A modified zeolite composite membrane material, its preparation method and application

By preparing a core-shell structured modified zeolite composite membrane material with a zinc-doped zeolite core and a titanium dioxide shell, the problems of polysulfide shuttle effect and lithium dendrite formation in lithium-sulfur batteries were solved, achieving high efficiency, cycle stability and safety of lithium-sulfur batteries.

CN117525745BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311370618.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2026-11-17
Estimated Expiration
2043-10-20

AI Technical Summary

Technical Problem

The commercial development of lithium-sulfur batteries is hampered by issues such as polysulfide shuttle effect and lithium dendrite formation in the negative electrode, resulting in low utilization of active materials, unstable cycling, and safety problems.

Method used

A modified zeolite composite membrane material with a core-shell structure is used, with a zinc-doped zeolite core and a titanium dioxide shell. It is prepared by coaxial spinning and calcination to synergistically improve the cycle stability of lithium-sulfur batteries.

Benefits of technology

It effectively accelerates the redox rate of polysulfides, suppresses the polysulfide shuttle effect, and improves the cycle stability and safety performance of lithium-sulfur batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117525745B_ABST
    Figure CN117525745B_ABST
Patent Text Reader

Abstract

This application discloses a modified zeolite composite membrane material, its preparation method, and its application. The modified zeolite composite membrane material has a core-shell structure with a core and a shell; the core is zinc-doped zeolite; and the shell is titanium dioxide. The composite membrane material prepared by this method exhibits outstanding mechanical properties and is suitable for use as a membrane material in lithium-sulfur batteries. The core layer contains zinc cations. 2+ Zeolite can serve as an active site for adsorbing lithium polysulfides (LiPSs) and catalyzing multi-electron redox reactions. Furthermore, the pore size of zeolite, as a molecular sieve, limits the shuttle movement of polysulfides. The polar TiO2 molecules in the shell further restrict the shuttle effect through chemical interaction, accelerating the conversion of intermediate products. The constructed core-shell structure synergistically enhances the cycle stability of lithium-sulfur batteries by combining the shell and core layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a modified zeolite composite membrane material, its preparation method, and its application, belonging to the field of battery technology. Background Technology

[0002] Rechargeable batteries have developed rapidly as energy storage devices and are widely used in various fields such as electric vehicles, electronic products, and power storage. To date, lithium-ion batteries are the best-performing commercially available rechargeable battery system, but they primarily use LiFeO4, LiCoO2, and LiNi... 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other materials are used as cathode materials, but the theoretical capacity of these cathode materials generally does not exceed 300 mAh g. -1 However, there is still a considerable distance to go before achieving the goal of high-energy-density batteries. Therefore, research on advanced energy storage technologies is urgently needed to solve the energy storage problem. The theoretical specific capacity of the new lithium-sulfur battery is about five times that of the commercial lithium-ion battery (theoretical specific capacity is 1675 mAh / g). Moreover, sulfur is abundant in nature, non-toxic, environmentally friendly, and inexpensive. Therefore, lithium-sulfur batteries are considered to be one of the most promising high-performance batteries.

[0003] However, the commercial development of lithium-sulfur batteries has faced many challenges, including the shuttle effect caused by polysulfides and the formation of lithium dendrites on the negative electrode, leading to low utilization of active materials, unstable cycling, and safety issues. The separator plays a crucial role in the battery, not only isolating the positive and negative electrodes to prevent short circuits and improve battery safety, but also possessing a certain capacity for electrolyte absorption and retention, reducing the battery's internal resistance. Summary of the Invention

[0004] One aspect of this application provides a modified zeolite composite membrane material that can effectively accelerate the redox rate of polysulfides and suppress the shuttle effect of polysulfides.

[0005] The modified zeolite composite membrane material has a core-shell structure with a core and a shell.

[0006] The core is a zinc-doped zeolite;

[0007] The shell is titanium dioxide.

[0008] Optionally, the zinc-doped zeolite contains 2% to 7% zinc by mass.

[0009] Optionally, in the zinc-doped zeolite, the zinc content is independently selected from any value of 2%, 3%, 4%, 5%, 6%, 7% or a range between any two of the above.

[0010] Another aspect of this application provides a method for preparing the above-mentioned modified zeolite composite membrane material, the method comprising:

[0011] (1) Mix the zeolite and zinc source solution, stir to obtain solution I, dry to obtain Zn. 2+ The incorporated zeolite powder;

[0012] (2) Containing polymers I and Zn 2+ A mixture of incorporated zeolite powders is dispersed in a solvent to obtain a nucleus solution;

[0013] (3) Polymer II is dissolved in a mixed solution of ethanol and acetic acid to obtain solution II. A titanium source is added to obtain a shell solution.

[0014] (4) The core solution and the shell solution are coaxially spun and calcined to obtain the modified zeolite composite membrane material.

[0015] Optionally, the zinc source is selected from at least one of zinc sulfate, zinc acetate, and zinc carbonate.

[0016] Optionally, the concentration of zinc ions in the zinc source solution is 0.5 mol / L to 2 mol / L.

[0017] Optionally, the concentration of zinc ions in the zinc source solution is independently selected from any value among 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, or a range between any two of the above.

[0018] Optionally, the zeolite concentration in solution I is 5–30 mg / mL.

[0019] Optionally, in solution I, the mass concentration of zeolite is independently selected from any value of 5 mg / mL, 15 mg / mL, 20 mg / mL, 25 mg / mL, 30 mg / mL, or a range between any two of the above.

[0020] Optionally, the stirring time is 3 to 8 hours.

[0021] Optionally, the stirring time is independently selected from any value of 3h, 4h, 5h, 6h, 7h, 8h or a range between any two of the above.

[0022] Optionally, the drying temperature is 60℃ to 100℃.

[0023] Optionally, the drying temperature is independently selected from any value of 60°C, 80°C, 100°C, or a range between any two of the above.

[0024] Optionally, the polymer I is selected from at least one of polystyrene, polyacrylonitrile, polymethyl methacrylate, and polyvinylpyrrolidone.

[0025] Optionally, the polymer I and the Zn 2+ The mass ratio of the incorporated zeolite powder is 3 to 8.

[0026] Optionally, the polymer I and the Zn 2+ The mass ratio of the incorporated zeolite powder is independently selected from any value of 3, 4, 5, 6, 7, 8 or a range between any two of the above.

[0027] Optionally, in the nuclear solution, the mass ratio of polymer I to solvent is 1:2 to 1:6.

[0028] Optionally, in the nuclear solution, the mass ratio of polymer I to solvent is independently selected from any value of 1:2, 1:4, 1:6 or a range between any two of the above.

[0029] Optionally, the solvent is selected from at least one of N,N-dimethylamide, isopropanol, and methanol.

[0030] Optionally, the polymer II is selected from at least one of polyvinylpyrrolidone, polyvinyl acetate, and polyacrylonitrile.

[0031] Optionally, in the mixed solution of ethanol and acetic acid, the mass ratio of ethanol to acetic acid is 2 to 4.

[0032] Optionally, in the mixed solution of ethanol and acetic acid, the mass ratio of ethanol to acetic acid is independently selected from any value of 2, 3, or 4, or a range between any two of the above.

[0033] Optionally, in solution II, the mass ratio of polymer II to the mixed solution of ethanol and acetic acid is 1:15 to 1:30.

[0034] Optionally, in solution II, the mass ratio of polymer II to the ethanol and acetic acid mixture is independently selected from any value of 1:15, 1:20, 1:25, 1:30 or a range between any two of the above.

[0035] Optionally, the titanium source is selected from at least one of titanium isopropoxide, tetrabutyl titanate, and titanium dioxide.

[0036] Optionally, in the shell solution, the mass concentration of the titanium source is 10% to 30%, based on the mass of titanium ions.

[0037] Optionally, in the shell solution, the mass concentration of the titanium source is independently selected from any value of 10%, 20%, 30%, or a range between any two of the above.

[0038] Optionally, the conditions for coaxial spinning are:

[0039] The operating voltage is 15-18kV, the receiving distance is 17-20cm, and the operating time is 2-5h.

[0040] Optionally, the operating voltage is independently selected from any value of 15kV, 16kV, 17kV, 18kV or a range between any two of the above.

[0041] Optionally, the receiving distance is independently selected from any value among 17cm, 18cm, 19cm, and 20cm, or a range between any two of the above.

[0042] Optionally, the running time is independently selected from any value of 2h, 3h, 4h, 5h or a range between any two of the above.

[0043] Optionally, the spinning flow rate of the coaxial spinning is:

[0044] The flow rate of the nuclear fluid is 0.5–1.2 mL / h. -1 ;

[0045] The flow rate of the shell fluid is 1.2–2.0 mL / h. -1 .

[0046] Optionally, the flow rate of the nuclear fluid is independently selected from 0.5 mL h. -1 0.7 mL h -1 0.9 mL h -1 1.2 mL h -1 Any value in or a range between any two of the above.

[0047] Optionally, the flow rate of the shell fluid is independently selected from 1.2 mL h. -1 1.5 mL h -1 1mL h -1 2.0 mL h -1 Any value in or a range between any two of the above.

[0048] Optionally, the calcination temperature is 500–700°C.

[0049] Optionally, the calcination temperature is independently selected from any value of 500°C, 600°C, 700°C, or a range between any two of the above.

[0050] The calcination time is 1 to 5 hours.

[0051] The calcination time is independently selected from any value of 1h, 2h, 3h, 4h, 5h or a range between any two of the above.

[0052] The calcination is carried out under an oxygen-containing atmosphere.

[0053] As one specific implementation method, the preparation method of the modified zeolite composite membrane material includes:

[0054] (1) Add zeolite to zinc sulfate solution, stir for a certain period of time, and repeatedly wash and dry to obtain Zn. 2+ The zeolite powder incorporated.

[0055] (2) Combining polymers with Zn 2+ -Zeolite powder is dispersed in 5-15g of DMF solution at a certain mass ratio to form a uniform core solution.

[0056] (3) Dissolve 0.3-0.6g PVP (Mw=1,300,000) in a mixed solution of ethanol and acetic acid in a certain ratio, slowly add 3-5g titanium isopropoxide and stir for a certain period of time to obtain the shell solution.

[0057] (4) The above core-shell solution is placed into a syringe and coaxial spinning technology is used, wherein the flow rates of the core fluid and the shell fluid are controlled, the working voltage is 15-18kV, the receiving distance is 17cm, and the process is carried out for a certain period of time to prepare the precursor nanofiber membrane of the diaphragm material.

[0058] (5) The precursor nanofiber membrane was calcined in air at 500-700℃ to obtain Zn. 2+ Membrane material with incorporated zeolite powder and TiO2

[0059] The polymer mentioned in step (2) is one or more of polystyrene, polyacrylonitrile, polymethyl methacrylate, and polyvinylpyrrolidone.

[0060] In another aspect of this application, the above-mentioned modified zeolite composite membrane material is provided as an application of the membrane material in lithium-sulfur batteries.

[0061] Based on the above technical solution, due to the core layer metal cation Zn 2+ Zeolite can serve as an active site for adsorbing lithium polysulfides (LiPSs) and catalyzing multi-electron redox reactions. Furthermore, the pore size of the zeolite, as a molecular sieve, limits the shuttle movement of polysulfides. The polar TiO2 molecules in the shell further restrict the shuttle effect through chemical interaction, accelerating the conversion of intermediate products. The constructed core-shell structure synergistically enhances the cycle stability of lithium-sulfur batteries by combining the shell and core layers.

[0062] The beneficial effects that this application can produce include:

[0063] 1) The modified zeolite composite membrane material proposed in this invention has a core-shell structure, with the core being zinc-doped zeolite and the shell being titanium dioxide. By working together, the shell and core layers can effectively accelerate the redox rate of polysulfides and suppress the shuttle effect of polysulfides. As a membrane material for lithium-sulfur batteries, it can jointly improve the cycle stability of lithium-sulfur batteries.

[0064] 2) The preparation method of the modified zeolite composite membrane material proposed in this invention is simple, environmentally friendly, low in cost, and has good safety performance. Attached Figure Description

[0065] Figure 1 This is a morphology diagram of the diaphragm material obtained in Example 1 of this application, where the scale bar is 2 μm.

[0066] Figure 2 This is a rate performance diagram of the diaphragm material obtained in Example 1 of this application under different current densities.

[0067] Figure 3 This is a cycling diagram of the membrane material obtained in Example 1 of this application at 0.2C. Detailed Implementation

[0068] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0069] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0070] Example 1

[0071] (1) Add 0.15g of zeolite to 30ml of 1mol / L zinc sulfate solution, stir for 3h, wash repeatedly, and dry at 60℃ to obtain Zn. 2+ The incorporated zeolite powder, of which Zn 2+ The content is 10mg.

[0072] (2) Mix 3.5g of polystyrene with 0.7g of Zn 2+ - Zeolite powder is dispersed in 10g of DMF solution to form a homogeneous core solution.

[0073] (3) Dissolve 0.5g PVP (Mw = 1,300,000) in a mixed solution of 8g ethanol and 4g acetic acid, slowly add 5g titanium isopropoxide and stir for 4h to obtain the shell solution.

[0074] (4) The above core-shell solution was placed into a syringe, and coaxial spinning technology was used, wherein the flow rates of the core fluid and the shell fluid were controlled to be 0.5 mL / h.-1 and 1.2 mL h -1 The process was carried out at a working voltage of 17kV and a receiving distance of 17cm for 2 hours to obtain the precursor nanofiber membrane.

[0075] (5) The precursor nanofiber membrane was calcined in air at 600°C for 1 hour to obtain Zn. 2+ A membrane material incorporating zeolite powder and TiO2.

[0076] Example 2

[0077] (1) Add 0.2 g of zeolite to 30 ml of 1 mol / L zinc sulfate solution, stir for 4 h, wash repeatedly, and dry at 60 °C to obtain Zn. 2+ The incorporated zeolite powder, of which Zn 2+ The content is 10mg.

[0078] (2) Mix 3.5g of polystyrene with 0.7g of Zn 2+ - Zeolite powder is dispersed in 10g of DMF solution to form a homogeneous core solution.

[0079] (3) Dissolve 0.5g PVP (Mw = 1,300,000) in a mixed solution of 8g ethanol and 4g acetic acid, slowly add 5g titanium isopropoxide and stir for 4h to obtain the shell solution.

[0080] (4) The above core-shell solution was placed into a syringe, and coaxial spinning was used, wherein the flow rates of the core fluid and the shell fluid were controlled to be 0.7 mL / h. -1 and 1.5 mL h -1 The process was carried out at a working voltage of 17kV and a receiving distance of 17cm for 2 hours to obtain the precursor nanofiber membrane.

[0081] (5) The precursor nanofiber membrane was calcined in air at 600°C for 1 hour to obtain Zn. 2+ A membrane material incorporating zeolite powder and TiO2.

[0082] Example 3

[0083] (1) Add 0.4 g of zeolite to 30 ml of 2 mol / L zinc sulfate solution, stir for 6 h, wash repeatedly, and dry at 60 °C to obtain Zn. 2+ The incorporated zeolite powder, of which Zn 2+ The content is 20mg.

[0084] (2) Mix 3.5g of polystyrene with 0.7g of Zn 2+ - Zeolite powder is dispersed in 10g of DMF solution to form a homogeneous core solution.

[0085] (3) Dissolve 0.5g PVP (Mw = 1,300,000) in a mixed solution of 8g ethanol and 4g acetic acid, slowly add 5g titanium isopropoxide and stir for 4h to obtain the shell solution.

[0086] (4) The above core-shell solution was placed into a syringe, and coaxial spinning technology was used, wherein the flow rates of the core fluid and the shell fluid were controlled to be 0.9 mL / h. -1 and 1.8 mL h -1 The process was carried out at a working voltage of 17kV and a receiving distance of 17cm for 2 hours to obtain the precursor nanofiber membrane.

[0087] (5) The precursor nanofiber membrane was calcined in air at 600°C for 1 hour to obtain Zn. 2+ A membrane material incorporating zeolite powder and TiO2.

[0088] Example 4

[0089] (1) Add 0.6 g of zeolite to 30 ml of 2 mol / L zinc sulfate solution, stir for 8 h, wash repeatedly, and dry at 60 °C to obtain Zn. 2+ The incorporated zeolite powder, of which Zn 2+ The content is 20mg.

[0090] (2) Mix 3.5g of polystyrene with 0.7g of Zn 2+ - Zeolite powder is dispersed in 10g of DMF solution to form a homogeneous core solution.

[0091] (3) Dissolve 0.5g PVP (Mw = 1,300,000) in a mixed solution of 8g ethanol and 4g acetic acid, slowly add 5g titanium isopropoxide and stir for 4h to obtain the shell solution.

[0092] (4) The above core-shell solution was placed into a syringe, and coaxial spinning was used, wherein the flow rates of the core fluid and the shell fluid were controlled to be 1.2 mL / h. -1 and 2.0 mL h -1 The process was carried out at a working voltage of 17kV and a receiving distance of 17cm for 2 hours to obtain the precursor nanofiber membrane.

[0093] (5) The precursor nanofiber membrane was calcined in air at 600°C for 1 hour to obtain Zn. 2+ A membrane material incorporating zeolite powder and TiO2.

[0094] Test case

[0095] The Zn obtained in the above embodiments 2+ The membrane material incorporating zeolite powder composite TiO2 was tested, using Zn obtained in Example 1.2+ A typical example is the membrane material made by incorporating zeolite powder with TiO2.

[0096] Zn obtained in Example 1 2+ The morphology of the diaphragm material incorporating zeolite powder and TiO2 was tested using a Quanta 250FEG Czech instrument. The test results are as follows: Figure 1 ,from Figure 1 It can be seen that the interior and exterior of the material exhibit different morphological structures; the interior consists of Zn. 2+ It is composed of doped zeolite and has a smooth TiO2 exterior.

[0097] Zn obtained in Example 1 2+ Taking the diaphragm material incorporating zeolite powder and TiO2 as an example, rate performance and cycle performance tests were conducted. The tests were performed within a voltage range of 1.7V-2.8V. The test results are shown below. Figure 2 , Figure 3 It can be seen that the Zn obtained in Example 1 2+ The membrane material with incorporated zeolite powder and TiO2 can achieve a current density of 812 mAh g at 5C. -1 After 100 cycles at a current density of 0.2C, the capacity retention reached 83.3%, which is mainly attributed to the core metal cation Zn. 2+ Zeolite can serve as an active site for adsorbing lithium polysulfides (LiPSs) and catalytically related multi-electron redox reactions. Furthermore, as a molecular sieve, zeolite limits the shuttle movement of polysulfides due to its pore size. The polar TiO2 molecules in the shell further limit the shuttle effect through chemical action, accelerating the conversion of intermediate products.

[0098] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A modified zeolite composite diaphragm material, characterized in that, The modified zeolite composite membrane material has a core-shell structure with a core and a shell. The core is a zinc-doped zeolite; The shell is titanium dioxide; The preparation method of the modified zeolite composite membrane material includes the following steps: (1) Mix the zeolite and zinc source solution, stir to obtain solution I, dry to obtain Zn 2+ The incorporated zeolite powder; (2) Containing polymers I and Zn 2+ A mixture of incorporated zeolite powders is dispersed in a solvent to obtain a nucleus solution; (3) Polymer II is dissolved in a mixed solution of ethanol and acetic acid to obtain solution II. A titanium source is added to obtain a shell solution. (4) The core solution and shell solution are coaxially spun and calcined to obtain the modified zeolite composite membrane material.

2. The modified zeolite composite diaphragm material according to claim 1, characterized in that, In zinc-doped zeolites, the zinc content is 2% to 7% by mass.

3. A method for preparing the modified zeolite composite membrane material according to claim 1 or 2, characterized in that, The preparation method includes: (1) Mix the zeolite and zinc source solution, stir to obtain solution I, dry to obtain Zn 2+ The incorporated zeolite powder; (2) Containing polymers I and Zn 2+ A mixture of incorporated zeolite powders is dispersed in a solvent to obtain a nucleus solution; (3) Polymer II is dissolved in a mixed solution of ethanol and acetic acid to obtain solution II. A titanium source is added to obtain a shell solution. (4) The core solution and shell solution are coaxially spun and calcined to obtain the modified zeolite composite membrane material.

4. The preparation method according to claim 3, characterized in that, The zinc source is selected from at least one of zinc sulfate, zinc acetate, and zinc carbonate; The zinc source solution contains zinc ions at a concentration of 0.5–2 mol / L. In solution I, the mass concentration of zeolite is 5~30 mg / mL; The stirring time is 3-8 hours; The drying temperature is 60℃~100℃.

5. The preparation method according to claim 3, characterized in that, The polymer I is selected from at least one of polystyrene, polyacrylonitrile, polymethyl methacrylate, and polyvinylpyrrolidone; The polymer I and the Zn 2+ The mass ratio of the incorporated zeolite powder is 3~8; In the nuclear solution, the mass ratio of polymer I to solvent is 1:2 to 1:6; The solvent is selected from at least one of N,N-dimethylamide, isopropanol, and methanol.

6. The preparation method according to claim 3, characterized in that, The polymer II is selected from at least one of polyvinylpyrrolidone, polyvinyl acetate, and polyacrylonitrile; In the mixed solution of ethanol and acetic acid, the mass ratio of ethanol to acetic acid is 2 to 4; In solution II, the mass ratio of polymer II to the mixed solution of ethanol and acetic acid is 1:15 to 1:30; The titanium source is selected from at least one of titanium isopropoxide, tetrabutyl titanate, and titanium dioxide. In the shell solution, the mass concentration of the titanium source is 10% to 30%, based on the mass of titanium ions.

7. The preparation method according to claim 3, characterized in that, The conditions for coaxial spinning are as follows: The operating voltage is 15~18 kV, the receiving distance is 17~20cm, and the operating time is 2~5h.

8. The preparation method according to claim 3, characterized in that, The spinning flow rate of the coaxial spinning is: The flow rate of the nuclear fluid is 0.5–1.2 mL / h. -1 ; The flow rate of the shell fluid is 1.2~2.0 mL / h. -1 .

9. The preparation method according to claim 3, characterized in that, The calcination temperature is 500~700℃; The calcination time is 1-5 hours; The calcination is carried out under an oxygen-containing atmosphere.

10. The application of the modified zeolite composite membrane material according to claim 1 or 2 as a lithium-sulfur battery membrane material.

Citation Information

Patent Citations

  • Functional composite membrane for lithium-sulfur battery and preparation method of functional composite membrane

    CN105140447A

  • S-Ni-O-C bonding enhanced lithium-sulfur battery composite positive electrode material and preparation method thereof