A multilayer film reflector and its preparation method

By introducing a ligand layer between the X and Y layers of a multilayer reflector, the strong coordination effect is used to suppress interfacial reactions, thus solving the problem of decreased reflectivity caused by interfacial mixing and achieving high stability and high reflectivity of the reflector.

CN117518321BActive Publication Date: 2026-11-17SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311748343.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-17
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

Existing multilayer mirrors suffer from reduced reflectivity and oxidation damage in short-wavelength applications due to interlayer mixing. Traditional intercalation methods also suffer from reflectivity loss or reduced interface contrast.

Method used

A ligand layer is introduced between the X layer and the Y layer, and an ultrathin molecular layer is formed by magnetron sputtering. The strong coordination between the ligand and the atoms of the X layer is used to suppress interfacial reactions and reduce interfacial roughness and mixing.

Benefits of technology

It significantly improves the reflectivity stability and long-term retention of multilayer film mirrors, reduces the attenuation of actual reflectivity relative to theoretical reflectivity, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004615662100000011
    Figure HDA0004615662100000011
  • Figure HDA0004615662100000012
    Figure HDA0004615662100000012
  • Figure HDA0004615662100000021
    Figure HDA0004615662100000021
Patent Text Reader

Abstract

This invention discloses a multilayer reflector, comprising a substrate, a substrate layer disposed on the substrate, and a multi-period X / ligand / Y layer disposed on the substrate layer; the multi-period X / ligand / Y layer comprises multiple stacked single-period X / ligand / Y layers; the single-period X / ligand / Y layer comprises an X layer, a ligand layer, and a Y layer stacked sequentially; the ligand layer is a compound having one or more groups selected from aldehyde, carbonyl, carboxyl, amino, carbon-carbon double bond, carbon-nitrogen double bond, cyano, azo, and borate groups. This invention utilizes ligands to suppress interfacial mixing in the multilayer reflector, reducing interfacial roughness and improving the reflectivity and long-term stability of the reflector. The process of this invention is simple and compatible with thin-film sputtering processes, making it suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of short-wavelength optical element technology, and relates to a multilayer film reflector and its preparation method. Background Technology

[0002] With the development of integrated circuits, chips are evolving towards lower power consumption and higher performance. Short-wavelength lithography machines, as tools for manufacturing high-end integrated circuits, can etch nanometer-scale chip channels, effectively reducing chip power consumption and improving performance. Therefore, the use of short-wavelength lithography light sources undoubtedly has a greater promoting effect on the development of integrated circuits. However, all materials exhibit strong absorption in the short-wavelength band; therefore, reflective optical systems, which can effectively increase the output power density of the light source, are widely used.

[0003] One of the key components of reflective optical systems is the multilayer mirror. Multilayer mirrors typically consist of a substrate and alternating X and Y layers with thicknesses ranging from nanometers to sub-nanometers. Variations in the thickness and roughness of these nanometer- to sub-nanometer layers significantly impact the reflectivity of short-wavelength multilayer mirrors. Diffusion and compound formation at the multilayer interfaces can severely reduce the reflectivity of short-wavelength mirrors and even cause damage. For example, with boron's K absorption edge at λ = 6.63 nm, the theoretical reflectivity of a La / B multilayer mirror can reach 80%, even higher than that of a Mo / Si multilayer mirror at λ = 13.5 nm. Therefore, La / B multilayer mirrors are considered the most promising material for next-generation extreme ultraviolet lithography. However, in practical applications, interdiffusion inevitably occurs between the layers of a La / B multilayer mirror, forming a certain LaB6 mixed layer. This leads to an increase in the roughness of the multilayer film, reduces the optical contrast of the film, causes a significant decrease in the actual reflectivity of the La / B multilayer film mirror compared to the theoretical reflectivity, and results in problems such as rapid oxidation damage of the multilayer film.

[0004] Currently, the main method for resolving La / B interface mixing is intercalation. For example, LaN or C is used as an interfacial intercalator to isolate the reaction between La and B. However, the preparation of LaN may lead to the formation of BN, further causing a decrease in the interfacial optical contrast. In addition, C intercalation can lead to a certain degree of decrease in reflectivity.

[0005] Therefore, there is still a need in the field for a multilayer reflector capable of suppressing interfacial mixing and its fabrication method. Summary of the Invention

[0006] To address the problems existing in the prior art, this invention provides a multilayer mirror capable of suppressing interfacial mixing and its fabrication method. This invention introduces ligands into the interface (Y-on-X interface) between the X layer and the Y layer located on top of the X layer via magnetron sputtering, utilizing the ligands to suppress interfacial diffusion in the multilayer mirror. The ligands have strong coordination with the X layer atoms, effectively suppressing the possibility of reactions between high-energy Y layer atoms and X layer atoms. Furthermore, the ligands cannot enter the X layer, thereby suppressing interfacial mixing, minimizing interfacial roughness, significantly reducing the decrease in actual reflectivity compared to theoretical reflectivity during mirror application, and improving the reflectivity stability of the mirror during long-term use.

[0007] Specifically, the present invention provides a multilayer film reflector, the reflector comprising a substrate, a substrate layer disposed on the substrate, and a multi-period X / ligand / Y layer disposed on the substrate layer;

[0008] The multi-period X / ligand / Y layer includes multiple stacked single-period X / ligand / Y layers;

[0009] The single-cycle X / ligand / Y layer comprises an X layer, a ligand layer, and a Y layer stacked sequentially.

[0010] The ligand layer is made of a compound having one or more groups selected from aldehyde, carbonyl, carboxyl, amino, carbon-carbon double bond, carbon-nitrogen double bond, cyano, azo, and borate.

[0011] In one or more embodiments, the ligand layer is made of one or more selected from lanthanum borate, urea, 2,4,6,8-tetrahydroxypyrimidin[5,4-d]pyrimidine, 5-aminoorotic acid, and 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene.

[0012] In one or more embodiments, the thickness of the ligand layer is 0.1 to 1 nm.

[0013] In one or more embodiments, the X layer in the single-cycle X / ligand / Y layer closest to the underlayment is in contact with the underlayment.

[0014] In one or more embodiments, the material of the underlayer is B, the material of the X layer is La, and the material of the Y layer is B or a compound of B.

[0015] In one or more embodiments, the material of the base layer is Si, the material of the X layer is Mo, and the material of the Y layer is Si or Be.

[0016] In one or more embodiments, the material of the base layer is C, the material of the X layer is Cr, and the material of the Y layer is C.

[0017] In one or more embodiments, the substrate is a silicon wafer, a quartz wafer, or a glass sheet.

[0018] In one or more embodiments, the roughness of the substrate is 0.1 to 0.2 nm.

[0019] In one or more embodiments, the number of periods in a single-period X / ligand / Y layer in the multi-period X / ligand / Y layer is 50 to 250.

[0020] In one or more embodiments, the thickness of the underlay layer is 1 to 5 nm.

[0021] In one or more embodiments, the thickness of the X layer is 0.5 to 5 nm.

[0022] In one or more embodiments, the thickness of the Y layer is 1 to 5 nm.

[0023] In one or more embodiments, the thickness of the single-cycle X / ligand / Y layer is 1.6 to 11 nm.

[0024] The present invention also provides a method for preparing a multilayer reflector according to any embodiment of the present invention, the method comprising the following steps:

[0025] (1) Prepare the underlayer on the substrate;

[0026] (2) On the substrate, an X layer, a ligand layer and a Y layer are prepared sequentially. The process of preparing the X layer, ligand layer and Y layer sequentially is repeated to obtain a multi-period X / ligand / Y layer.

[0027] In one or more embodiments, the method for preparing the substrate layer is radio frequency magnetron sputtering or DC magnetron sputtering, and the magnetron sputtering parameters for preparing the substrate layer include: a base vacuum degree ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target purity ≥99.5%, working gas is argon, working gas pressure is 0.15~0.25Pa, sputtering power is 100~300W.

[0028] In one or more embodiments, the X layer is prepared by DC magnetron sputtering, and the magnetron sputtering parameters for preparing the X layer include: a background vacuum of ≤1×10⁻⁶. -5 Pa, sputtering method is target grazing, target purity ≥99.5%, working gas is argon, working pressure is 0.15~0.25Pa, sputtering power is 40~120W.

[0029] In one or more embodiments, the ligand layer is prepared by radio frequency magnetron sputtering, and the magnetron sputtering parameters for preparing the ligand layer include: a background vacuum of ≤1×10⁻⁶. -5 Pa, sputtering method is target grazing, target purity ≥99.5%, working gas is argon, working gas pressure is 0.15~0.25Pa, sputtering power is 100~300W.

[0030] In one or more embodiments, the Y-layer is fabricated by radio frequency magnetron sputtering or DC magnetron sputtering, and the magnetron sputtering parameters for fabricating the Y-layer include: a base vacuum degree ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target purity ≥99.5%, working gas is argon, working gas pressure is 0.15~0.25Pa, sputtering power is 100~300W.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) This invention utilizes ligands (e.g., organic molecules) to suppress interfacial mixing in multilayer mirrors. Although traditional methods can also achieve some suppression, LaN itself may be oxidized, and BN may form during the preparation process, or high-energy C atoms may partially react with the La layer, leading to a certain degree of mixing at the interface, resulting in a decrease in interfacial optical contrast and / or reflectivity. In this invention, the ligands have a strong coordination effect with the X-layer atoms, which can effectively suppress the possibility of high-energy Y-layer atoms reacting with X-layer atoms. Furthermore, ligands with a certain molecular size cannot enter the X-layer, thus making it difficult for ligands to mix with the X-layer at the interface, minimizing interfacial roughness, and improving the stability of the mirror's reflectivity in practical applications.

[0033] (2) In this invention, ligands (e.g., organic molecules) can form an ultrathin molecular layer with a thickness of only one to a few layers on the X layer through self-assembly, which is impossible to achieve with conventional sputtering methods. In addition, the ultrathin molecular layer can effectively reduce its absorption of short wavelengths, thereby effectively improving the reflectivity of short-wavelength mirrors.

[0034] (3) In practical applications, the decrease in actual reflectivity compared to theoretical reflectivity of the X / ligand / Y short-wavelength multilayer reflector of the present invention is significantly less than that of conventional X / Y multilayer reflectors. In fact, some reflectors containing ligand layers in the present invention have higher theoretical reflectivity than the control group without ligand layers. This will help maintain a high level of reflectivity in practical engineering applications, thereby improving the stability of key performance indicators of the reflector.

[0035] (4) The process of this invention is relatively simple and compatible with thin film sputtering process, making it suitable for mass production. Attached Figure Description

[0036] Figure 1 This is a schematic diagram of the structure of the multilayer film reflector of the present invention.

[0037] Figure 2 This is a schematic diagram illustrating the principle of suppressing interface mixing in the multilayer film mirror of the present invention in some embodiments.

[0038] Figure 3 The wavelength-theoretical reflectivity curve is shown for the multilayer film reflector of Example 1.

[0039] Figure 4 The wavelength-theoretical reflectivity curve is shown for the multilayer film reflector of Example 2.

[0040] Figure 5 The wavelength-theoretical reflectivity curve is shown for the multilayer film mirror in Comparative Example 1.

[0041] Figure 6 The wavelength-theoretical reflectivity curve is shown for the multilayer film mirror in Comparative Example 2.

[0042] The annotations in the attached figures are explained as follows:

[0043] 1 is the base layer, 2 is the bottom layer, 3 is the multi-cycle X / ligand / Y layer, 31 is the X layer, 32 is the ligand layer, and 33 is the Y layer. Detailed Implementation

[0044] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0046] In this document, the terms “contains,” “includes,” “containing,” and similar terms encompass the meanings of “basically composed of” and “composed of.” For example, when this document discloses “A contains B and C,” “A is basically composed of B and C” and “A is composed of B and C” should be considered as having been disclosed in this document.

[0047] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0048] Unless otherwise specified, percentages refer to mass percentages and proportions refer to mass ratios in this article.

[0049] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples. Rather, all alternatives, modifications, and equivalents of the methods and materials described herein are covered within the scope defined by the claims.

[0050] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0051] The multilayer film reflector of the present invention has a high reflectivity for short wavelength or extreme ultraviolet bands. Therefore, the multilayer film reflector of the present invention is a short wavelength multilayer film reflector or an extreme ultraviolet multilayer film reflector.

[0052] like Figure 1 As shown, the multilayer reflector of the present invention includes a substrate 1, a substrate layer 2 disposed on the substrate, and a multi-period X / ligand / Y layer 3 disposed on the substrate layer. The substrate layer 2 is located between the substrate 1 and the multi-period X / ligand / Y layer 3, with both sides of the substrate layer 2 contacting the substrate 1 and the multi-period X / ligand / Y layer 3, respectively. The multi-period X / ligand / Y layer 3 includes a plurality of stacked single-period X / ligand / Y layers. Each single-period X / ligand / Y layer includes an X layer 31, a ligand layer 32, and a Y layer 33 stacked sequentially. The X layer in the single-period X / ligand / Y layer closest to the substrate layer 2 is in contact with the substrate layer 2. The X layer in each single-period X / ligand / Y layer is in contact with the Y layer in the adjacent single-period X / ligand / Y layer. The Y layer in each single-period X / ligand / Y layer is in contact with the X layer in the adjacent single-period X / ligand / Y layer.

[0053] In some embodiments, the multilayer reflector of the present invention comprises a substrate, a substrate layer disposed on the substrate, and a multi-period X / ligand / Y layer disposed on the substrate layer. In some embodiments, the multi-period X / ligand / Y layer comprises a plurality of stacked single-period X / ligand / Y layers. In some embodiments, the single-period X / ligand / Y layer comprises an X layer, a ligand layer, and a Y layer stacked sequentially.

[0054] In this invention, the ligand layer is made of ligands. In this document, the ligands are capable of coordinating with atoms in the X layer. The groups contained in the ligands include, but are not limited to, one or more selected from aldehyde, carbonyl, carboxyl, amino, carbon-carbon double bond, carbon-nitrogen double bond, cyano, azo, and borate groups.

[0055] In a preferred embodiment, the ligands used in this invention are selected from lanthanum borate (LaBO3) and urea (structural formula: ), 2,4,6,8-tetrahydroxypyrimidine[5,4-d]pyrimidine (structural formula is ), 5-aminoorotic acid (structural formula is) ) and 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene (structural formula is One or more of the compounds referred to as HAT-CN. Through in-depth research, this invention has discovered that the above-mentioned compounds, as ligands, have a strong coordination effect with X-layer atoms, which can particularly effectively suppress the possibility of high-energy Y-layer atoms reacting with X-layer atoms, and the ligands cannot enter the X-layer. Therefore, there is no interface mixing between the ligands and the X-layer, which greatly reduces the interface roughness and significantly improves the long-term stability of the reflectivity of the mirror in practical applications.

[0056] In this invention, the thickness of the ligand layer can be 0.1–1 nm, for example, 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, or 0.9 nm. This invention has found that controlling the thickness of the ligand layer within the aforementioned range can very effectively suppress the possibility of reactions between high-energy Y-layer atoms and X-layer atoms, greatly reduce interface roughness, significantly improve the long-term stability of the reflectivity of the mirror in practical applications, and without causing significant adverse effects on the theoretical reflectivity of the mirror.

[0057] In some embodiments, the ligand is an organic ligand. Organic ligands suitable for use in this invention include, but are not limited to, one or more selected from urea, 2,4,6,8-tetrahydroxypyrimidin[5,4-d]pyrimidine, 5-aminoorotic acid, and 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene.

[0058] like Figure 2 As shown, in some embodiments, the ligand contains one or more groups selected from carbonyl, carboxyl, amino, carbon-carbon double bond, cyano and azo groups. Therefore, the ligand has a strong coordination effect with the high-order atoms in the X layer, which can effectively suppress the possibility of high-energy Y layer atoms reacting with X layer atoms. In addition, ligands of a certain size cannot enter the X layer, so it is difficult for interfacial mixing to occur, thus minimizing interfacial roughness and improving the reflectivity of the mirror.

[0059] The inventors of this invention discovered that when a Y layer is formed on an X layer, interfacial mixing easily occurs at the Y-on-X interface, while when an X layer is formed on a Y layer, interfacial mixing is less likely to occur at the X-on-Y interface. Therefore, this invention provides a ligand layer between the X and Y layers within a single-period X / Y layer to obtain a single-period X / ligand / Y layer. The ligand layer may not be provided between the single-period X / ligand / Y layers (i.e., at the X-on-Y interface).

[0060] In this invention, the material of the underlayer can be the same as or different from the material of the Y layer. In some embodiments, the material of the underlayer is the same as the material of the Y layer. In this invention, the materials of the X layer and the Y layer can be the materials of the X layer and the Y layer in a single-period X / Y layer of a known multilayer mirror (e.g., a short-wavelength soft X-ray multilayer mirror, an extreme ultraviolet multilayer mirror).

[0061] In some embodiments, the underlayer material is B, the X layer material is La, and the Y layer material is B or a compound of B. In some embodiments, the underlayer material is Si, the X layer material is Mo, and the Y layer material is Si or B. In some embodiments, the underlayer material is C, the X layer material is Cr, and the Y layer material is C.

[0062] In some implementations, the base layer is made of material B, the X layer is made of material La, the ligand layer is made of HAT-CN or urea, and the Y layer is made of material B. In these implementations, introducing a ligand layer between the X and Y layers can improve the theoretical reflectivity of the mirror.

[0063] In this invention, the substrate can be a silicon wafer, a quartz wafer, or a glass wafer. The roughness of the substrate can be 0.1 to 0.2 nm, for example, 0.12 nm, 0.14 nm, 0.16 nm, or 0.18 nm.

[0064] In this invention, the number of periods of a single-period X / ligand / Y layer in a multi-period X / ligand / Y layer can be 50 to 250, for example, 100, 150, or 200. It is understood that the number of periods of a single-period X / ligand / Y layer in a multi-period X / ligand / Y layer refers to the number of single-period X / ligand / Y layers contained within the multi-period X / ligand / Y layer.

[0065] In this invention, the thickness of the underlayer can be 1 to 5 nm, for example 2 nm, 3 nm, or 4 nm.

[0066] In this invention, the thickness of the X layer can be 0.5 to 5 nm, for example 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, or 4.5 nm.

[0067] In this invention, the thickness of the Y layer can be 1 to 5 nm, for example, 2 nm, 3 nm, or 4 nm.

[0068] In this invention, the thickness of a single-cycle X / ligand / Y layer can be 1.6 to 11 nm, for example, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, or 10 nm.

[0069] The sputtering rate of each material can be determined by grazing incidence X-ray reflection testing. Knowing the sputtering rate of each material, the thickness of each layer obtained by magnetron sputtering can be determined.

[0070] The multilayer reflector of the present invention can be prepared by a method including the following steps:

[0071] (1) Prepare the underlayer on the substrate;

[0072] (2) On the substrate, an X layer, a ligand layer and a Y layer are prepared sequentially. The process of preparing the X layer, ligand layer and Y layer sequentially is repeated to obtain a multi-period X / ligand / Y layer.

[0073] In this invention, magnetron sputtering is used to prepare the underlayer, X layer, ligand layer, and Y layer. The target material used for magnetron sputtering is usually the same as the material of the layers to be prepared.

[0074] In this invention, the substrate preparation method can be either radio frequency magnetron sputtering or DC magnetron sputtering. The magnetron sputtering parameters for preparing the substrate can be set as follows: the background vacuum level before magnetron sputtering can be ≤1×10⁻⁶. -5 Pa, the sputtering method can be grazing target, the purity of the target material can be ≥99.5%, the working gas can be argon, the working gas pressure can be 0.15~0.25Pa (e.g. 0.18Pa, 0.2Pa, 0.22Pa), and the sputtering power can be 100~300W (e.g. 150W, 200W, 250W).

[0075] The choice between radio frequency (RF) or direct current (DC) magnetron sputtering can be made based on the conductivity of the target material. For example, RF magnetron sputtering can be used when the target material is B, while DC magnetron sputtering can be used when the target material is Si or C.

[0076] In this invention, the preferred method for fabricating the X layer is DC magnetron sputtering. The magnetron sputtering parameters for fabricating the X layer can be set such that the background vacuum before magnetron sputtering is ≤1×10⁻⁶. -5 Pa, the sputtering method can be grazing target, the purity of the target material can be ≥99.5%, the working gas can be argon, the working gas pressure can be 0.15~0.25Pa (e.g. 0.18Pa, 0.2Pa, 0.22Pa), and the sputtering power can be 40~120W (e.g. 60W, 80W, 100W).

[0077] In this invention, the preferred method for preparing the ligand layer is radio frequency magnetron sputtering. The magnetron sputtering parameters for preparing the ligand layer can be set such that the background vacuum before magnetron sputtering is ≤1×10⁻⁶. -5 Pa, the sputtering method can be grazing target, the purity of the target material can be ≥99.5%, the working gas can be argon, the working gas pressure can be 0.15~0.25Pa (e.g. 0.18Pa, 0.2Pa, 0.22Pa), and the sputtering power can be 100~300W (e.g. 150W, 200W, 250W).

[0078] In this invention, the Y-layer can be fabricated by radio frequency magnetron sputtering or DC magnetron sputtering. The magnetron sputtering parameters for fabricating the Y-layer can be set as follows: the base vacuum level before magnetron sputtering can be ≤1×10⁻⁶. -5 Pa, the sputtering method can be grazing target, the purity of the target material can be ≥99.5%, the working gas can be argon, the working gas pressure can be 0.15~0.25Pa (e.g. 0.18Pa, 0.2Pa, 0.22Pa), and the sputtering power can be 100~300W (e.g. 150W, 200W, 250W).

[0079] The present invention will be described below by way of specific embodiments. It should be understood that these embodiments are merely illustrative and are not intended to limit the scope of the invention. The methods, reagents, and materials used in the embodiments are conventional methods, reagents, and materials in the art, unless otherwise stated. The raw material compounds in the embodiments are all commercially available.

[0080] Example 1

[0081] This embodiment describes the fabrication of a La / HAT-CN / B extreme ultraviolet multilayer mirror, including the following steps:

[0082] (1) A silicon wafer is used as the substrate, and the roughness of the substrate is 0.2 nm.

[0083] (2) A 1.95 nm thick base layer (B layer) was fabricated on the substrate using radio frequency magnetron sputtering. The fabrication parameters included: base vacuum ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target material is B (purity ≥99.5%), working gas is argon, working gas pressure is 0.2 Pa, sputtering power is 250 W.

[0084] (3) A 1 nm thick La layer was prepared on the B layer by DC magnetron sputtering. The preparation parameters included: background vacuum ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target material is La (purity ≥99.5%), working gas is argon, working gas pressure is 0.1 Pa, sputtering power is 80 W.

[0085] (4) A HAT-CN layer with a thickness of 0.4 nm was prepared on the La layer by radio frequency magnetron sputtering. The preparation parameters included: background vacuum degree ≤1×10 -5 The sputtering method is grazing target, the target material is HAT-CN (purity ≥99.5%), the working gas is argon, the working pressure is 0.2 Pa, and the sputtering power is 250 W.

[0086] (5) A B layer with a thickness of 1.95 nm was prepared on the HAT-CN layer by radio frequency magnetron sputtering. The preparation parameters included: background vacuum degree ≤ 1 × 10 -5 Pa, sputtering method is target grazing, target material is B (purity ≥99.5%), working gas is argon, working gas pressure is 0.15 Pa, sputtering power is 250 W.

[0087] (6) Repeat steps (3) to (5) 199 times to obtain a multi-period La / HAT-CN / B layer with 200 periods, thereby obtaining a La / HAT-CN / B extreme ultraviolet multilayer reflector, wherein the thickness of a single-period La / HAT-CN / B layer is 3.35 nm.

[0088] Example 2

[0089] This embodiment describes the fabrication of a Mo / HAT-CN / Si extreme ultraviolet multilayer mirror, including the following steps:

[0090] (1) A silicon wafer is used as the substrate, and the roughness of the substrate is 0.2 nm.

[0091] (2) A 4.17 nm thick base layer Si was fabricated on the substrate by DC magnetron sputtering. The fabrication parameters included: base vacuum ≤ 1 × 10⁻⁶. -5 The sputtering method is grazing target, the target material is Si (purity ≥ 99.5%), the working gas is argon, the working pressure is 0.15 Pa, and the sputtering power is 140 W.

[0092] (3) A Mo layer with a thickness of 2.38 nm was prepared on the Si layer by DC magnetron sputtering. The preparation parameters included: background vacuum degree ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target material is Mo (purity ≥99.5%), working gas is argon, working gas pressure is 0.15 Pa, sputtering power is 100 W.

[0093] (4) A HAT-CN layer with a thickness of 0.4 nm was prepared on the Mo layer by radio frequency magnetron sputtering. The preparation parameters included: background vacuum degree ≤1×10 -5 The sputtering method is grazing target, the target material is HAT-CN (purity ≥99.5%), the working gas is argon, the working pressure is 0.2 Pa, and the sputtering power is 250 W.

[0094] (5) A 4.17 nm thick Si layer was prepared on the substrate by DC magnetron sputtering. The preparation parameters included: background vacuum ≤ 1 × 10⁻⁶. -5 The sputtering method is grazing target, the target material is Si (purity ≥ 99.5%), the working gas is argon, the working pressure is 0.15 Pa, and the sputtering power is 140 W.

[0095] (6) Repeat steps (3) to (5) 49 times to obtain a multi-period Mo / HAT-CN / Si layer with 50 periods, thereby obtaining a Mo / HAT-CN / Si extreme ultraviolet multilayer reflector, wherein the thickness of a single-period Mo / HAT-CN / Si layer is 6.95 nm.

[0096] Example 3

[0097] This embodiment describes the fabrication of a Cr / HAT-CN / C extreme ultraviolet multilayer mirror, including the following steps:

[0098] (1) A silicon wafer is used as the substrate, and the roughness of the substrate is 0.2 nm.

[0099] (2) A 3 nm thick base layer C was prepared on the substrate by DC magnetron sputtering. The preparation parameters included: base vacuum ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target material is C (purity ≥99.5%), working gas is argon, working gas pressure is 0.15 Pa, sputtering power is 140 W.

[0100] (3) A Cr layer with a thickness of 1.24 nm was prepared on the C layer by DC magnetron sputtering. The preparation parameters included: background vacuum degree ≤1×10 -5 Pa, sputtering method is target grazing, target material is Cr (purity ≥99.5%), working gas is argon, working gas pressure is 0.15 Pa, sputtering power is 100 W.

[0101] (4) A 0.2 nm thick HAT-CN layer was prepared on the Cr layer by radio frequency magnetron sputtering. The preparation parameters included: background vacuum degree ≤ 1 × 10⁻⁶. -5 The sputtering method is grazing target, the target material is HAT-CN (purity ≥99.5%), the working gas is argon, the working pressure is 0.15Pa, and the sputtering power is 250W.

[0102] (5) A C layer with a thickness of 1.24 nm was prepared on the HAT-CN layer by DC magnetron sputtering. The preparation parameters included: background vacuum degree ≤ 1 × 10⁻⁶. -5 Pa, sputtering method is target grazing, target material is C (purity ≥99.5%), working gas is argon, working gas pressure is 0.15 Pa, sputtering power is 140 W.

[0103] (6) Repeat steps (3) to (5) 299 times to obtain a multi-period Cr / HAT-CN / C layer with a period number of 300, thereby obtaining a Cr / HAT-CN / C extreme ultraviolet multilayer reflector, wherein the thickness of a single-period Cr / HAT-CN / C layer is 2.68 nm.

[0104] Comparative Example 1

[0105] Compared with Example 1, all other conditions are the same, except that the thickness of the La layer is 1.4 nm, the thickness of the HAT-CN layer is 0 nm, and the thickness of the B layer is 1.95 nm; that is, the HAT-CN layer is not deposited, and the thickness of the La / B layer in a single cycle is kept constant by increasing the thickness of the La layer.

[0106] Comparative Example 2

[0107] Compared with Example 2, all other conditions are the same, except that the thickness of the Mo layer is 2.38 nm, the thickness of the HAT-CN layer is 0 nm, and the thickness of the Si layer is 4.57 nm; that is, the HAT-CN layer is not deposited, and the thickness of the Mo / Si layer in a single cycle is kept constant by increasing the thickness of the Si layer.

[0108] Comparative Example 3

[0109] Compared with Example 3, all other conditions are the same, except that the thickness of the Cr layer is 1.24 nm, the thickness of the HAT-CN layer is 0 nm, and the thickness of the C layer is 1.44 nm; that is, the HAT-CN layer is not deposited, and the thickness of the Cr / C layer in a single cycle is kept constant by increasing the thickness of the C layer.

[0110] Example 4

[0111] Compared with Example 1, all other conditions are the same, except that the ligand is replaced by lanthanum borate instead of HAT-CN, that is, in step (4), a lanthanum borate layer with a thickness of 0.4 nm is prepared using lanthanum borate as the target material.

[0112] Example 5

[0113] Compared with Example 1, all other conditions are the same, except that the ligand is replaced by urea instead of HAT-CN, that is, in step (4), a urea layer with a thickness of 0.4 nm is prepared using urea as the target material.

[0114] Example 6

[0115] Compared with Example 1, all other conditions are the same, except that the ligand is replaced by 2,4,6,8-tetrahydroxypyrimidine[5,4-d]pyrimidine, that is, in step (4), a 2,4,6,8-tetrahydroxypyrimidine[5,4-d]pyrimidine layer with a thickness of 0.4 nm is prepared using 2,4,6,8-tetrahydroxypyrimidine[5,4-d]pyrimidine as the target material.

[0116] Example 7

[0117] Compared with Example 1, all other conditions are the same, except that the ligand is replaced by 5-aminoorotic acid, that is, in step (4), a 5-aminoorotic acid layer with a thickness of 0.4 nm is prepared using 5-aminoorotic acid as the target material.

[0118] The wavelength-theoretical reflectivity curves of the multilayer film mirrors of Examples 1-7 and Comparative Examples 1-3 were obtained using IMD software simulation. The theoretical reflectivity of the multilayer film mirrors of Examples 1-7 and Comparative Examples 1-3 at wavelengths of 6.65 nm, 13.5 nm, or 4.7 nm is shown in Table 1. The wavelength-theoretical reflectivity curves of the multilayer film mirrors of Examples 1, 2, Comparative Examples 1, and 2 are shown in Table 1. Figure 3-6 As shown.

[0119] Table 1: Theoretical reflectivity of multilayer mirrors in Examples 1-7 and Comparative Examples 1-3

[0120] Wavelength (nm) Angle of incidence (°) Theoretical reflectance (%) Example 1 6.65 11.2 84.8 Example 2 13.5 6 72.1 Example 3 4.7 10.3 41.7 Example 4 6.65 11.2 81.3 Example 5 6.65 11.2 84.7 Example 6 6.65 11.2 83.6 Example 7 6.65 11.2 83.8 Comparative Example 1 6.65 11.2 84.1 Comparative Example 2 13.5 6 73.3 Comparative Example 3 4.7 10.3 42

[0121] From Table 1 and Figures 3-6 It can be seen that, compared with conventional X / Y multilayer mirrors, the theoretical reflectivity of the X / ligand / Y multilayer mirror with the introduction of a ligand layer is not significantly different. However, in practical applications, because the ligand layer introduced in this invention at the Y-on-X interface reduces interfacial diffusion and improves optical contrast, the actual reflectivity of the X / ligand / Y extreme ultraviolet multilayer mirror of this invention decreases significantly less than that of the conventional X / Y multilayer mirror.

[0122] Furthermore, some mirrors with ligand layers even exhibited theoretical reflectivities higher than the control group. For example, for the La / B system, the theoretical reflectivities of Example 1 (ligand HAT-CN) and Example 5 (ligand urea) were higher than those of Comparative Example 1. This will help maintain a high level of reflectivity in mirrors during practical engineering applications, thereby improving the long-term stability of key performance indicators of mirrors.

Claims

1. A multilayer film mirror, characterized by, The reflector includes a substrate, a base layer disposed on the substrate, and a multi-period X-layer / ligand / Y-layer disposed on the base layer; The multi-period X-layer / ligand / Y-layer comprises multiple stacked single-period X-layer / ligand / Y-layers; The single-cycle X-layer / ligand / Y-layer comprises an X-layer, a ligand layer, and a Y-layer stacked sequentially. The ligand layer is made of one or more selected from lanthanum borate, urea, 2,4,6,8-tetrahydroxypyrimidin[5,4-d]pyrimidine, 5-aminoorotic acid and 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene; The ligand layer coordinates with the X layer, inhibiting the reaction between the X layer and the Y layer; The X layer in the single-cycle X layer / ligand / Y layer closest to the substrate is in contact with the substrate. The thickness of the ligand layer is 0.1~1 nm; The thickness of the substrate layer is 1~5 nm; The thickness of the X layer is 0.5~5 nm; The thickness of the Y layer is 1~5 nm; The thickness of the single-cycle X-layer / ligand / Y-layer is 1.6~11 nm.

2. The multilayer film reflector as described in claim 1, characterized in that, The material of the base layer is B, the material of the X layer is La, and the material of the Y layer is B or a compound of B; or The material of the base layer is Si, the material of the X layer is Mo, and the material of the Y layer is either Si or Be; or The material of the base layer is C, the material of the X layer is Cr, and the material of the Y layer is C.

3. The multilayer film mirror of claim 1, wherein, The substrate is a silicon wafer, a quartz wafer, or a glass sheet.

4. The multilayer film mirror of claim 1, wherein, The roughness of the substrate is 0.1~0.2 nm.

5. The multilayer film mirror of claim 1, wherein, The number of cycles in a single-cycle X-layer / ligand / Y-layer in the multi-cycle X-layer / ligand / Y-layer is 50 to 250.

6. A method of making the multilayer film mirror of any of claims 1-5, wherein, The method includes the following steps: (1) Prepare the underlayer on the substrate; (2) On the substrate, the X layer, ligand layer and Y layer are prepared sequentially, and the process of preparing the X layer, ligand layer and Y layer sequentially is repeated to obtain a multi-cycle X layer / ligand / Y layer.

7. The method of claim 6, wherein, The preparation method of the ligand layer is radio frequency magnetron sputtering, and the magnetron sputtering parameters for preparing the ligand layer include: a background vacuum degree ≤ 1 × 10 -5 -1 Pa, a sputtering mode is a target grazing, a purity of a target material ≥ 99.5%, a working gas is argon, a working pressure is 0.1-0.25 Pa, and a sputtering power is 100-300 W.

Citation Information

Patent Citations

  • Infrared shielding film having dielectric multilayer film structure

    CN104428698A

  • LaNx / La / B4C extreme ultraviolet multilayer film reflector and preparation method thereof

    CN116107001A