that: The method comprises the following steps: mixing Mg and Ti ion composite doped lithium iron phosphate positive electrode material, conductive carbon black and adhesive polyvinylidene fluoride in a mass ratio of 93:3:4, using N-methylpyrrolidone as a solvent, preparing the slurry and uniformly coating the slurry on the surface of aluminum foil, and rolling the slurry into a desired thickness after drying to obtain the positive electrode sheet.
13. Use of a Mg and Ti ion composite doped lithium iron phosphate positive electrode material prepared by the preparation method as described in any one of claims 1 to 9, or a Mg and Ti ion composite doped lithium iron phosphate positive electrode material as described in claim 10, or a positive electrode sheet as described in claim 11, or a positive electrode sheet prepared by the preparation method as described in claim 12 in a lithium ion battery.
14. A button-type lithium-ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet is the positive electrode sheet as claimed in claim 11 or the positive electrode sheet prepared by the preparation method as claimed in claim 12.
Citation Information
Patent Citations
Preparation method of lithium iron phosphate precursor with high electrical property
CN118026122A
Cited By
Lithium iron phosphate positive electrode material with low interface impedance, preparation method of lithium iron phosphate positive electrode material and lithium battery
CN120600797A
Lithium iron phosphate positive electrode material with low interfacial impedance, preparation method thereof and lithium battery
CN120600797B
Nanometer spherical lithium iron phosphate material as well as preparation method and application thereof
CN120793877A
Manufacturing process of lithium iron phosphate energy storage battery
CN121123420A
Preparation method of high-compaction high-capacity lithium iron phosphate
CN122704872A