Display panel, manufacturing method thereof and display device

By combining dry and wet etching, the side slope of the source and drain layers is controlled to form a positive trapezoidal structure, which solves the problem of breakage or wire breakage during film layer overlap in the display panel and improves the quality and electrical performance of the display panel.

CN117476671BActive Publication Date: 2026-11-10GUANGZHOU CHINA STAR OPTOELECTRONICS SEMICON DISPLAY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310268921.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-12-30
Filing Date
2023-03-17
Publication Date
2026-11-10
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

In the manufacturing process of display panels, the overlapping process between the source/drain electrode layer and the upper film layer can easily lead to film layer breakage or wire breakage, resulting in electrical abnormalities and affecting the quality of the display panel.

Method used

The first protective layer and the conductive layer are patterned by combining dry etching and wet etching. The side slope of the source and drain layers is controlled to form a trapezoidal cross-section of the source and drain layers, ensuring that the orthogonal projection of the first protective layer on the substrate does not exceed the orthogonal projection of the conductive layer.

Benefits of technology

This reduces the risk of breakage or wire breakage when the source/drain electrode layer overlaps with the upper film layer, improving the quality and electrical performance of the display panel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117476671B_ABST
    Figure CN117476671B_ABST
Patent Text Reader

Abstract

Embodiments of the present application disclose a display panel, a manufacturing method thereof and a display device. The display panel comprises a substrate, an active layer and a source-drain layer on the surface of the active layer. The source-drain layer comprises at least a first protective layer and a conductive layer. The orthogonal projection of the first protective layer on the substrate is not more than the orthogonal projection of the conductive layer on the substrate. The angle corresponding to the slope of the corresponding side of any film layer in the source-drain layer is 50° to 60°. The first protective layer and the conductive layer are patterned by dry etching and wet etching respectively. The damage of the conductive layer by dry etching is small, and the side slope of the source-drain layer can be easily controlled. The side slope of the source-drain layer is appropriately reduced to form a structure in which the cross section of the film layer of the source-drain layer is a right trapezoid. The orthogonal projection of the first protective layer on the substrate is not more than the orthogonal projection of the conductive layer on the substrate, which avoids the shrinkage of the conductive layer and reduces the risk of fracture or disconnection of the overlapping film layer of the source-drain layer, thereby improving the quality of the display panel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of displays, specifically to a display panel and its manufacturing method, and a display device. Background Technology

[0002] In recent years, the consumer market has placed increasingly higher demands on the quality of display panels. During the manufacturing process, when patterning the source and drain layers, the etching rates of the acid solution on the conductive layer and the first protective layer of the source and drain layers are different. This can easily lead to the conductive layer shrinking or the side slope of the source and drain layers being too large. When the source and drain layers overlap with the upper film layer, the upper film layer is prone to breakage or wire breakage, resulting in electrical abnormalities and reducing the quality of the display panel.

[0003] Therefore, there is an urgent need for a display panel, its manufacturing method, and a display device to solve the above-mentioned technical problems. Summary of the Invention

[0004] This application provides a display panel and its manufacturing method, as well as a display device, which can alleviate the technical problem that the upper film layer is prone to breakage or wire breakage when the source and drain electrode layers are overlapped with the upper film layer, resulting in abnormal electrical properties.

[0005] This application provides a display panel, including:

[0006] Substrate;

[0007] An active layer is disposed on one side of the substrate;

[0008] A source / drain layer is disposed on the surface of the active layer away from the substrate, and the source / drain layer includes at least a first protective layer and a conductive layer located between the first protective layer and the active layer;

[0009] Wherein, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, the orthographic projection of the surface of the conductive layer away from the substrate on the substrate is within the orthographic projection of the surface of the conductive layer close to the substrate on the substrate, the orthographic projection of the surface of the first protective layer away from the substrate on the substrate is within the orthographic projection of the surface of the first protective layer close to the substrate on the substrate, and the slope angle corresponding to the corresponding side of any film layer in the source and drain layers is 50° to 60°.

[0010] In some embodiments, in any two adjacent film layers of the source and drain layers, the outer contour of the surface of the film layer away from the substrate on the side closest to the substrate coincides with the outer contour of the surface of the film layer close to the substrate on the side away from the substrate; the slopes of the corresponding sides of any two adjacent film layers of the source and drain layers are the same.

[0011] In some embodiments, in any two adjacent film layers of the source and drain layers, the orthographic projection of the surface of the film layer away from the substrate on the side closest to the substrate onto the substrate lies within the orthographic projection of the surface of the film layer away from the substrate on the side closest to the substrate onto the substrate.

[0012] In some embodiments, the slope of the corresponding side of the first protective layer is greater than the slope of the corresponding side of the conductive layer.

[0013] In some embodiments, the active layer is made of metal oxide, and the display panel further includes a gate layer located on the side of the active layer near the substrate; the source and drain layers further include a second protective layer located between the conductive layer and the active layer.

[0014] In some embodiments, the slope of the corresponding side of the conductive layer is greater than the slope of the corresponding side of the second protective layer.

[0015] In some embodiments, the slope of the corresponding side of the first protective layer is greater than the slope of the corresponding side of the conductive layer, and the slope of the corresponding side of the conductive layer is greater than the slope of the corresponding side of the second protective layer.

[0016] This application also provides a method for manufacturing a display panel, including:

[0017] Provide a substrate;

[0018] An active layer is formed on one side of the substrate;

[0019] At least a conductive material layer and a first protective material layer are formed on the side of the active layer away from the substrate.

[0020] The first protective material layer is patterned using dry etching to form the first protective layer;

[0021] The conductive material layer is patterned using wet etching to form a conductive layer;

[0022] Wherein, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, the orthographic projection of the surface of the conductive layer away from the substrate on the substrate is within the orthographic projection of the surface of the conductive layer close to the substrate on the substrate, the orthographic projection of the surface of the first protective layer away from the substrate on the substrate is within the orthographic projection of the surface of the first protective layer close to the substrate on the substrate, and the slope angle corresponding to the corresponding side of any film layer in the source and drain layers is 50° to 60°.

[0023] In some embodiments, the active layer is made of metal oxide, and the step of forming at least a conductive material layer and a first protective material layer on the surface of the active layer away from the substrate and on the surface of the conductive material layer away from the substrate includes: sequentially forming a second protective material layer, a conductive material layer, and a first protective material layer on the surface of the active layer away from the substrate; after the step of patterning the conductive material layer using wet etching to form a conductive layer, the step further includes: patterning the second protective material layer using dry etching to form a second protective layer, wherein the orthographic projection of the conductive layer on the substrate is located within the orthographic projection of the second protective layer on the substrate.

[0024] This application also provides a display device, including a display panel as described in any of the above.

[0025] Beneficial effects of this application: This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source and drain layers. By appropriately reducing the side slope of the source and drain layers, a trapezoidal structure is formed in the cross-section of the source and drain layers. Furthermore, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, thus avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or disconnection of the overlapping film layer with the source and drain layers, thereby improving the quality of the display panel. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a schematic diagram of the structure of the display panel provided in an embodiment of this application;

[0028] Figure 2 yes Figure 1 The first type of magnified view of region A;

[0029] Figure 3 yes Figure 1 The second type of magnified view of region A;

[0030] Figure 4 yes Figure 1 The third type of magnified view of region A;

[0031] Figure 5 yes Figure 1 The fourth enlarged view of region A;

[0032] Figure 6 yes Figure 1 The fifth type of magnified view of region A;

[0033] Figure 7 This is a flowchart of the steps in the method for manufacturing a display panel provided in an embodiment of this application;

[0034] Figures 8A to 8D This is a flowchart illustrating the method for manufacturing a display panel according to an embodiment of this application;

[0035] Figure 9 This is a schematic diagram of the structure of the display device provided in the embodiments of this application. Detailed Implementation

[0036] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application. In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in actual use or operation, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device.

[0037] In recent years, the consumer market has placed increasingly higher demands on the quality of display panels. During the manufacturing process, when patterning the source and drain layers, the etching rates of the acid solution on the conductive layer and the first protective layer of the source and drain layers are different. This can easily lead to the conductive layer shrinking or the side slope of the source and drain layers being too large. When the source and drain layers overlap with the upper film layer, the upper film layer is prone to breakage or wire breakage, resulting in electrical abnormalities and reducing the quality of the display panel.

[0038] Please see Figures 1 to 6 This application provides a display panel 100, including:

[0039] Substrate 200;

[0040] An active layer 300 is disposed on one side of the substrate 200;

[0041] A source / drain layer 400 is disposed on the surface of the active layer 300 away from the substrate 200. The source / drain layer 400 includes at least a first protective layer 410 and a conductive layer 420 located between the first protective layer 410 and the active layer 300.

[0042] Wherein, the orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200, the orthographic projection of the surface of the conductive layer 420 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the conductive layer 420 on the side close to the substrate 200 on the substrate 200, the orthographic projection of the surface of the first protective layer 410 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the first protective layer 410 on the side close to the substrate 200 on the substrate 200, and the slope of the corresponding side of any film layer in the source and drain layers corresponds to an angle of 50° to 60°.

[0043] This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer, respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source and drain layers. By appropriately reducing the side slope of the source and drain layers, a trapezoidal structure is formed in the cross-section of the source and drain layers. Furthermore, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, thus avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or wire breakage of the overlapping film layer with the source and drain layers, thereby improving the quality of the display panel.

[0044] The technical solution of this application will now be described in conjunction with specific embodiments.

[0045] In this embodiment, please refer to Figure 1 , Figure 2 The display panel 100 includes a substrate 200, an active layer 300 disposed on one side of the substrate 200, and a source / drain layer 400 disposed on the surface of the active layer 300 away from the substrate 200. The source / drain layer 400 includes at least a first protective layer 410 and a conductive layer 420 located between the first protective layer 410 and the active layer 300. The orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200. The orthographic projection of the surface of the conductive layer 420 away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the conductive layer 420 near the substrate 200 on the substrate 200. The orthographic projection of the surface of the first protective layer 410 away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the first protective layer 410 near the substrate 200 on the substrate 200.

[0046] Generally, the patterning of the source / drain layer 400 is a single patterning process, such as wet etching using acid etching solution. The etching rate of the acid on the conductive layer 420 is greater than that on the first protective layer 410, which easily leads to the width of the conductive layer 420 being smaller than the width of the first protective layer 410, or the slope of the side of the source / drain layer 400 being too large. In subsequent film layers, such as pixel electrodes and insulating layers, breakage or broken lines are easily generated at the junction of the conductive layer 420 and the first protective layer 410 or at the side of the source / drain layer 400. However, dry etching is used to pattern the first protective layer 410, and then... Wet etching patterns the conductive layer 420, while dry etching causes less damage to the conductive layer 420 and makes it easier to control the side slope of the source / drain layer 400. By appropriately reducing the side slope of the source / drain layer 400, a trapezoidal structure is formed in the cross-section of the film layer 400. The orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200. The upper film layer does not protrude from the lower film layer, avoiding the inward shrinkage of the conductive layer 420. The trapezoidal structure reduces the risk of breakage or wire breakage of the overlapping film layer with the source / drain layer 400, thus improving the quality of the display panel 100.

[0047] In some embodiments, the slope of the corresponding side of any of the source and drain layers 400 corresponds to an angle of 50° to 60°.

[0048] The slope of the corresponding side of any film layer in the source / drain layer 400 should not be too large, as this will increase the risk of breakage or wire breakage of the overlapping film layer with the source / drain layer 400; the slope of the corresponding side of any film layer in the source / drain layer 400 should not be too small, as this will result in the source / drain layer 400 occupying too much space and the channel of the active layer 300 being too narrow.

[0049] In some embodiments, optionally, the slope of the corresponding side of any film layer in the source / drain layer 400 corresponds to an angle such as 50°, 52°, 54°, 55°, 56°, 58°, 60° or a non-integer angle.

[0050] In some embodiments, please refer to Figure 2 , Figure 3 In any two adjacent film layers in the source / drain layer 400, the outer contour of the surface of the film layer away from the substrate 200 on the side closest to the substrate 200 coincides with the outer contour of the surface of the film layer close to the substrate 200 on the side away from the substrate 200; the slopes of the corresponding sides of any two adjacent film layers in the source / drain layer 400 are the same.

[0051] The sides of the film layers in the source and drain layers 400 are on the same plane, which can reduce the difficulty of covering the upper film layers on the sides, reduce the risk of film layer breakage or fracture, and improve the quality of the display panel 100.

[0052] In some embodiments, please refer to Figure 4 , Figure 5 , Figure 6 In any two adjacent film layers of the source / drain layer 400, the orthographic projection of the surface of the film layer away from the substrate 200 on the side closer to the substrate 200 onto the substrate 200 lies within the orthographic projection of the surface of the film layer away from the substrate 200 on the side closer to the substrate 200 onto the substrate 200.

[0053] In any two adjacent film layers of the source / drain layer 400, the orthographic projection of the upper film layer is located within the orthographic projection of the lower film layer, which avoids the upper film layer shrinking inward, reduces the risk of breakage or wire breakage of the overlapping film layer with the source / drain layer, and improves the quality of the display panel.

[0054] In some embodiments, please refer to Figure 4 , Figure 5 , Figure 6 In any two adjacent film layers of the source / drain layer 400, the area of ​​the surface of the film layer away from the substrate 200 on the side closer to the substrate 200 is smaller than the area of ​​the surface of the film layer closer to the substrate 200 on the side away from the substrate 200.

[0055] In any two adjacent film layers of the source / drain layer 400, the upper film layer and the lower film layer form an upward step, thereby increasing the contact area between the upper film layer of the source / drain layer 400 and the source / drain layer 400. For example, it increases the contact area between the pixel electrode layer 270 and the source / drain layer 400, thereby strengthening the connection stability between the pixel electrode layer 270 and the source / drain layer 400 and improving electrical performance.

[0056] In some embodiments, please refer to Figure 3 , Figure 5 The slope of the corresponding side of the first protective layer 410 is greater than the slope of the corresponding side of the conductive layer 420.

[0057] The overlap between the pixel electrode layer 270 and the source / drain layer 400 extends from the upper portion of the film layer of the source / drain layer 400 to the side of the lower portion of the film layer of the source / drain layer 400. This reduces the slope of the lower portion of the film layer of the source / drain layer 400, making the slope of the conductive layer 420 located below the first protective layer 410 gentler. This helps reduce the difficulty of covering the pixel electrode layer 270 on the side of the conductive layer 420, reduces the risk of film layer breakage or fracture, and improves the quality of the display panel 100. In the figure, for ease of understanding and comparison of slope changes, the slope of the side is shown as an illustrative angle.

[0058] In some embodiments, please refer to Figure 1 , Figure 2The active layer 300 is made of metal oxide, and the display panel 100 further includes a gate layer 210 located on the side of the active layer 300 near the substrate 200; the source-drain layer 400 further includes a second protective layer 430 located between the conductive layer 420 and the active layer 300.

[0059] When the active layer 300 is made of metal oxide, the channel area of ​​the active layer 300 needs to be protected. When the second protective layer 430 is formed, a second protective material layer 431 is formed first, followed by the formation of the first protective layer 410 and the conductive layer 420. Then, the second protective material layer 431 is patterned to form the second protective layer 430. Therefore, the second protective layer 430 can protect the channel area of ​​the active layer 300, prevent damage to the channel of the active layer 300, and improve the quality of the display panel 100.

[0060] In some embodiments, please refer to Figure 3 , Figure 5 The slope of the corresponding side of the conductive layer 420 is greater than the slope of the corresponding side of the second protective layer 430.

[0061] The slope of the corresponding side of the conductive layer 420 is greater than the slope of the corresponding side of the second protective layer 430. Reducing the slope of the lower part of the source / drain layer 400 helps to reduce the difficulty of covering the upper film layer on the side, reduces the risk of film layer breakage or fracture at the junction of the pixel electrode layer 270 and the source / drain layer 400, and improves the quality of the display panel 100. In the figure, for ease of understanding and comparison of slope changes, the slope of the side is shown as an illustrative angle.

[0062] In some embodiments, please refer to Figure 3 , Figure 5 For example, the source / drain layer 400 further includes a second protective layer 430 located between the conductive layer 420 and the active layer 300. The slope of the corresponding side of the first protective layer 410 is greater than the slope of the corresponding side of the conductive layer 420, and the slope of the corresponding side of the conductive layer 420 is greater than the slope of the corresponding side of the second protective layer 430. Reducing the slope of the lower portion of the film layer of the source / drain layer 400 helps to reduce the difficulty of covering the upper film layer at the side, reduces the risk of film layer breakage or fracture at the junction of the pixel electrode layer 270 and the source / drain layer 400, and improves the quality of the display panel 100. In the figure, for ease of understanding and comparison of slope changes, the slope of the side is an illustrative angle.

[0063] In some embodiments, if the entire source / drain layer 400 is etched using an acidic etching solution, the width of the bottom of the second protective layer 430 will be smaller than the width of the top of the second protective layer 430, which may easily lead to breakage of the upper film layer of the source / drain layer 400; see also Figure 3 By using dry etching to form the second protective layer 430, a trapezoidal cross-section structure can be formed, reducing the risk of film breakage or fracture and improving the quality of the display panel 100.

[0064] In some embodiments, the materials of the first protective layer 410, the conductive layer 420, and the second protective layer 430 can be any one of Mo alloy / Cu / Mo alloy, Mo / Cu / Mo, and Ti / Cu / Ti, where " / " indicates layering. For example, Ti / Cu / Ti indicates that the materials of the first protective layer 410, the conductive layer 420, and the second protective layer 430 are Ti, Cu, and Ti in sequence. The Mo alloy / Cu / Mo alloy can be MoTi / Cu / MoTi, which is only an example and not a specific limitation.

[0065] In some embodiments, please refer to Figure 1 The gate layer 210 includes a gate, which can serve as a bottom gate to form a BCE structure (back channel etched structure).

[0066] In some embodiments, the active layer 300 may include metal oxide materials such as indium zinc oxide (IZO), indium gallium oxide (IGO), indium gallium zinc oxide (IGZO), indium gallium tin oxide (IGTO), indium tin zinc oxide (ITZO), or single or multi-element metal oxides composed of indium (In), gallium (Ga), zinc (Zn), tin (Sn), aluminum (Al), tungsten (W), zirconium (Zr), hafnium (Hf), and silicon (Si).

[0067] In some embodiments, please refer to Figure 6 The distance between the outer contour of the bottom surface of the first protective layer 410 and the outer contour of the top surface of the conductive layer 420 is less than the distance between the outer contour of the bottom surface of the conductive layer 420 and the outer contour of the top surface of the second protective layer 430.

[0068] For example, the overlap between the pixel electrode layer 270 and the source / drain layer 400 is mainly in the upper part of the film layer of the source / drain layer 400. This can reduce the difficulty of covering the upper film layer at the step, reduce the risk of film layer breakage or fracture, and improve the quality of the display panel 100.

[0069] In some embodiments, the gate layer 210 may also serve as a top gate structure.

[0070] In some embodiments, the active layer 300 is made of monocrystalline silicon and / or polycrystalline silicon, and the display panel 100 further includes a gate layer 210 located on the side of the active layer 300 near the substrate 200; the source-drain layer 400 includes the first protective layer 410 and the conductive layer 420.

[0071] The active layer 300 is made of monocrystalline silicon and / or polycrystalline silicon. The active layer 300 has strong etching resistance and does not require a second protective layer 430 for protection. However, providing a second protective layer 430 is also acceptable and will not be elaborated further here.

[0072] In some embodiments, please refer to Figure 1 Taking the display panel 100 as a liquid crystal display panel 100 as an example, the display panel 100 includes a substrate 200, a gate layer 210 located on the substrate 200, a first insulating layer 220 located on the gate layer 210, an active layer 300 located on the first insulating layer 220, a source / drain layer 400 located on the active layer 300, a second insulating layer 230 located on the source / drain layer 400, a planarization layer 240 located on the second insulating layer 230, a common electrode layer 250 located on the planarization layer 240, a third insulating layer 260 located on the common electrode layer 250, a pixel electrode layer 270 located on the third insulating layer 260, a liquid crystal layer 280 located on the pixel electrode layer 270, and a color filter layer 290 located on the liquid crystal layer 280.

[0073] In some embodiments, this application can be used in FFS (edge ​​field switching) technology, which generates an edge electric field through inter-pixel electrodes in the same plane, so that the oriented liquid crystal molecules between the electrodes and directly above the electrodes can rotate and switch in a plane parallel to the substrate, thereby improving the light transmission efficiency of the liquid crystal layer.

[0074] In some embodiments, please refer to Figure 1 Taking a back channel structure as an example, with the gate layer 210 as a bottom gate structure, the gate layer 210 can also be used as a wiring layer. The display panel 100 also includes a first common electrode wiring layer 211 disposed on the same layer as the gate layer 210.

[0075] In some embodiments, please refer to Figure 1 The display panel 100 also includes a connection line layer 401 disposed on the same layer as the source-drain layer 400.

[0076] In some embodiments, please refer to Figure 1 The display panel 100 also includes a second common electrode trace layer 271 disposed on the same layer as the pixel electrode layer 270.

[0077] In some embodiments, please refer to Figure 1 The second common electrode routing layer 271 is electrically connected to the common electrode layer 250 and the connecting line layer 401 through a via, and the connecting line layer 401 is electrically connected to the first common electrode routing layer 211 through a via.

[0078] In some embodiments, please refer to Figure 1 The pixel electrode layer 270 is electrically connected to the source / drain layer 400 through a via.

[0079] In some embodiments, the substrate 200 may be made of a rigid material, such as glass, or a flexible material, such as polyimide, without specific limitation.

[0080] This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer, respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source and drain layers. By appropriately reducing the side slope of the source and drain layers, a trapezoidal structure is formed in the cross-section of the source and drain layers. Furthermore, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, thus avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or wire breakage of the overlapping film layer with the source and drain layers, thereby improving the quality of the display panel.

[0081] Please see Figure 7 This application embodiment also provides a method for manufacturing a display panel 100, including:

[0082] S100, providing a substrate 200;

[0083] S200, An active layer 300 is formed on one side of the substrate 200;

[0084] S300, at least a conductive material layer 421 and a first protective material layer 411 are formed on the side of the active layer 300 away from the substrate 200.

[0085] S400. Using dry etching, the first protective material layer 411 is patterned to form the first protective layer 410.

[0086] S500: The conductive material layer 421 is patterned using wet etching to form a conductive layer 420.

[0087] Wherein, the orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200, the orthographic projection of the surface of the conductive layer 420 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the conductive layer 420 on the side close to the substrate 200 on the substrate 200, the orthographic projection of the surface of the first protective layer 410 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the first protective layer 410 on the side close to the substrate 200 on the substrate 200, and the slope of the corresponding side of any film layer in the source and drain layers corresponds to an angle of 50° to 60°.

[0088] This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer, respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source and drain layers. By appropriately reducing the side slope of the source and drain layers, a trapezoidal structure is formed in the cross-section of the source and drain layers. Furthermore, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, thus avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or wire breakage of the overlapping film layer with the source and drain layers, thereby improving the quality of the display panel.

[0089] The technical solution of this application will now be described in conjunction with specific embodiments.

[0090] In this embodiment, the method for manufacturing the display panel 100 includes:

[0091] S100, provides a substrate 200, please refer to... Figure 8A .

[0092] In some embodiments, the substrate 200 may be made of a rigid material, such as glass, or a flexible material, such as polyimide, without specific limitation.

[0093] In some embodiments, the display panel 100 has a bottom-gate back channel structure, and step S100 includes:

[0094] S110, Provide a substrate 200, please refer to... Figure 8A .

[0095] S120, A gate layer 210 is formed on the substrate 200. (See below) Figure 8A .

[0096] S130, A first insulating layer 220 is formed on the gate layer 210. (See below) Figure 8A .

[0097] In some embodiments, please refer to Figure 1Taking a back channel structure as an example, with the gate layer 210 as a bottom gate structure, the gate layer 210 can also be used as a wiring layer. The display panel 100 also includes a first common electrode wiring layer 211 disposed on the same layer as the gate layer 210.

[0098] S200, An active layer 300 is formed on one side of the substrate 200. (See also...) Figure 8A .

[0099] In some embodiments, the active layer 300 comprises a metal oxide. The metal oxide material comprising the active layer 300 may include indium zinc oxide (IZO), indium gallium oxide (IGO), indium gallium zinc oxide (IGZO), indium gallium tin oxide (IGTO), indium tin zinc oxide (ITZO), or a single or multi-element metal oxide composed of indium (In), gallium (Ga), zinc (Zn), tin (Sn), aluminum (Al), tungsten (W), zirconium (Zr), hafnium (Hf), and silicon (Si).

[0100] In some embodiments, the active layer 300 comprises monocrystalline silicon and / or polycrystalline silicon.

[0101] S300, at least a conductive material layer 421 and a first protective material layer 411 are formed on the side of the active layer 300 away from the substrate 200. Please refer to [link to previous section]. Figure 8A .

[0102] In some embodiments, the display panel 100 has a bottom-gate back channel structure, and step S300 includes:

[0103] S310, a second protective material layer 431, a conductive material layer 421, and a first protective material layer 411 are sequentially formed on the surface of the active layer 300 on the side away from the substrate 200. Please refer to [link to previous section]. Figure 8A .

[0104] S400. Using dry etching, the first protective material layer 411 is patterned to form the first protective layer 410. Please refer to [link to relevant documentation]. Figure 8B .

[0105] In some embodiments, the process gas for dry etching is primarily an inert gas, such as argon.

[0106] S500. Using wet etching, the conductive material layer 421 is patterned to form the conductive layer 420. Please refer to [link to relevant documentation]. Figure 8C .

[0107] In some embodiments, the etching solution for wet etching is an acid solution corresponding to the conductive material layer 421. For example, if the conductive layer 420 is copper, then the etching solution is copper acid.

[0108] In some embodiments, please refer to Figure 1 , Figure 2 , Figure 3 , Figure 4 The orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200. The orthographic projection of the surface of the conductive layer 420 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the conductive layer 420 on the side close to the substrate 200 on the substrate 200. The orthographic projection of the surface of the first protective layer 410 on the side away from the substrate 200 on the substrate 200 is located within the orthographic projection of the surface of the first protective layer 410 on the side close to the substrate 200 on the substrate 200.

[0109] Generally, the patterning of the source / drain layer 400 is a single patterning process, such as wet etching using acid etching solution. The etching rate of the acid on the conductive layer 420 is greater than that on the first protective layer 410, which easily leads to the width of the conductive layer 420 being smaller than the width of the first protective layer 410, or the slope of the side of the source / drain layer 400 being too large. In subsequent film layers, such as pixel electrodes and insulating layers, breakage or broken lines are easily generated at the junction of the conductive layer 420 and the first protective layer 410 or at the side of the source / drain layer 400. However, dry etching is used to pattern the first protective layer 410, and then... Wet etching patterns the conductive layer 420, while dry etching causes less damage to the conductive layer 420 and makes it easier to control the side slope of the source / drain layer 400. By appropriately reducing the side slope of the source / drain layer 400, a trapezoidal structure is formed in the cross-section of the film layer 400. The orthographic projection of the first protective layer 410 on the substrate 200 does not exceed the orthographic projection of the conductive layer 420 on the substrate 200. The upper film layer does not protrude from the lower film layer, avoiding the inward shrinkage of the conductive layer 420. The trapezoidal structure reduces the risk of breakage or wire breakage of the overlapping film layer with the source / drain layer 400, thus improving the quality of the display panel 100.

[0110] In some embodiments, the slope of the corresponding side of any of the source and drain layers 400 corresponds to an angle of 50° to 60°.

[0111] The slope of the corresponding side of any membrane layer in the source / drain layer 400 should not be too large, as this will increase the risk of breakage or wire breakage of the membrane layer overlapping with the source / drain layer 400; the slope of the corresponding side of any membrane layer in the source / drain layer 400 should not be too small, as this will result in the source / drain layer 400 occupying too much space and the channel of the active layer 300 being too narrow.

[0112] In some embodiments, the method of manufacturing the display panel 100 further includes:

[0113] S600. Using dry etching, the second protective material layer 431 is patterned to form the second protective layer 430, wherein the orthographic projection of the conductive layer on the substrate lies within the orthographic projection of the second protective layer on the substrate. Please refer to [link to relevant documentation]. Figure 8D .

[0114] In some embodiments, the process gas for dry etching is primarily an inert gas, such as argon.

[0115] In some embodiments, if the source-drain layer 400 is etched entirely with an acidic etching solution, the width of the bottom of the second protective layer 430 will be smaller than the width of the top of the second protective layer 430, which may easily lead to the breakage of the upper film layer of the source-drain layer 400; however, by using dry etching to etch the second protective layer 430, a structure with a regular trapezoidal cross section can be formed, reducing the risk of film layer breakage or fracture and improving the quality of the display panel 100.

[0116] In some embodiments, the materials of the first protective layer 410, the conductive layer 420, and the second protective layer 430 can be any one of Mo alloy / Cu / Mo alloy, Mo / Cu / Mo, and Ti / Cu / Ti, where " / " indicates layering. For example, Ti / Cu / Ti indicates that the materials of the first protective layer 410, the conductive layer 420, and the second protective layer 430 are Ti, Cu, and Ti in sequence. The Mo alloy / Cu / Mo alloy can be MoTi / Cu / MoTi, which is only an example and not a specific limitation.

[0117] In some embodiments, please refer to Figure 1 Taking a liquid crystal display panel 100 as an example, the display panel 100 includes a substrate 200, a gate layer 210 on the substrate 200, a first insulating layer 220 on the gate layer 210, an active layer 300 on the first insulating layer 220, a source / drain layer 400 on the active layer 300, a second insulating layer 230 on the source / drain layer 400, a planarization layer 240 on the second insulating layer, a common electrode layer 250 on the planarization layer 240, a third insulating layer 260 on the common electrode layer 250, a pixel electrode layer 270 on the third insulating layer 260, a liquid crystal layer 280 on the pixel electrode layer 270, and a color filter layer 290 on the liquid crystal layer 280. The fabrication processes of the above layers are easy to understand and will not be described in detail.

[0118] This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer, respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source and drain layers. By appropriately reducing the side slope of the source and drain layers, a trapezoidal structure is formed in the cross-section of the source and drain layers. Furthermore, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, thus avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or wire breakage of the overlapping film layer with the source and drain layers, thereby improving the quality of the display panel.

[0119] Please see Figure 9 The present invention also provides a display device 10, including a display panel 100 as described above.

[0120] For the specific structure of the display panel 100, please refer to any of the above-described embodiments of the display panel 100 and the accompanying drawings, which will not be repeated here.

[0121] In some embodiments, please refer to Figure 9 The display device also includes a device body 20, which is integrated with the display panel 100.

[0122] In this embodiment, the main body 20 of the device may include a middle frame, frame adhesive, etc., and the display device 10 may be a mobile phone, tablet, TV, giant screen, or other display terminal, which is not limited here.

[0123] This application discloses a display panel and its manufacturing method and display device. The display panel includes a substrate, an active layer, and a source / drain layer on the surface of the active layer. The source / drain layer includes at least a first protective layer and a conductive layer. The orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate. The slope angle of the corresponding side of any film layer in the source / drain layer is 50° to 60°. This application uses dry etching and wet etching to pattern the first protective layer and the conductive layer, respectively. Dry etching causes less damage to the conductive layer and makes it easier to control the side slope of the source / drain layer. By appropriately reducing the side slope of the source / drain layer, a trapezoidal structure is formed in the cross-section of the film layer of the source / drain layer. The orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, avoiding the inward shrinkage of the conductive layer and reducing the risk of breakage or wire breakage of the overlapping film layer with the source / drain layer, thereby improving the quality of the display panel.

[0124] The above provides a detailed description of a display panel, its manufacturing method, and the display device provided in the embodiments of this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A display panel, characterized in that, include: Substrate; An active layer is disposed on one side of the substrate; A source / drain layer is disposed on the surface of the active layer away from the substrate, and the source / drain layer includes at least a first protective layer and a conductive layer located between the first protective layer and the active layer; Wherein, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, the orthographic projection of the surface of the conductive layer away from the substrate on the substrate is within the orthographic projection of the surface of the conductive layer close to the substrate on the substrate, the orthographic projection of the surface of the first protective layer away from the substrate on the substrate is within the orthographic projection of the surface of the first protective layer close to the substrate on the substrate, and the slope angle corresponding to the corresponding side of any film layer in the source and drain layers is 50° to 60°.

2. The display panel according to claim 1, characterized in that, In any two adjacent film layers of the source and drain layers, the outer contour of the surface of the film layer away from the substrate on the side closest to the substrate coincides with the outer contour of the surface of the film layer close to the substrate on the side away from the substrate. The slope of corresponding sides of any two adjacent film layers in the source and drain layers is the same.

3. The display panel according to claim 1, characterized in that, In any two adjacent film layers of the source and drain layers, the orthographic projection of the surface of the film layer away from the substrate on the substrate is located within the orthographic projection of the surface of the film layer away from the substrate on the substrate.

4. The display panel according to claim 1, characterized in that, The slope of the corresponding side of the first protective layer is greater than the slope of the corresponding side of the conductive layer.

5. The display panel according to any one of claims 1 to 4, characterized in that, The active layer is made of metal oxide, and the display panel further includes a gate layer located on the side of the active layer near the substrate; The source-drain layer further includes a second protective layer located between the conductive layer and the active layer.

6. The display panel according to claim 5, characterized in that, The slope of the corresponding side of the conductive layer is greater than the slope of the corresponding side of the second protective layer.

7. The display panel according to claim 5, characterized in that, The slope of the corresponding side of the first protective layer is greater than the slope of the corresponding side of the conductive layer, and the slope of the corresponding side of the conductive layer is greater than the slope of the corresponding side of the second protective layer.

8. A method for manufacturing a display panel, characterized in that, include: Provide a substrate; An active layer is formed on one side of the substrate; At least a conductive material layer and a first protective material layer are formed on the side of the active layer away from the substrate. The first protective material layer is patterned using dry etching to form the first protective layer; The conductive material layer is patterned using wet etching to form a conductive layer; Wherein, the orthographic projection of the first protective layer on the substrate does not exceed the orthographic projection of the conductive layer on the substrate, the orthographic projection of the surface of the conductive layer away from the substrate on the substrate is within the orthographic projection of the surface of the conductive layer close to the substrate on the substrate, the orthographic projection of the surface of the first protective layer away from the substrate on the substrate is within the orthographic projection of the surface of the first protective layer close to the substrate on the substrate, the source and drain layers include at least the first protective layer and the conductive layer, and the slope of the corresponding side of any film layer in the source and drain layers corresponds to an angle of 50° to 60°.

9. The method for manufacturing a display panel according to claim 8, characterized in that, The active layer is made of metal oxide, and the step of forming at least a conductive material layer and a first protective material layer on the surface of the conductive material layer on the side away from the substrate on the active layer includes: A second protective material layer, a conductive material layer, and a first protective material layer are sequentially formed on the surface of the active layer away from the substrate. The step of patterning the conductive material layer using wet etching to form the conductive layer further includes: The second protective material layer is patterned using dry etching to form a second protective layer, wherein the orthogonal projection of the conductive layer on the substrate lies within the orthogonal projection of the second protective layer on the substrate.

10. A display device, characterized in that, Includes the display panel as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Display panel, preparation method thereof and display device

    CN113658990A

  • Organic light-emitting display apparatus and method of manufacturing the same

    US20170352712A1