Early-strength anti-cracking concrete for assembly and preparation method thereof
By using pre-strength and crack-resistant concrete for assembly in high-speed rail construction, the problem of insufficient wet connection performance of existing concrete is solved, efficient construction and high-quality connection are achieved, and the early strength and crack-resistant performance of concrete are significantly improved.
Patent Information
- Application Number
- CN202311534179.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-11-17
AI Technical Summary
The existing concrete has insufficient wet connection performance in high-speed rail construction, resulting in delayed construction progress and poor crack resistance, affecting the quality of the project.
A premature strength anti-crack concrete for assembly is used, which consists of ordinary silicate cement, fly ash, sand, gravel, composite admixture and steel fiber. The composite admixture includes premature strength components and expansion agents. , water reducing agent, defoaming agent and retarding components, modified nanomaterials and high-performance polymer fibers, and improve the early strength and crack resistance of concrete through surface modification treatment and segmented stirring.
It significantly improves the early compressive strength, volume stability and crack resistance of concrete, extends the service life of the structure, and is suitable for wet joint connections in high-speed rail bridges and other projects, meeting the requirements of rapid construction and high quality.
Smart Images

Figure CN117585955B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of prefabricated buildings, and in particular to an early-strength anti-cracking concrete for assembly and a preparation method thereof. Background Art
[0002] As an important strategic industry in my country in the 21st century, high-speed rail construction has had a profound impact on national infrastructure construction and economic development. In the process of high-speed rail construction, the proportion of prefabricated structures has gradually increased, and the wet connection performance between prefabricated components has become an important factor restricting construction efficiency and project quality. The existing wet connection method mainly uses concrete materials, but it has some limitations. First, concrete connections require a long curing time, which leads to delays in the construction progress; second, the construction time of concrete is relatively short, which is a challenge for engineering projects that require long-distance transportation and slow construction speed; at the same time, concrete is prone to cracking in the early drying stage, which has a negative impact on the quality and aesthetics of the structure.
[0003] Based on the shortcomings of the prior art, there is an urgent need for an early-strength, crack-resistant concrete for assembly and a preparation method thereof. Summary of the invention
[0004] The purpose of the present invention is to provide an early-strength anti-cracking concrete for assembly and a preparation method thereof to improve the above-mentioned problems. In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows:
[0005] On the one hand, the present application provides an early-strength and crack-resistant concrete for assembly, characterized in that it is prepared from ordinary Portland cement, fly ash, sand, gravel, composite admixtures, steel fiber and water, the composite admixtures are prepared from early-strength components, expansion agents, water reducers, defoaming agents, retarding components, modified nanomaterials, high-performance polymer fibers and organic microspheres, and the modified nanomaterials are prepared from carbon nanotubes, nano-silicon powder and nano-titanium oxide.
[0006] Furthermore, the weight ratio of the ordinary Portland cement, the fly ash, the sand, the crushed stone, the composite admixture, the steel fiber and the water is (480-530): (70-120): (750-830): (680-750): (60-110): (20-40): (180-195), and the weight ratio of the early strength component, the expansion agent, the water reducer, the defoamer, the retarding component, the modified nanomaterial, the high-performance polymer fiber and the organic microsphere is (35-65): (18-38): (4-5): (0.9-1.8): (0.9-1.8): (2-8): (5-15): (3-10).
[0007] Furthermore, the early strength component includes an accelerator and an early strength agent, the expansion agent is a calcium-magnesium composite expansion agent, the water reducer is a polycarboxylate water reducer, and the retarding component includes sodium gluconate and sodium citrate. The accelerator and the early strength agent react chemically with water and cement particles to generate calcium silicate hydrate, the polycarboxylate water reducer interacts with ions in water to form a surfactant, the calcium-magnesium composite expansion agent reacts with water to generate a colloidal substance, the colloidal substance includes magnesium hydroxide and calcium hydroxide, the colloidal substance fills the micropores inside the concrete, and the sodium gluconate and the sodium citrate react with the colloidal substance to generate calcium gluconate and calcium citrate.
[0008] Furthermore, the organic microspheres are polystyrene microspheres.
[0009] Furthermore, the high-performance polymer fiber is polyvinyl alcohol fiber.
[0010] In a second aspect, the present application also provides a method for preparing the early-strength and crack-resistant concrete for assembly, the method comprising:
[0011] Performing surface modification on carbon nanotubes, nano silicon powder and nano titanium oxide to obtain modified nano materials;
[0012] The modified nanomaterial is mixed with high-performance polymer fibers, and dispersed into a polymer matrix using ultrasonic technology to obtain a nanocomposite material;
[0013] The early strength component, the expansion agent, the water reducing agent, the defoaming agent and the retarding component are subjected to ion exchange and molecular level modification to obtain a composite admixture dry mix;
[0014] Premixing ordinary Portland cement, fly ash and the composite admixture dry mix, and then adding the nanocomposite material and polystyrene microspheres for stirring and mixing to obtain a concrete premix;
[0015] The steel fibers are uniformly mixed into the concrete premix, and the early-strength anti-cracking concrete for assembly is obtained through staged mixing.
[0016] The beneficial effects of the present invention are:
[0017] The present invention uses a coagulant and an early strength agent to rapidly form calcium silicate hydrate in the early stage of concrete, thereby improving the early compressive strength of concrete. The use of a calcium-magnesium composite expansion agent enables concrete to react in stages to generate a colloidal substance, which fills the micropores inside the concrete, reduces the shrinkage deformation of the concrete, and improves the volume stability of the concrete. At the same time, the magnesium hydroxide and calcium hydroxide in the colloidal substance and the generated calcium gluconate and calcium citrate help to improve the durability of the concrete, reduce the risk of cracking, and extend the service life of the concrete structure; by adding modified nanomaterials and high-performance polymer fibers to the concrete, the mechanical properties of the concrete are significantly improved.
[0018] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or be understood by implementing the embodiments of the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 This is a test diagram of the limited expansion rate of different expansion agent dosages in the embodiment of the present invention after curing in water for 14 days;
[0021] Figure 2 This is a test diagram of the limiting expansion rate of different expansion agent dosages in the embodiment of the present invention after curing in water for 14 days and then in air for 28 days;
[0022] Figure 3 This is a test diagram of the limited expansion rate of different steel fiber dosages in the embodiment of the present invention after curing in water for 14 days;
[0023] Figure 4 This is a test diagram of the restricted expansion rate of different steel fiber dosages in the embodiment of the present invention after being cured in water for 14 days and then in air for 28 days. DETAILED DESCRIPTION
[0024] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0025] Unless otherwise specified, the raw materials in the examples of this application were purchased from commercial sources. Unless otherwise specified, the test methods all adopted conventional methods, and the instruments all adopted the configuration recommended by the manufacturer.
[0026] High-speed rail construction has made great achievements in China since the 21st century and has become an important part of the country's strategic industry. The extensive laying of high-speed rail has not only accelerated the transportation connectivity between various parts of our country, but also greatly improved people's travel experience. The continuous expansion of China's high-speed rail network has had a profound social and economic impact. However, this huge construction is also accompanied by a series of challenges, one of which is the construction and quality assurance of the substructure of the high-speed rail bridge.
[0027] In high-speed rail construction, the use of prefabricated components has gradually increased. This construction method can significantly improve construction efficiency and project quality. However, wet joints between prefabricated components have always been a key issue. Usually these joints are cast in concrete. Concrete wet joints meet the requirements of structural strength and stability to a certain extent, but there are some obvious shortcomings. First, traditional concrete structures require a long maintenance period, which will extend the construction period, especially in harsh climatic conditions. Second, the strength of concrete increases slowly and is not suitable for rapid construction requirements. Most importantly, structures such as high-speed rail bridges have strict requirements on crack resistance, and traditional concrete may have some limitations in this regard, especially in wet joints.
[0028] Although the traditional wet-joint method of concrete meets the requirements of structural strength to a certain extent, its long maintenance period seriously affects the progress of high-speed rail projects. Especially under winter construction conditions, the extension of the maintenance period becomes a great problem. In addition, the strength growth of traditional concrete at the wet-joint part is relatively slow, which is difficult to meet the requirements of high-speed rail projects for rapid construction. At the same time, the crack resistance of traditional concrete may not be ideal, which may cause a series of problems in long-term use.
[0029] An early-strength anti-cracking concrete for assembly in the following embodiments is prepared from ordinary Portland cement, fly ash, sand, crushed stone, composite admixture, steel fiber and water, and the composite admixture is prepared from an early-strength component, an expansion agent, a water-reducing agent, a defoaming agent and a retarding component. Ordinary Portland cement is the main cementitious material, and fly ash is used to improve the durability of concrete. Sand and crushed stone are used as aggregates to increase the strength of concrete. The composite admixture includes an early-strength component to provide early strength, an expansion agent to compensate for the shrinkage deformation of concrete, a water-reducing agent to provide a longer construction time, a defoaming agent to reduce bubbles in concrete, and a retarding component to ensure that concrete has sufficient construction time. The modified nanomaterial is prepared from carbon nanotubes, nano silicon powder and nano titanium oxide, and the addition of carbon nanotubes, nano silicon powder and nano titanium oxide significantly improves the microstructure of concrete. The strengthening effect of the nanometer scale makes the concrete more compact and uniform at the molecular level, which helps to improve the overall strength and durability of the material. Through surface modification, these nanomaterials can better bond with the cement matrix, effectively transfer stress, reduce the formation of microcracks, and enhance early strength and crack resistance. High-performance polymer fibers can form a three-dimensional network in concrete, improve the toughness of concrete, and make it less prone to brittle fracture when subjected to load. The introduction of fibers can also effectively control plastic shrinkage cracks and shrinkage cracks during the hardening process of concrete, reducing the development of cracks. Organic microspheres, as lightweight aggregates in concrete, not only reduce the overall weight of concrete, but also act as filling materials on a microscopic scale to improve the density and impermeability of concrete. The addition of microspheres also improves the insulation and impact resistance of concrete, making concrete show better performance under special environments. In addition, steel fibers are introduced to improve the crack resistance of concrete. This freshly mixed early-strength crack-resistant concrete for assembly is a self-compacting concrete with good working performance, long construction time, high early strength, and excellent volume stability. Specifically, it has good working performance and long construction time, initial slump ≥270mm, initial slump expansion ≥680mm, 2h slump ≥250mm, 2h slump expansion ≥600mm, construction time ≥2h; high early strength, 12h compressive strength ≥40MPa; good volume stability, and small change in limiting expansion rate.
[0030] Preferably, the weight ratio of ordinary Portland cement, fly ash, sand, crushed stone, composite admixture, steel fiber and water is (480-530): (70-120): (750-830): (680-750): (60-110): (20-40): (180-195), and the weight ratio of early strength component, expansion agent, water reducer, defoamer, retarding component, modified nanomaterial, high performance polymer fiber and organic microsphere is (35-65): (18-38): (4-5): (0.9-1.8): (0.9-1.8): (2-8): (5-15): (3-10). By adopting these preferred weight ratios, it can be ensured that the amount of each component is within a suitable range. This helps to avoid excessive or insufficient use of materials, thereby ensuring that the performance of concrete reaches the best state.
[0031] Preferably, the early strength component includes a coagulant and an early strength agent, the expansion agent is a calcium-magnesium composite expansion agent, the water reducer is a polycarboxylate water reducer, and the retarding component includes sodium gluconate and sodium citrate. The early strength component is prepared by the coagulant and the early strength agent in a ratio of 5:1; the water reducer is a slow-release high-performance polycarboxylate water reducer with a water reduction rate of 28%; the defoamer is a polyether defoamer; the retarder is a mixture of sodium gluconate and sodium citrate in a ratio of 1:3; the coagulant and the early strength agent react chemically with water and cement particles to form calcium silicate hydrates, and the polycarboxylate water reducer interacts with ions in water to form surfactants, which helps to reduce the viscosity of the concrete and increase the construction time. This makes concrete easier to mix and construct, especially in assembly construction, which helps to improve construction efficiency. The action of the calcium-magnesium composite expansion agent is a multi-stage process. First, it reacts with water to form a colloidal substance of magnesium hydroxide and calcium hydroxide. These colloidal substances fill the micropores of the concrete and reduce the temperature and humidity sensitivity of the concrete. Then, during the concrete curing process, these substances continue to react with the moisture in the concrete, maintaining the volume stability of the concrete. This is very important for component connections in prefabricated construction, because the connection requirements may be different at different stages. For example, in the initial connection, it is necessary to ensure that the connection is tight, and over time, the connection still needs to be maintained firmly, which requires the concrete to be able to compensate for shrinkage in multiple stages. Due to the staged action of the calcium-magnesium composite expansion agent, it is suitable for concrete connections under different environmental conditions, including high temperature, low temperature and large humidity changes. This increases the applicability of the connection, especially in projects such as high-speed railway bridges, which may face various climatic and environmental challenges. Sodium gluconate and sodium citrate react with colloidal substances to form calcium gluconate and calcium citrate. The formation of calcium gluconate and calcium citrate can fill the micropores and pores inside the concrete, further enhancing the volume stability of the concrete. This is very critical for wet joints, because the stability of the connection requires that the concrete remain unchanged after the connection. This reaction also has a retarding effect, that is, it delays the solidification and hardening speed of the concrete. This is very beneficial for wet joints because it gives construction personnel enough time to arrange and adjust the connection parts to ensure the accuracy and quality of the connection. Furthermore, the calcium gluconate and calcium citrate produced help to reduce internal stresses in the concrete, reducing the risk of cracking. This is crucial for the durability and reliability of the connection, especially in high pressure and vibration environments.
[0032] Preferably, the organic microspheres are polystyrene microspheres. Polystyrene microspheres have an extremely low density, and their addition can significantly reduce the deadweight of concrete, which is particularly beneficial in prefabricated buildings that need to reduce structural loads.
[0033] Preferably, the high-performance polymer fiber is polyvinyl alcohol fiber. Polyvinyl alcohol fiber has excellent adhesion and chemical resistance, which significantly improves the crack resistance and durability of concrete. In early-strength concrete, the rapid development of compressive strength may be accompanied by shrinkage stress, and polyvinyl alcohol fiber can resist these stresses at the microscopic level and prevent the generation and expansion of cracks.
[0034] Furthermore, the present application discloses a method for preparing early-strength and crack-resistant concrete for assembly, comprising the following steps:
[0035] Step S100: performing surface modification treatment on carbon nanotubes, nano silicon powder and nano titanium oxide to obtain modified nano materials.
[0036] It is understood that surface modification is the process of changing the surface properties of nanomaterials by chemical or physical methods to make them more suitable for specific applications. In this step, surface modification not only improves the dispersion of nanomaterials and reduces agglomeration in the concrete matrix, but also increases their resistance to chemical attack, especially in alkaline environments. In addition, the stronger adhesion between the modified nanomaterials and the cement matrix reduces interfacial weaknesses, thereby reducing the formation and propagation of cracks.
[0037] Step S200: Mix the modified nanomaterial with the high-performance polymer fiber, and disperse them into the polymer matrix with the aid of ultrasonic technology to obtain a nanocomposite material.
[0038] It is understood that ultrasonic dispersion is a very effective nanomaterial processing technique that can improve the physical properties of materials without changing their chemical properties. In concrete applications, this step ensures uniform distribution of nanomaterials and good interfacial bonding,
[0039] Step S300, performing ion exchange and molecular level modification treatment on the early strength component, the expansion agent, the water reducing agent, the defoaming agent and the retarding component to obtain a composite admixture dry mix.
[0040] It is understood that ion exchange is the process of changing the ionic form of certain components in the admixture through specific ion exchange resins or other media, thereby optimizing the performance of these components in the cement matrix. Molecular level modification involves adding specific chemical substances (such as organosilicon compounds) to change the molecular structure of the admixture through chemical reactions to improve its effect in concrete. In this step, the ion exchange and molecular modification of the early strength component help accelerate the cement hydration reaction, allowing the concrete to obtain the required strength in a shorter time. The optimization of the expansive agent can more effectively control the volume change of the concrete and reduce cracks caused by shrinkage. The modification of the water reducer and defoamer can improve the fluidity and density of the concrete, and the adjustment of the retarding component ensures that the concrete has sufficient construction time.
[0041] Step S400: premixing ordinary Portland cement, fly ash and composite admixture dry mix, and then adding nanocomposite materials and polystyrene microspheres for stirring and mixing to obtain concrete premix.
[0042] It is understandable that the premixing process is not only a physical mixing process, but also provides a platform for possible chemical reactions between cement and admixtures, which can further develop during the concrete hardening process and improve the performance of the final product. The synergistic effect of nanocomposites and polystyrene microspheres significantly improves the crack resistance of concrete. Nanomaterials enhance the microstructure of concrete, while high-performance polymer fibers such as polyvinyl alcohol fibers provide an anti-crack network at the macro level, jointly counteracting the expansion of micro cracks and enhancing the overall durability and service life of assembled components.
[0043] Step S500: uniformly mix the steel fibers into the concrete premix, and obtain early-strength and crack-resistant concrete for assembly through staged mixing.
[0044] Understandably, steel fibers are selected to further enhance concrete’s crack resistance and toughness. By being evenly dispersed in the concrete matrix, steel fibers can effectively intercept and control the propagation of cracks, thereby improving the integrity of the concrete structure. At the same time, by providing an internal support structure, steel fibers help concrete demonstrate good load-bearing capacity at an early stage, which is crucial to accelerating the construction schedule. Staged mixing is a method of mixing after each new ingredient is added, which ensures that the materials are fully mixed each time, rather than mixing all the ingredients at once. This method helps avoid premature reactions or stratification between the ingredients.
[0045] It should be noted that step S100 includes step S110, step S120 and step S130.
[0046] Step S110, adding carbon nanotubes, nano silicon powder and nano titanium oxide into deionized water, and ultrasonically treating in a water bath at 30° C. for 3 minutes to obtain a nano suspension.
[0047] It is understandable that the high-frequency vibration of ultrasound can break up the aggregation of nanoparticles in water and promote them to form a more stable and uniform suspension. Through ultrasonic treatment, the activity of the nanoparticle surface is enhanced, which is conducive to the reaction with the coupling agent.
[0048] Step S120, adding the pre-proportioned silane coupling agent to the nano suspension, stirring evenly at room temperature, and ultrasonically treating for 5 minutes to obtain a modified mixture.
[0049] It is understood that silane coupling agents can form a modified layer on the surface of nanomaterials, improving their compatibility and dispersibility in the concrete matrix. Silane coupling agents improve the adhesion between nanoparticles and the cement matrix, increasing strength and durability. In addition, the modified layer formed by the coupling agent helps protect the nanoparticles and prevents them from reacting in an alkaline environment.
[0050] Step S130, placing the modified mixture into a dryer preheated to 100°C, spreading it evenly on a drying tray, and drying it continuously at a constant temperature for 4 hours, using a pulverizer to pulverize the dried material to obtain a modified nanomaterial.
[0051] It is understood that this step is to remove moisture from the mixture to ensure that the modified nanomaterial is dried. After drying, the material is crushed using a crusher to ensure the use effect and storage stability of the modified nanomaterial in concrete. Through drying and crushing, it is ensured that the modified nanomaterial is easy to store and mix into concrete.
[0052] It should be noted that step S200 includes step S210, step S220, step S230 and step S240.
[0053] Step S210, soaking the high-performance polymer fiber in deionized water at room temperature, and stirring the water at 200 rpm with a stirrer for 20 minutes to obtain wet fibers.
[0054] It is understood that in this step, the fibers are fully wetted and their bundled state is opened, which is to ensure that the fibers can be better integrated with the modified nanomaterials in the subsequent mixing step. The bonding force between the wet fibers and the modified nanomaterials and the cement matrix is enhanced, which is beneficial to improving the overall performance of the concrete.
[0055] Step S220, adding the wet fiber and the modified nanomaterial into the mixer, setting the stirring speed to 500 rpm, and continuously stirring at room temperature for 10 minutes to obtain a preliminary mixture.
[0056] It can be understood that through this step, the contact area between the fibers and the nanomaterials is maximized, ensuring that the fibers and nanomaterials are evenly distributed at the microscopic level, providing consistent reinforcement to the concrete.
[0057] Step S230, transferring the crude mixture to an ultrasonic processor, setting the ultrasonic frequency to 30 kHz, and performing the treatment for 20 minutes, maintaining the temperature not exceeding 40°C during the treatment, to obtain a nanocomposite mixture.
[0058] It is understood that the crude mixture is further processed in an ultrasonic processor to ensure that the nanomaterial is evenly dispersed in the fiber matrix. The high frequency vibration of the ultrasound helps to break up the agglomeration of the nanoparticles, further improving the uniformity of the mixture. The uniform distribution of the nanomaterial in the fiber matrix is improved, which is conducive to achieving more uniform mechanical properties. The processing temperature is kept at no more than 40°C to avoid damage to the fibers or nanomaterials due to high temperature processing.
[0059] Step S240: Use a vacuum dryer to dry the nanocomposite mixture at a temperature of 60° C. for 4 hours to obtain a nanocomposite material.
[0060] Understandably, the moisture content of the vacuum-dried nanocomposite is tightly controlled, which helps in precisely controlling the water-cement ratio when mixing concrete. The correct water-cement ratio is critical for the early hydration reaction and ultimate strength development of concrete. During the early hardening stage, the crack resistance and strength development of concrete are affected by the stability of the microstructure. Vacuum-dried nanocomposites ensure that no additional moisture or air is introduced during the hardening process, maintaining the homogeneity of the concrete.
[0061] It should be noted that step S300 includes step S310, step S320, step S330 and step S340.
[0062] Step S310: at room temperature, mix the early strength component, the expansion agent, the water reducing agent, the defoaming agent and the retarding component, and use a powder mixer to stir at 200 rpm for 15 minutes to obtain a dry mixture.
[0063] It is understood that by mixing in this way, the ideal mix can be achieved without adding excessive moisture, which is essential to maintain the early strength properties of concrete.
[0064] Step S320, subjecting the dry mixture to ion exchange reaction treatment in an ion exchange column for 2 hours to obtain a modified admixture dry mix.
[0065] It is understood that the treatment carried out in the ion exchange column improves the performance of specific components in the cementitious matrix by replacing the ions of these components in the admixture. The activity of the early strength components is enhanced by ion exchange, thereby accelerating the early strength development of concrete. Ion exchange of the expansive agent helps to control the volume stability of the concrete and reduce the formation of cracks.
[0066] Step S330, transferring the modified admixture dry mix to a reaction container, adding the organosilicon compound at a temperature of 50°C, and stirring in a constant temperature stirrer for 1 hour to obtain the modified admixture.
[0067] It is understood that the silane coupling agent improves the bonding strength between the admixture and the cement matrix, thereby enhancing the crack resistance of the concrete. The stability of the admixture is improved in the cement matrix, which is beneficial to the long-term durability of the concrete.
[0068] Step S340, drying the modified composite admixture in a vacuum drying oven at a temperature of 60° C. for 4 hours, and sieving the dried material to obtain a composite admixture dry mix.
[0069] It can be understood that drying the modified composite admixture avoids the introduction of additional moisture into the concrete, maintains the accuracy of the concrete mix ratio, and is conducive to the performance of early strength.
[0070] It should be noted that step S400 includes step S410, step S420, step S430 and step S440.
[0071] Step S410: ordinary Portland cement and fly ash are mixed, and stirred at a speed of 100 rpm at room temperature for about 5 minutes to obtain a basic mixture.
[0072] It is understandable that the purpose of mixing ordinary Portland cement with fly ash is to utilize the admixture effect of fly ash, which not only improves the workability and final hardening properties of concrete, but also utilizes the secondary hydration reaction of fly ash to increase the later strength of concrete and improve its early crack resistance.
[0073] Step S420, adding the composite admixture dry mix to the basic mix and stirring at 150 rpm for 10 minutes to obtain a cement-based premix.
[0074] It is understood that the purpose of mixing the composite admixture dry mix with the base mix in this step is to evenly distribute the admixture in the cement matrix, which is crucial for adjusting and optimizing the early properties of concrete such as pumpability, slump and ultimate strength and durability.
[0075] Step S430: adding the nanocomposite material to the cement-based premix, and stirring the mixture at a speed of 200 rpm using a high shear mixer for 20 minutes to obtain a cement-based nanocomposite premix.
[0076] It is understood that in this step, the nanocomposite material is added to the cement-based premix and stirred using a high shear mixer to ensure uniform distribution of the nanomaterial. The uniform distribution of the nanomaterial enhances the microstructure of the concrete and improves its compressive strength and crack resistance.
[0077] Step S440: Add polystyrene microspheres into the cement-based nanocomposite premix, adjust the stirring speed to 60 rpm, and stir for 5 minutes to obtain a concrete premix.
[0078] It can be understood that adding polystyrene microspheres to concrete can not only serve as lightweight aggregates to reduce the density of concrete, but the elasticity of the polystyrene microspheres helps to absorb impact energy and reduce the formation of cracks.
[0079] In order to further understand the present application, the early-strength anti-cracking concrete for assembly and the preparation method thereof provided by the present invention are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0080] Embodiment 1:
[0081] An early-strength anti-cracking concrete for assembly is made of the following raw materials in parts by weight:
[0082] The composite material is prepared from 500 parts of ordinary Portland cement, 100 parts of fly ash, 795 parts of sand, 730 parts of 5-16 mm crushed stone, 50 parts of early strength component, 20 parts of expansion agent, 5 parts of water reducer, 1 part of defoaming agent, 1 part of retarding component, 20 parts of steel fiber, 180 parts of water, 8 parts of modified nanomaterials, 10 parts of high-performance polymer fibers and 5 parts of organic microspheres.
[0083] The preparation method of early-strength anti-cracking concrete for assembly includes the following steps:
[0084] (1) Weigh the raw materials by weight, first pour ordinary Portland cement, fly ash, sand, 5-16 mm crushed stone, modified nanomaterials, high-performance polymer fibers, organic microspheres and composite admixtures into a mixer and mix them evenly for 60 seconds;
[0085] (2) Pour water into the mixer and stir for 120 seconds to obtain fresh concrete;
[0086] (3) Pour the steel fibers into a mixer and stir for 120 seconds to obtain freshly mixed early-strength and crack-resistant concrete for assembly.
[0087] (4) Pour the obtained freshly mixed early-strength and crack-resistant concrete into the prepared mold for molding. During the molding process, no vibration is required, and only compaction and smoothing are required.
[0088] Embodiment 2:
[0089] Different from Example 1, the early-strength and crack-resistant concrete for assembly is prepared from 500 parts of ordinary Portland cement, 90 parts of fly ash, 795 parts of sand, 730 parts of 5-16 mm crushed stone, 50 parts of early-strength component, 30 parts of expansion agent, 5 parts of water reducer, 1 part of defoaming agent, 1 part of retarding component, 20 parts of steel fiber, 180 parts of water, 8 parts of modified nanomaterials, 10 parts of high-performance polymer fibers, and 5 parts of organic microspheres.
[0090] Embodiment 3:
[0091] Different from Example 1, the prefabricated early-strength anti-cracking concrete is prepared from 500 parts of ordinary Portland cement, 80 parts of fly ash, 795 parts of sand, 730 parts of 5-16 mm crushed stone, 50 parts of early-strength component, 40 parts of expansion agent, 5 parts of water reducer, 1 part of defoamer, 1 part of retarding component, 20 parts of steel fiber, 180 parts of water, 8 parts of modified nanomaterials, 10 parts of high-performance polymer fibers, and 5 parts of organic microspheres.
[0092] Embodiment 4:
[0093] Different from Example 2, the early strength and crack resistance concrete for assembly is prepared from 500 parts of ordinary Portland cement, 90 parts of fly ash, 795 parts of sand, 720 parts of 5-16 mm crushed stone, 50 parts of early strength component, 30 parts of expansion agent, 5.2 parts of water reducer, 1 part of defoamer, 1 part of retarding component, 30 parts of steel fiber, 183 parts of water, 8 parts of modified nanomaterials, 10 parts of high-performance polymer fibers, and 5 parts of organic microspheres. Compared with Example 2, it is necessary to increase the appropriate amount of water reducer and water by weight to achieve the required working performance.
[0094] Embodiment 5:
[0095] Different from Example 2, the early-strength anti-cracking concrete for assembly is prepared from 500 parts of ordinary Portland cement, 90 parts of fly ash, 795 parts of sand, 710 parts of 5-16 mm crushed stone, 50 parts of early-strength component, 30 parts of expansion agent, 5.5 parts of water reducer, 1 part of defoamer, 1 part of retarding component, 40 parts of steel fiber, 185 parts of water, 8 parts of modified nanomaterials, 10 parts of high-performance polymer fibers, and 5 parts of organic microspheres. Compared with Example 2, it is necessary to increase the appropriate amount of water reducer and water by weight to achieve the required working performance.
[0096] The early-strength anti-cracking concrete for assembly prepared in the above Examples 1 to 5 was tested for performance according to the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T 50080), the Standard for Test Methods for Mechanical Properties of Ordinary Concrete (GB / T 50081) and the Concrete Expansion Agent (GB / T 23439). The results are as follows:
[0097] Table 1 Working performance of freshly mixed early strength crack resistant concrete
[0098] Example <![CDATA[T 50 (s)]]> Slump expansion (mm) 1 5.1 725 2 5.3 718 3 5.4 701 4 5.7 722 5 6.2 714
[0099] Table 2 Compressive strength of early-strength anti-cracking concrete for assembly
[0100] Example 12h compressive strength / MPa 28d compressive strength / MPa 56d compressive strength / MPa 1 44.3 70.3 76.5 2 45.1 71.2 77.3 3 44.6 70.6 78.7 4 48.7 75.1 81.6 5 49.2 78.7 82.3
[0101] The following conclusions can be drawn from Table 1:
[0102] 1. From the comparison of Example 1, Example 2, and Example 3 in Table 1, it can be seen that different weight portions of expansive agents have little effect on the working performance of freshly mixed early-strength anti-cracking concrete. This is because although the increase in the amount of expansive agent will increase the viscosity of the concrete to a certain extent, resulting in an increase in the time T50 when the expansion reaches 500mm, and the slump expansion will also decrease, the expansive agent will not significantly change the yield stress of the freshly mixed concrete, and its influence does not play a decisive role in the working performance of the concrete. However, when used in combination with modified nanomaterials, the microstructure and early strength of the concrete can be improved without significantly increasing the viscosity, because the nanomaterials help fill the pores and provide better intergranular bonding.
[0103] 2. By comparing Example 2, Example 4, and Example 5, it can be seen that as the amount of steel fiber increases, it is necessary to appropriately increase the water reducer and water to achieve the desired self-compacting performance. The time T50 for the expansion to reach 500 mm in Table 1 also increases with the increase in the amount of steel fiber. This is because the addition of steel fiber will significantly increase the yield stress of fresh concrete, resulting in a decrease in the working performance of fresh concrete. Increasing the water reducer and water can reduce the yield stress of fresh concrete to a certain extent and improve the working performance. At the same time, the increase in the amount of steel fiber can effectively improve the compressive strength of concrete at different ages. This strengthening effect is further enhanced by adding organic microspheres, because the microspheres can improve the overall structural performance of concrete, while reducing weight and increasing the absorption of impact energy, thereby reducing microcracks caused by volume changes.
[0104] The following conclusions can be drawn from Table 2:
[0105] Table 2 Compressive strength of early-strength anti-cracking concrete for assembly The results show that the change in the amount of expansion agent has little effect on the compressive strength of concrete at different ages, while the increase in the amount of steel fiber can effectively improve the compressive strength of concrete at different ages. This is because the addition of steel fiber constrains the volume change of concrete during compression, delays the destruction of concrete, and is beneficial to improving compressive performance.
[0106] Figure 1The following is a test chart of the limited expansion rate of Example 1, Example 2, and Example 3 with different expansion agent dosages cured in water for 14 days. The results show that the limited expansion rate of prefabricated early-strength anti-cracking concrete shows a trend of continuous expansion during the curing period in water, and the higher the expansion agent dosage, the greater the expansion rate. The limited expansion rates of Example 1, Example 2, and Example 3 in water for 14 days are 2.9×10-4, 3.4×10-4, and 3.7×10-4, respectively, which meet the standard requirement of ≥2.5×10-4.
[0107] Figure 2 The following is a test diagram of the limited expansion rate of Example 1, Example 2, and Example 3 with different expansion agent dosages after curing in water for 14 days and then curing in the air for 28 days. The results show that the early-strength anti-cracking concrete for assembly shows a state of continuous shrinkage during curing in the air, and the shrinkage is relatively smaller when the expansion agent dosage is higher. This is because the expansion agent can compensate for the shrinkage of concrete to a certain extent. At the same time, modified nanomaterials such as nano-silicon powder and nano-titanium oxide enhance the early hydration reaction of concrete by filling the microscopic space of the cement matrix and providing higher interfacial activity. The addition of high-performance polymer fibers such as polyvinyl alcohol enhances the crack resistance and impact resistance by improving the flexibility and tensile properties of concrete. These fibers also help to reduce the internal stress caused by shrinkage, thereby reducing the formation of cracks. Organic microspheres absorb part of the internal stress generated during the curing process through their excellent elastic quality, reducing the risk of cracks. The restricted expansion rates of Example 1, Example 2 and Example 3 after being cultured in water for 14 days and then transferred to air for 28 days were -1.3×10-4, -1.1×10-4 and -1.0×10-4 respectively, meeting the standard requirement of ≥-2.0×10-4.
[0108] Figure 3 The following is a test chart of the limited expansion rate of Example 2, Example 4, and Example 5 with different steel fiber dosages after curing in water for 14 days. The results show that as the steel fiber dosage increases, the limited expansion rate becomes smaller. This is because steel fibers can significantly improve the tensile and shear properties of concrete and improve the volume stability of concrete. The addition of high-performance polymer fibers and organic microspheres further enhances this effect. High-performance polymer fibers increase the toughness and ductility of concrete, while organic microspheres provide additional spatial stability, which together reduce stress concentration caused by volume changes. The limited expansion rates of Example 2, Example 4, and Example 5 in water for 14 days are 3.4×10-4, 2.9×10-4, and 2.4×10-4, respectively, and do not meet the standard requirement of ≥2.5×10-4 when using 40kg of steel fiber.
[0109] Figure 4The following is a test chart of the limited expansion rate of Example 2, Example 4, and Example 5 with different steel fiber dosages after curing in water for 14 days and then in the air for 28 days. The results show that the higher the steel fiber dosage, the smaller the shrinkage of the early-strength anti-cracking concrete for assembly. The limited expansion rates of Example 2, Example 4, and Example 5 after curing in water for 14 days and then in the air for 28 days were -1.1×10-4, -0.8×10-4, and -0.7×10-4, respectively, meeting the standard requirement of ≥-2.0×10-4.
[0110] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0111] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. An early-strength anti-cracking concrete for assembly, characterized in that: The composite admixture is prepared from ordinary Portland cement, fly ash, sand, crushed stone, composite admixture, steel fiber and water, wherein the composite admixture is prepared from early strength component, expansion agent, water reducing agent, defoaming agent, retarding component, modified nanomaterial, high-performance polymer fiber and organic microsphere, and the modified nanomaterial is prepared from carbon nanotube, nano silicon powder and nano titanium oxide; Wherein, the weight ratio of the ordinary Portland cement, the fly ash, the sand, the crushed stone, the composite admixture, the steel fiber and the water is (480-530): (70-120): (750-830): (680-750): (60-110): (20-40): (180-195), and the weight ratio of the early strength component, the expansion agent, the water reducer, the defoamer, the retarding component, the modified nanomaterial, the high-performance polymer fiber and the organic microsphere is (35-65): (18-38): (4-5): (0.9-1.8): (0.9-1.8): (2-8): (5-15): (3-10); The early strength component comprises a setting accelerator and an early strength agent, the expansion agent is a calcium-magnesium composite expansion agent, the water reducer is a polycarboxylate water reducer, the retarding component comprises sodium gluconate and sodium citrate, the setting accelerator and the early strength agent react chemically with water and cement particles to generate calcium silicate hydrate, the polycarboxylate water reducer interacts with ions in water to form a surfactant, the calcium-magnesium composite expansion agent reacts with water to generate a colloidal substance, the colloidal substance comprises magnesium hydroxide and calcium hydroxide, the colloidal substance fills the micropores inside the concrete, and the sodium gluconate and the sodium citrate react with the colloidal substance to generate calcium gluconate and calcium citrate.
2. The early-strength anti-cracking concrete for assembly according to claim 1, characterized in that: The organic microspheres are polystyrene microspheres.
3. The early-strength anti-cracking concrete for assembly according to claim 1, characterized in that: The high performance polymer fiber is polyvinyl alcohol fiber.
4. A method for preparing the early-strength anti-cracking concrete for assembly as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: Performing surface modification on carbon nanotubes, nano silicon powder and nano titanium oxide to obtain modified nano materials; The modified nanomaterial is mixed with high-performance polymer fibers, and dispersed into a polymer matrix using ultrasonic technology to obtain a nanocomposite material; The early strength component, the expansion agent, the water reducing agent, the defoaming agent and the retarding component are subjected to ion exchange and molecular level modification to obtain a composite admixture dry mix; Premixing ordinary Portland cement, fly ash and the composite admixture dry mix, and then adding the nanocomposite material and polystyrene microspheres for stirring and mixing to obtain a concrete premix; The steel fibers are uniformly mixed into the concrete premix, and the early-strength anti-cracking concrete for assembly is obtained through staged mixing.
5. The method for preparing the early-strength anti-cracking concrete for assembly according to claim 4, characterized in that: The surface of carbon nanotubes, nano silicon powder and nano titanium oxide is modified to obtain modified nano materials, including: The carbon nanotubes, nano-silicon powder and nano-titanium oxide were added to deionized water and ultrasonically treated in a water bath at 30°C for 3 minutes to obtain a nano suspension; Adding the pre-proportioned silane coupling agent to the nanosuspension, stirring evenly at room temperature, and ultrasonically treating for 5 minutes to obtain a modified mixture; The modified mixture was placed in a dryer preheated to 100° C., spread evenly on a drying tray, and dried continuously at a constant temperature for 4 hours. The dried material was crushed using a crusher to obtain a modified nanomaterial.
6. The method for preparing the early-strength anti-cracking concrete for assembly according to claim 4, characterized in that: The modified nanomaterial is mixed with high-performance polymer fibers, and dispersed into a polymer matrix using ultrasonic technology to obtain a nanocomposite material, including: The high-performance polymer fiber was immersed in deionized water at room temperature and stirred at 200 rpm for 20 minutes using a stirrer to obtain a wet fiber; Add the wet fiber and the modified nanomaterial into a mixer, set the stirring speed to 500 rpm, and continue stirring at room temperature for 10 minutes to obtain a preliminary mixture; The crude mixture was transferred to an ultrasonic processor, the ultrasonic frequency was set to 30 kHz, and the treatment was performed for 20 minutes, and the temperature was maintained at no more than 40° C. during the treatment, to obtain a nanocomposite mixture; The nanocomposite mixture was dried in a vacuum dryer at 60° C. for 4 hours to obtain a nanocomposite material.
7. The method for preparing the early-strength anti-cracking concrete for assembly according to claim 4, characterized in that: The early strength component, expansion agent, water reducing agent, defoamer and retarding component are subjected to ion exchange and molecular level modification to obtain a composite admixture dry mix, including: At room temperature, the early strength component, the expansion agent, the water reducing agent, the defoaming agent and the retarding component are mixed and stirred at 200 rpm for 15 minutes using a powder mixer to obtain a dry mixture; The dry mixture is subjected to an ion exchange reaction treatment in an ion exchange column for 2 hours to obtain a modified admixture dry mix; The modified admixture dry mix is transferred to a reaction container, an organosilicon compound is added at a temperature of 50° C., and stirred in a constant temperature stirrer for 1 hour to obtain a modified composite admixture; The modified composite admixture is dried in a vacuum drying oven at 60° C. for 4 hours, and the dried material is sieved to obtain a composite admixture dry mix.
8. The method for preparing the early-strength anti-cracking concrete for assembly according to claim 4, characterized in that: Ordinary Portland cement, fly ash and the composite admixture dry mix are premixed, and then the nanocomposite material and polystyrene microspheres are added and stirred to obtain a concrete premix, comprising: Ordinary Portland cement and fly ash are mixed and stirred at a speed of 100 rpm at room temperature for about 5 minutes to obtain a basic mixture; Adding the composite admixture dry mix to the base mix and stirring at 150 rpm for 10 minutes to obtain a cement-based premix; Adding the nanocomposite material to the cement-based premix, stirring the mixture at a speed of 200 rpm using a high shear mixer for 20 minutes to obtain a cement-based nanocomposite premix; The polystyrene microspheres were added into the cement-based nanocomposite premix, the stirring speed was adjusted to 60 rpm, and the mixture was stirred for 5 minutes to obtain a concrete premix.