A functional phosphate-based water reducer, superplasticizer, and preparation method and application thereof

Through nanohybrid technology of functional phosphate-based water reducing agent, hydrophobic carbon nanomaterials and magnesium-aluminum layered double metal hydroxide, the problem of dispersion of hydrophobic nanomaterials in high-alkali and high-salt environments is solved, and cement-based materials are realized. The early strength improvement and later toughening effect improve the overall performance.

CN117700655BActive Publication Date: 2024-10-22江苏博思通新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311524371.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2024-10-22
Estimated Expiration
2043-11-16

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively disperse hydrophobic nanomaterials in high-alkali and high-salt environments, which limits its toughening effect in cement-based materials, and it is difficult to balance early strength improvement with later strength development.

Method used

Functional phosphate-based water reducing agent is used with hydrophobic carbon nanomaterials and magnesium-aluminum layered double metal hydroxide to form a stable nanohybrid structure through nanohybridization, which promotes cement hydration and improves the early and early life of cement-based materials. Late intensity.

Benefits of technology

It achieves both early strength improvement and later toughening effect in cement-based materials, ensures good dispersion performance of hydrophobic carbon nanomaterials in high-alkali and high-salt environments, and improves the overall performance of cement-based materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a functional phosphate-based water reducer, a superplasticizer, and a preparation method and application thereof. The functional phosphate-based water reducer is formed by polycondensation of a polyether macromonomer, a polyether phosphate ester monomer, a hydrophobic soft and hard block macromonomer, and an aldehyde monomer, and the first three monomers are connected by an aldehyde monomer. The superplasticizer is mainly obtained by nano-hybridization of the functional phosphate-based water reducer, a hydrophobic carbon nanomaterial, and a magnesium-aluminum layered double metal hydroxide (LDH). The phosphate-based nano-hybrid superplasticizer of the present invention can be used alone, or it can be used in combination with aminosulfonic acid-based water reducers, polycarboxylic acid water reducers, etc. on the market. At the same time, it can also be added with air entraining agents, retarders, thickening and water-retaining agents, retarders, and defoamers for compound use, which can achieve early strength and toughening effects in cement-based materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete admixtures, and specifically relates to a functional phosphate-based water reducer, a superplasticizer, and a preparation method and application thereof. Background Art

[0002] With the construction of infrastructure, polycarboxylic acid system water reducers have been widely used in engineering projects such as water conservancy, high-speed rail, tunnels, bridges, and nuclear power, but more requirements have been put forward for their performance. For example, many large-scale projects require that the early strength of concrete can meet the design requirements. For example, the strength of concrete develops slowly in the low temperature environment in winter. How to avoid the influence of inorganic salt early strength agents on its working performance, long-term mechanical properties and durability, and effectively improve its early strength, is a research hotspot that scholars at home and abroad continue to pay attention to. For another example, precast concrete needs to be cured at high temperature for a long time and can only be demolded after reaching the expected strength. How to reduce the steam curing time and improve the mold turnover efficiency is a key technical problem facing the production of precast concrete. At the same time, a large number of mineral admixtures are applied to concrete to improve the degree of concrete's resistance to environmental erosion. However, most of the mineral admixtures will significantly reduce the early mechanical properties of concrete, affecting its wider application in the field of building materials.

[0003] In recent years, with the development of nanotechnology, new ideas have been provided for the field of concrete admixtures. The small size and high specific surface area of ​​nanomaterials make them have a great influence on the performance of cement-based materials at a lower dosage. The hybridization of nanomaterials and water reducers can effectively improve the performance of cement-based materials. For example, the early strength of cement is provided by hydrated calcium silicate gel. Existing studies have shown that nano-scale calcium silicate can provide nucleation sites in cement paste, thereby greatly promoting the nucleation growth of hydrated calcium silicate gel, and the early strength of cement-based materials can be greatly improved. Patent CN112979204B introduces a magnesium-doped calcium silicate nucleus early strength agent with long-term stability and its preparation method. By introducing magnesium ions into the structure of silicate polymers, a stable calcium silicate nucleus early strength agent is obtained, which can improve the early strength of cement. Patent CN108178549B introduces a method for preparing a composite super-early strength admixture, which is composed of a POSS-based star-shaped block polycarboxylate water-reducing agent, a soluble calcium salt and a soluble silicate. It can not only improve the early strength of cement materials, but also has a high water reduction rate, does not affect the later strength of concrete, and also reduces the transportation cost of the early strength agent. The above reports all use polycarboxylate water-reducing agents to disperse hydrophilic nanomaterials such as nano calcium silicate. However, there are few reports on the composite hybridization of water-reducing agents and hydrophobic nanomaterials. Research reports show that carbon nanomaterials such as carbon nanotubes and graphene can often significantly improve the strength of cement-based materials at a relatively small dosage. However, these carbon nanomaterials are difficult to disperse in a high-alkali and high-salt environment due to their high hydrophobicity, thereby limiting their toughening effect in cement-based materials and even potentially leading to a decrease in performance. Therefore, how to effectively disperse hydrophobic nanomaterials in cement paste has become a current research difficulty. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a functional phosphate-based water reducer, a superplasticizer and a preparation method and application thereof. The superplasticizer can not only improve the early strength of cement-based materials, but also has a toughening effect on the later strength development of concrete.

[0005] Technical solution: In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a functional phosphate-based water reducer, whose molecular structure is a random copolymerized comb-shaped structure, wherein the functional phosphate-based water reducer is polycondensed by structural units A1, B1, C1, and D1, wherein the structural units A1, B1, and C1 are connected by D1, and the structural formula of the structural units A1, B1, C1, and D1 is shown in (I):

[0007]

[0008] (I)

[0009] Wherein, r is an integer of 90 to 120, s is an integer of 4 to 8, t is an integer of 10 to 40, and m is an integer of 0 to 15; R1 is a bicyclic or monocyclic C6-C10 aromatic group; and R2 is H or a C1-C3 alkyl group.

[0010] Preferably, R1 is phenyl, α-naphthyl or β-naphthyl, and R2 is H or methyl.

[0011] In a second aspect, the present invention provides a method for preparing the functional phosphate-based water reducer, comprising the following steps:

[0012] The polyether macromonomer A, the polyether phosphate monomer B, and the hydrophobic soft and hard block macromonomer C are melted under inert gas conditions, and then the temperature is raised to the reaction temperature, an acid catalyst and an aldehyde monomer D are added, and the reaction is refluxed at normal pressure. After the reaction is completed, the temperature is lowered to obtain a phosphoric acid-based water reducer;

[0013] The polyether macromonomer A is a phenol polyether monomer, which is obtained by the addition of phenol or phenoxyethanol and ethylene oxide, and can be prepared according to the method described in the public literature or patents; its structural formula is shown in (II):

[0014]

[0015] (II)

[0016] In the formula, r has the same definition as in formula (I).

[0017] The polyether phosphate monomer B is prepared by modifying phenol polyether through phosphorylation reaction, and can be prepared according to the method described in the public literature or patents; its structural formula is shown as (III):

[0018]

[0019] (III)

[0020] In the formula, s is defined the same as in formula (I).

[0021] The hydrophobic soft and hard block macromonomer C is obtained by sequentially adding phenol or phenoxyethanol to propylene oxide, phenyl or naphthyl substituted glycidyl ether, and can be prepared according to the method described in the public literature or patents; its structural formula is shown in (IV):

[0022] (IV)

[0023] In the formula, t, m, and R1 are defined the same as in formula (I).

[0024] The aldehyde monomer D has a structural formula as shown in (V), and can be selected from any one of formaldehyde, paraformaldehyde and acetaldehyde:

[0025] or

[0026] (V)

[0027] The definition of R2 is the same as in formula (I), and n=8-15.

[0028] As a specific implementation scheme, the melting is carried out at 80-90°C, the reaction temperature is 120-140°C, and the reflux reaction is carried out at normal pressure for 4-8 hours.

[0029] As a specific implementation scheme, the molar ratio of the polyether macromonomer A, polyether phosphate monomer B, hydrophobic soft and hard block macromonomer C and aldehyde monomer D is a:b:c:d, wherein a:b:c=1:1~4:1~1.5, (a+b+c):d=1.045~1.45:1;

[0030] Preferably, the acid catalyst is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or a combination of two of them in any proportion, and its usage is 0.5-3% of the total mass of monomer A, monomer B, monomer C, and monomer D.

[0031] In a third aspect, the present invention provides a phosphate-based nano-hybrid superplasticizer, which is made from the above-mentioned functional phosphate-based water reducer.

[0032] As an implementation scheme, the phosphate-based nano-hybrid superplasticizer is mainly obtained by nano-hybridization of the functional phosphate-based water reducer, hydrophobic carbon nanomaterial, and magnesium-aluminum layered double hydroxide (LDH).

[0033] In a fourth aspect, the present invention provides a method for preparing the phosphate-based nano-hybrid superplasticizer, comprising the following steps:

[0034] The functional phosphate-based water reducer and the hydrophobic carbon nanomaterial G are dissolved in water to prepare a stable and uniform solution; under certain temperature conditions, the pH value is adjusted, and under stirring conditions, a soluble magnesium salt H aqueous solution, a soluble aluminum salt I aqueous solution and an alkaline solution J are added dropwise at a uniform speed at the same time. After the addition is completed, the solution is kept warm to obtain the phosphate-based nano hybrid superplasticizer.

[0035] Preferably, the method for preparing the stable and uniform solution comprises: performing high-speed mixing and stirring for 25-35 minutes at 30-50°C, and ultrasonic treatment for 8-12 minutes to form a stable and uniform solution; adjusting the pH value under certain temperature conditions is to adjust the pH value to 9±1 with ammonia water at 50-80°C; the dripping time is 2-10 hours, and after the dripping is completed, keeping warm for 2-5 hours.

[0036] Preferably, the weight average molecular weight of the functional phosphate-based water reducer is in the range of 20,000 to 100,000; if the weight average molecular weight is too large or too small, the dispersibility of the water reducer will be deteriorated.

[0037] Preferably, the hydrophobic carbon nanomaterial G is selected from any one of graphene and carbon nanotubes or a combination of the two in any proportion;

[0038] Preferably, the soluble magnesium salt H is selected from any one of magnesium nitrate and magnesium sulfate or a combination of the two in any proportion;

[0039] Preferably, the soluble aluminum salt I is selected from any one of aluminum nitrate and aluminum sulfate or a combination of the two in any proportion;

[0040] Preferably, the alkaline solution J is selected from any one of sodium hydroxide and potassium hydroxide or a combination of the two in any proportion.

[0041] Preferably, the mass concentration of the functional phosphate-based water reducer in the phosphate-based nano hybrid superplasticizer is 5-15% (i.e., the mass of the functional phosphate-based water reducer accounts for the mass percentage of the superplasticizer solution finally prepared), and the mass ratio of the functional phosphate-based water reducer, the hydrophobic carbon nanomaterial G, and the magnesium-aluminum layered double metal hydroxide is f:g:h, wherein f:g:h is 1:0.4-0.8:0.5-1;

[0042] Preferably, the soluble magnesium salt H, the soluble aluminum salt I, and the alkaline solution J are used to prepare the magnesium aluminum layered double hydroxide in a molar ratio of x:y:z, wherein the molar ratio of x:y is 5:1-2:1, and 2x+3y=z should be satisfied.

[0043] In a fifth aspect, the present invention provides an application of the phosphate-based nano-hybrid superplasticizer, specifically: the phosphate-based nano-hybrid superplasticizer is used as an admixture for cement-based materials.

[0044] The phosphate-based nano hybrid superplasticizer of the present invention can be used alone or in combination with aminosulfonic acid-based water reducers, polycarboxylic acid water reducers, etc. on the market. It can also be added with air entraining agents, retarders, thickening and water-retaining agents, retarders and defoamers for compounding.

[0045] Beneficial effects: Compared with the prior art, the phosphate-based nano-hybrid superplasticizer of the present invention can achieve early strength and toughening effects in cement-based materials in the following way: (1) The hydrophilic long side chains (molecular weight ≥ 4000) in the structure of the functional phosphate-based water-reducing agent have an early strength effect; (2) The functional phosphate-based water-reducing agent and the magnesium-aluminum layered double metal hydroxide form a stable nano-hybrid structure, which can induce and accelerate cement hydration, thereby achieving an early strength effect; (3) The soft and hard block hydrophobic side chains in the structure of the functional phosphate-based water-reducing agent can be well combined with the hydrophobic carbon nanomaterial, so that the hydrophobic carbon nanomaterial has a better dispersion effect in high-alkali and high-salt cement paste, which has a promoting effect on improving the later toughening of cement-based materials. DETAILED DESCRIPTION

[0046] The present invention is described in detail below by examples, which are merely illustrative and do not limit the scope of application of the present invention. According to the disclosure herein, those skilled in the art can change the reagents, catalysts and reaction process conditions within the scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

[0047] The present invention provides a phosphate-based nano-hybrid superplasticizer with both early strength and toughening effects, which is obtained by nano-hybridization of functional phosphate-based water reducer, hydrophobic carbon nanomaterial, and magnesium-aluminum layered double hydroxide (LDH). The specific steps are:

[0048] (1) Preparation of functional phosphate-based water reducer F: polyether macromonomer A, polyether phosphate monomer B, and hydrophobic soft and hard block macromonomer C are placed in a reaction vessel under nitrogen protection, heated to 80-90°C, stirred evenly after melting, then heated to 120-140°C, acid catalyst E and aldehyde monomer D are added, refluxed at normal pressure for 4-8 hours, and after the reaction is completed, slowly cooled to room temperature to obtain a solid phosphate-based water reducer.

[0049] (2) Preparation of phosphate-based nano-hybrid superplasticizer: functional phosphate-based water reducer F and hydrophobic carbon nanomaterial G are dissolved in a certain amount of water, and mixed and stirred at high speed for 30 min at 30-50 °C, and ultrasonically treated for 10 min to form a stable and uniform solution; at 50-80 °C, the pH value is adjusted to about 9 with ammonia water, and the above solution is continuously stirred. At the same time, a soluble magnesium salt H aqueous solution, a soluble aluminum salt I aqueous solution and an alkaline solution J are uniformly added dropwise for 2-10 h. After the addition is completed, the solution is kept warm for 2-5 h to obtain a phosphate-based nano-hybrid superplasticizer.

[0050] The raw materials used in the examples are listed in Table 1, as follows:

[0051] Table 1 Compound codes in the synthetic examples

[0052]

[0053]

[0054] The information of the functional phosphate-based water reducer F in the embodiment is listed in Table 2, as follows:

[0055] Table 2 Functional phosphate-based water reducer information

[0056]

[0057] The information of the phosphate-based nano-hybrid superplasticizer in the embodiment is listed in Table 3, as follows:

[0058] Table 3 Phosphate-based nano-hybrid superplasticizer information

[0059]

[0060] Example 1

[0061] (1) Preparation of functional phosphate-based water reducer F-1: 1 mol of polyether macromonomer A-1, 1 mol of polyether phosphate monomer B-3, and 1 mol of hydrophobic soft and hard block macromonomer C-1 were placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, and then heated to 120°C. Acid catalyst E-1 (3% of the total mass of monomers A, B, C, and D) and 2.86 mol of aldehyde monomer D-1 were added, and refluxed at normal pressure for 4 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0062] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-1 and 4 parts by weight of hydrophobic carbon nanomaterial G-1 were dissolved in 70 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 30°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution. At 50°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 7.61 parts by weight of a soluble magnesium salt H-1 aqueous solution, 5.47 parts by weight of a soluble aluminum salt I-1 aqueous solution and 7.19 parts by weight of an alkaline solution J-1 were uniformly added dropwise for 2 hours. After the addition was completed, the mixture was kept warm for 2 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0063] Example 2

[0064] (1) Preparation of functional phosphate-based water reducer F-2: 1 mol of polyether macromonomer A-2, 2 mol of polyether phosphate monomer B-1, and 1.1 mol of hydrophobic soft and hard block macromonomer C-3 were placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, and then heated to 130°C. Acid catalyst E-2 (2.5% of the total mass of monomers A, B, C, and D) and 2.93 mol of aldehyde monomer D-1 were added, and refluxed at normal pressure for 6 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0065] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-2 and 8 parts by weight of hydrophobic carbon nanomaterial G-2 were dissolved in 30 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 40°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 60°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 16.56 parts by weight of a soluble magnesium salt H-1 aqueous solution, 7.65 parts by weight of a soluble aluminum salt I-2 aqueous solution and 14.30 parts by weight of an alkaline solution J-1 were uniformly added dropwise for 5 hours. After the addition was completed, the mixture was kept warm for 4 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0066] Example 3

[0067] (1) Preparation of functional phosphate-based water reducer F-3: 1 mol of polyether macromonomer A-3, 3 mol of polyether phosphate monomer B-3, and 1.3 mol of hydrophobic soft and hard block macromonomer C-2 were placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, and then heated to 140°C. Acid catalyst E-3 (1% of the total mass of monomers A, B, C, and D) and 4.08 mol of aldehyde monomer D-2 were added, and refluxed at normal pressure for 8 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0068] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-3 and 6 parts by weight of hydrophobic carbon nanomaterial G-1 were dissolved in 16.67 parts by weight of water, and mixed and stirred at high speed for 30 minutes at 50°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 80°C, the pH value was adjusted to about 9 with ammonia water, and the above solution was continuously stirred, and 8.73 parts by weight of soluble magnesium salt H-2 aqueous solution, 8.27 parts by weight of soluble aluminum salt I-2 aqueous solution and 11.60 parts by weight of alkaline solution J-1 were uniformly added dropwise at a uniform speed for 10 hours. After the addition was completed, the solution was kept warm for 5 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0069] Example 4

[0070] (1) Preparation of functional phosphate-based water reducer F-4: 1 mol of polyether macromonomer A-2, 4 mol of polyether phosphate monomer B-2, and 1.5 mol of hydrophobic soft and hard block macromonomer C-4 were placed in a reaction vessel under nitrogen protection, heated to 90°C, stirred evenly after melting, and then heated to 125°C. Acid catalyst E-4 (0.5% of the total mass of monomers A, B, C, and D) and 5.2 mol of aldehyde monomer D-3 were added, and refluxed at normal pressure for 5 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0071] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-4 and 5 parts by weight of hydrophobic carbon nanomaterial G-2 were dissolved in 60 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 50°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 70°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 13.92 parts by weight of a soluble magnesium salt H-2 aqueous solution, 6.16 parts by weight of a soluble aluminum salt I-1 aqueous solution and 12.72 parts by weight of an alkaline solution J-1 were uniformly added dropwise for 6 hours. After the addition was completed, the mixture was kept warm for 4 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0072] Example 5

[0073] (1) Preparation of functional phosphate-based water reducer F-5: 1 mol of polyether macromonomer A-1, 1 mol of polyether phosphate monomer B-2, and 1.2 mol of hydrophobic soft and hard block macromonomer C-1 were placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, and then heated to 125°C. Acid catalyst E-5 (2% of the total mass of monomers A, B, C, and D) and 3.05 mol of aldehyde monomer D-1 were added, and refluxed at normal pressure for 7 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0074] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-5 and 7 parts by weight of hydrophobic carbon nanomaterial G-1 were dissolved in 65 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 45°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 65°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 9.41 parts by weight of a soluble magnesium salt H-2 aqueous solution, 6.66 parts by weight of a soluble aluminum salt I-1 aqueous solution and 14.04 parts by weight of an alkaline solution J-2 were uniformly added dropwise for 4 hours. After the addition was completed, the mixture was kept warm for 3 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0075] Example 6

[0076] (1) Preparation of functional phosphate-based water reducer F-6: 1 mol of polyether macromonomer A-1, 3.5 mol of polyether phosphate monomer B-2, and 1 mol of hydrophobic soft and hard block macromonomer C-3 were placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, and then heated to 135°C. Acid catalyst E-1 (2.5% of the total mass of monomers A, B, C, and D) and 4.58 mol of aldehyde monomer D-3 were added, and refluxed at normal pressure for 4.5 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0077] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-6 and 8 parts by weight of hydrophobic carbon nanomaterial G-1 were dissolved in 50 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 40°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 70°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 11.04 parts by weight of a soluble magnesium salt H-1 aqueous solution, 4.53 parts by weight of a soluble aluminum salt I-1 aqueous solution and 11.93 parts by weight of an alkaline solution J-2 were uniformly added dropwise for 8 hours. After the addition was completed, the mixture was kept warm for 5 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0078] Example 7

[0079] (1) Preparation of functional phosphate-based water reducer F-7: 1 mol of polyether macromonomer A-1, 4 mol of polyether phosphate monomer B-1, and 1.4 mol of hydrophobic soft and hard block macromonomer C-3 were placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, and then heated to 120°C. Acid catalyst E-1 (2% of the total mass of monomers A, B, C, and D) and 4.57 mol of aldehyde monomer D-1 were added, and refluxed at normal pressure for 5 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0080] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-7 and 4 parts by weight of hydrophobic carbon nanomaterial G-1 were dissolved in 60 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 45°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 80°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 15.95 parts by weight of a soluble magnesium salt H-1 aqueous solution, 8.18 parts by weight of a soluble aluminum salt I-2 aqueous solution and 20.11 parts by weight of an alkaline solution J-2 were uniformly added dropwise for 4 hours. After the addition was completed, the mixture was kept warm for 3 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0081] Example 8

[0082] (1) Preparation of functional phosphate-based water reducer F-8: 1 mol of polyether macromonomer A-4, 2.5 mol of polyether phosphate monomer B-1, and 1 mol of hydrophobic soft and hard block macromonomer C-3 were placed in a reaction vessel under nitrogen protection, heated to 90°C, stirred evenly after melting, and then heated to 135°C. Acid catalyst E-2 (1.5% of the total mass of monomers A, B, C, and D) and 3.46 mol of aldehyde monomer D-1 were added, and refluxed at normal pressure for 7 h. After the reaction was completed, the temperature was slowly lowered to room temperature to obtain a solid phosphate-based water reducer.

[0083] (2) Preparation of phosphate-based nano-hybrid superplasticizer: 10 parts by weight of functional phosphate-based water reducer F-8 and 8 parts by weight of hydrophobic carbon nanomaterial G-2 were dissolved in 70 parts by weight of water, and the mixture was stirred at high speed for 30 minutes at 50°C, and ultrasonically treated for 10 minutes to form a stable and uniform solution; at 50°C, the pH value was adjusted to about 9 with ammonia water, and the solution was continuously stirred. At the same time, 6.72 parts by weight of a soluble magnesium salt H-2 aqueous solution, 3.82 parts by weight of a soluble aluminum salt I-2 aqueous solution and 10.03 parts by weight of an alkaline solution J-2 were uniformly added dropwise for 5 hours. After the addition was completed, the mixture was kept warm for 4 hours to obtain a phosphate-based nano-hybrid superplasticizer.

[0084] Comparative Example 1

[0085] During the synthesis of the functional phosphate-based water reducer F-1 in Example 1, the hydrophobic soft and hard block macromonomer C-1 was removed, and the other reaction conditions remained unchanged to obtain a phosphate-based nano-hybrid superplasticizer.

[0086] Comparative Example 2

[0087] In the preparation process of the phosphate-based nano-hybrid superplasticizer in Example 2, the functional phosphate-based water reducer F-2 was replaced with a commercially available conventional polycarboxylate water reducer PCE, and the other reaction conditions remained unchanged to obtain the phosphate-based nano-hybrid superplasticizer.

[0088] Comparative Example 3

[0089] The composite ultra-early strength admixture is prepared according to Example 1 in patent CN108178549B.

[0090] Application Example 1

[0091] The above embodiments are all dispersion and composite hybridization effects of functional phosphate-based water reducer F on hydrophobic carbon nanomaterial G and magnesium-aluminum layered double metal hydroxide. The dispersion stabilization effect of the embodiments and comparative examples was tested respectively. During the test, the solid content of the sample was uniformly adjusted to 10%, and pure water was added to dilute it by one time, and stirred and dispersed for 30 minutes; in addition, saturated calcium hydroxide was used to simulate the environment of the cement paste pore solution, and the sample was diluted by one time with a saturated calcium hydroxide aqueous solution, and stirred and dispersed for 30 minutes. As a comparison, the hydrophobic carbon nanomaterial G-1 was prepared into a solution with a mass concentration of 2% using pure water and a saturated calcium hydroxide aqueous solution, stirred for 30 minutes, and ultrasonicated for 10 minutes. After the above-obtained sample was left to stand for 48 hours, the uniform supernatant was removed, its solid content was tested, and the sedimentation rate was calculated by comparing it with the theoretical solid content. The experimental results are listed in Table 4.

[0092] Table 4 Dispersion stabilization effect of the embodiments and comparative examples

[0093]

[0094] As can be seen from the above table: in pure water, the 48h sedimentation rates in the embodiments are all less than 5.5%, while comparative examples 1 and 2 have larger sedimentation amounts; in saturated calcium hydroxide solution, the sedimentation amount of the embodiment increases, but does not exceed 10%, while comparative examples 1 and 2 have more sedimentation amounts, wherein the sedimentation rate of comparative example 1 is 65.4%, and the sedimentation rate of comparative example 2 is 80.3%; in addition, the sedimentation rate of the prepared 2% mass concentration G-1 solution in pure water and saturated calcium hydroxide solution is greater than 99%; the above all illustrate that the stabilizing effect of the prepared phosphate-based nano hybrid superplasticizer is better. The stabilizing effect of comparative example 3 in pure water and saturated calcium hydroxide solution is also better.

[0095] Application Example 2

[0096] In order to evaluate the early strength and toughening effect of the phosphate-based nano hybrid superplasticizer prepared by the present invention, mortar was used for evaluation. Onoda P·Ⅱ52.5 cement was used, with a mix ratio of 450g cement, 1350g standard sand, and a water-cement ratio of 0.4; the high-performance water reducer BST-900 (polycarboxylic acid water reducer, weight-average molecular weight of 36800) produced by Boshitong was used as the basic water reducer, and it was used in combination with the embodiments and comparative examples, wherein the dosage in the embodiments and comparative examples was fixed to 0.12%; the dosage of the phosphate-based nano hybrid superplasticizer prepared by the present invention was calculated based on the solid content of the cementitious material, and the bulk density of each group of mortars was basically the same by controlling the defoamer. The test results of the mortar and compressive strength are shown in Table 5 below.

[0097] Table 5 Evaluation of mortar and compressive strength performance

[0098]

[0099] It can be seen from the above table that: when the fluidity of the mortar remains basically the same, the dosage of the basic water-reducing agent used in the corresponding embodiments is relatively small, while the dosage of the basic water-reducing agent in Comparative Examples 1 and 2 is greatly increased, indicating that the hydrophobic soft and hard block side chain structure contained in the functional phosphate-based water-reducing agent can be well combined with the hydrophobic carbon nanomaterial, so that the dispersion effect of the hydrophobic carbon nanomaterial in the high-alkali and high-salt cement paste is better; in Comparative Examples 1 and 2, due to the poor hybridization of the hydrophobic carbon nanomaterial and the water-reducing agent, the precipitated hydrophobic carbon nanomaterial has an adsorption effect on the water-reducing agent, and its flocculation structure also has a water-locking effect on the cement paste, which also greatly increases the dosage of the basic water-reducing agent. Comparative Example 3 itself has good stability, and the corresponding basic water-reducing agent dosage is normal. In terms of strength, the early strength of the embodiment and comparative example 3 at 12h and 24h is significantly improved compared with the reference sample, and the early strength of the embodiment is slightly higher than that of the comparative example 3, indicating that the early strength effect of the phosphate-based nano superplasticizer prepared by the present invention is better than that of the polycarboxylic acid system early strength agent. This is mainly because the phosphate-based water reducer and the magnesium-aluminum layered double metal hydroxide form a stable nano hybrid structure, which has a more excellent ability to accelerate the induction of cement hydration than the polycarboxylic acid water reducer / CSH nano hybrid structure. The 28d strength of the embodiment is significantly higher than that of the polycarboxylic acid system early strength agent system of comparative example 3, indicating that the carbon nanomaterial in the phosphate-based nano superplasticizer has a toughening effect on the later strength of the cement-based material. However, due to the instability of the nano hybrid material in comparative examples 1 and 2, both the early strength and toughening effects are poor.

[0100] The implementation modes of the present invention have been described in detail above in conjunction with specific embodiments, but the present invention is not limited to the above-mentioned implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A functional phosphate-based water reducer, characterized in that: The functional phosphate-based water reducer is formed by polycondensation of structural units A1, B1, C1, and D1. The structural units A1, B1, and C1 are connected by D1. The structural formula of the structural units A1, B1, C1, and D1 is shown in (I): Among them, r is an integer of 90 to 120, s is an integer of 4 to 8, t is an integer of 10 to 40, and m is an integer of 0 to 15; R1 is a bicyclic or monocyclic C6-C10 aromatic group; and R2 is H or a C1-C3 alkyl group.

2. The functional phosphate-based water reducer according to claim 1, characterized in that: R1 is phenyl, α-naphthyl or β-naphthyl, and R2 is H or methyl.

3. The method for preparing the functional phosphate-based water reducer according to claim 1 or 2, characterized in that: The following steps are involved: The polyether macromonomer A, the polyether phosphate monomer B, and the hydrophobic soft and hard block macromonomer C are melted under inert gas conditions, then heated to the reaction temperature, an acid catalyst and an aldehyde monomer D are added, and refluxed under normal pressure for reaction. After the reaction is completed, the temperature is lowered to obtain a phosphoric acid-based water reducer; the structural formulas of the polyether macromonomer A, the polyether phosphate monomer B, the hydrophobic soft and hard block macromonomer C, and the aldehyde monomer D are respectively shown in the following formulas (II), (III), (IV) and (V): Wherein, r, s, t, m, R1 and R2 are selected as described in claim 1 or 2, and n=8-15.

4. The method for preparing the functional phosphate-based water reducer according to claim 3, characterized in that: The melting is carried out at 80-90° C., the reaction temperature is 120-140° C., and the reaction is carried out under normal pressure and reflux for 4-8 hours.

5. The method for preparing the functional phosphate-based water reducer according to claim 3, characterized in that: The molar ratio of the polyether macromonomer A, polyether phosphate monomer B, hydrophobic soft and hard block macromonomer C and aldehyde monomer D is a:b:c:d, wherein a:b:c=1:1-4:1-1.5, (a+b+c):d=1.045-1.45:1; the acid catalyst is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid and ethylsulfonic acid or a combination of two of them in any proportion, and its usage is 0.5-3% of the total mass of monomer A, monomer B, monomer C and monomer D.

6. A phosphate-based nano-hybrid superplasticizer, made from the functional phosphate-based water reducer according to claim 1 or 2.

7. The phosphate-based nano-hybrid superplasticizer according to claim 6, characterized in that: The phosphate-based nano-hybrid superplasticizer is mainly obtained by nano-hybridization of the functional phosphate-based water reducer according to claim 1 or 2, a hydrophobic carbon nanomaterial, and a magnesium-aluminum layered double metal hydroxide.

8. The method for preparing the phosphate-based nano-hybrid superplasticizer according to claim 6 or 7, characterized in that: The following steps are involved: The functional phosphate-based water reducer and the hydrophobic carbon nanomaterial G are dissolved in water to prepare a stable and uniform solution; under certain temperature conditions, the pH value is adjusted, and under stirring conditions, a soluble magnesium salt H aqueous solution, a soluble aluminum salt I aqueous solution and an alkaline solution J are added dropwise at a uniform speed at the same time. After the addition is completed, the solution is kept warm to obtain the phosphate-based nano hybrid superplasticizer.

9. The method for preparing the phosphate-based nano-hybrid superplasticizer according to claim 8, characterized in that: The preparation method of the stable and uniform solution comprises: performing high-speed mixing and stirring for 25-35 minutes and ultrasonic treatment for 8-12 minutes at 30-50° C. to form a stable and uniform solution; adjusting the pH value under certain temperature conditions is to adjust the pH value to 9±1 with ammonia water at 50-80° C.; the dripping time is 2-10 hours, and after the dripping is completed, keeping warm for 2-5 hours.

10. The method for preparing the phosphate-based nano-hybrid superplasticizer according to claim 8, characterized in that: The weight average molecular weight of the functional phosphate-based water reducer is in the range of 20,000 to 100,000; the hydrophobic carbon nanomaterial G is selected from any one of graphene and carbon nanotubes or a combination of two of them in any proportion; the soluble magnesium salt H is selected from any one of magnesium nitrate and magnesium sulfate or a combination of two of them in any proportion; the soluble aluminum salt I is selected from any one of aluminum nitrate and aluminum sulfate or a combination of two of them in any proportion; the alkaline solution J is selected from any one of sodium hydroxide and potassium hydroxide or a combination of two of them in any proportion.

11. The method for preparing the phosphate-based nano-hybrid superplasticizer according to claim 8, characterized in that: The mass concentration of the functional phosphate-based water reducer in the phosphate-based nano hybrid superplasticizer is 5-15%, and the mass ratio of the functional phosphate-based water reducer, the hydrophobic carbon nanomaterial G, and the magnesium-aluminum layered double metal hydroxide is f:g:h, wherein f:g:h is 1:0.4-0.8:0.5-1; the soluble magnesium salt H, the soluble aluminum salt I, and the alkaline solution J are used to prepare the magnesium-aluminum layered double metal hydroxide according to the molar ratio of x:y:z, wherein the molar ratio of x:y is 5:1-2:1, and 2x+3y=z should be satisfied.

12. The use of the phosphate-based nano-hybrid superplasticizer according to claim 6 or 7, characterized in that: The phosphate-based nano hybrid superplasticizer is used as a cement-based material admixture.