A negative electrode material, its preparation method, and a sodium-ion battery

By combining metal sulfide phosphide nanosheets with carbon materials, especially the combination of VCu(PS3)2 nanosheets with few-layer Mxene, the capacity and cycle performance problems of sodium-ion battery anode materials have been solved, realizing anode materials with high capacity, long cycle and high rate performance, suitable for sodium-ion batteries.

CN117810401BActive Publication Date: 2026-11-17SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311814659.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Sodium-ion battery anode materials suffer from limited capacity, poor cycle performance, and poor rate performance during charge and discharge, especially due to the sluggish insertion/extraction kinetics of sodium ions.

Method used

A composite structure of metal sulfide phosphide nanosheets and carbon materials, especially the combination of VCu(PS3)2 nanosheets and few-layer Mxene, was used to prepare metal sulfide phosphide nanosheets through vacuum calcination and exfoliation, and then mixed with carbon materials to form a negative electrode material.

Benefits of technology

It improves the reversible capacity and rate capacity of the anode material, exhibits excellent stability and fast charge/discharge capability, alleviates volume expansion during charge/discharge cycles, and promotes rapid electron/ion transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117810401B_ABST
    Figure CN117810401B_ABST
Patent Text Reader

Abstract

This invention relates to the field of sodium-ion battery technology, and in particular to a negative electrode material, its preparation method, and a sodium-ion battery. The negative electrode material provided by this invention comprises: metal sulfide phosphide nanosheets and carbon materials; the metal sulfide phosphide nanosheets include VCu(PS3)2 nanosheets and / or V2PS... 10 Nanosheets; the carbon material includes at least one of few-layer Mxene, carbon nanotubes, carbon nanofibers, hollow carbon spheres, hard carbon, and soft carbon. This invention combines metal sulfide phosphides with carbon materials, improving the limited capacity of anode materials, enhancing reversible capacity and rate capacity, while exhibiting excellent stability and good fast-charge / fast-discharge capability during charge-discharge cycles. Its application in sodium-ion batteries is beneficial for improving the cycle performance and rate performance of sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery technology, and in particular to a negative electrode material, its preparation method, and a sodium-ion battery. Background Technology

[0002] Sodium belongs to the same group as lithium and has similar physicochemical properties. Moreover, sodium is abundant and inexpensive, attracting widespread attention from the scientific community and being considered the best candidate for large-scale application in energy storage systems. Sodium is the fourth most abundant metallic element in the Earth's crust and is widely distributed and easily accessible. Given the abundance of sodium resources, exploring and researching sodium-ion batteries as an alternative to lithium-ion batteries is of great significance.

[0003] The large ionic radius and high molar mass of sodium ions result in sluggish sodium ion insertion / extraction kinetics, limiting the development of sodium-ion batteries. Therefore, finding suitable anode materials with high specific capacity, long cycle life, and high rate performance is crucial for the practical application of sodium-ion batteries.

[0004] In view of this, this invention is hereby proposed. Summary of the Invention

[0005] The primary objective of this invention is to provide a negative electrode material with high capacity, long cycle life, and high rate performance, exhibiting excellent stability and good fast charging and discharging capabilities during charge-discharge cycles.

[0006] The second objective of this invention is to provide a method for preparing a negative electrode material, which produces a material with high purity and has the potential for further verification.

[0007] A third objective of this invention is to provide a sodium-ion battery with excellent cycle performance and rate performance.

[0008] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:

[0009] This invention provides an anode material comprising: metal sulfide phosphide nanosheets and carbon materials;

[0010] The metal sulfophosphide nanosheets include VCu(PS3)2 nanosheets and / or V2PS. 10 Nanosheets;

[0011] The carbon material includes at least one of few-layer Mxene, carbon nanotubes, carbon nanofibers, hollow carbon spheres, hard carbon, and soft carbon.

[0012] Furthermore, the mass ratio of the metal sulfophosphide nanosheets to the carbon material is (82-91):(9-18).

[0013] Furthermore, the preparation method of the metal sulfide phosphide nanosheets includes the following steps:

[0014] Metal sulfide phosphide crystals were obtained by calcining metal, P and S sources; the metal sulfide phosphide crystals were then exfoliated to obtain metal sulfide phosphide nanosheets.

[0015] The metal source includes a V source and a Cu source; or, the metal source includes a V source.

[0016] Furthermore, it includes at least one of the following features (1) to (4);

[0017] (1) The V source includes vanadium powder;

[0018] (2) The Cu source includes copper powder;

[0019] (3) The P source includes red phosphorus;

[0020] (4) The S source includes sulfur powder.

[0021] Furthermore, the calcination includes: vacuum calcination at 650–750°C for 120–144 hours.

[0022] Furthermore, the vacuum calcination process further includes calcining at 500–600°C for 1–3 hours under an inert atmosphere.

[0023] Further, the stripping process includes: ultrasonically treating an aqueous solution of the metal sulfophosphide crystals in an ice bath for 6–10 hours.

[0024] The present invention also provides a method for preparing the negative electrode material as described above, comprising the following steps:

[0025] The negative electrode material is obtained by mixing metal sulfide phosphide nanosheets and carbon materials.

[0026] Further, the mixing includes: stirring an aqueous solution containing the metal sulfide phosphide nanosheets and the carbon material for 20 to 30 hours.

[0027] The present invention also provides a sodium-ion battery comprising the negative electrode material as described above.

[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0029] 1. The negative electrode material of the present invention includes metal sulfide phosphide and carbon material, which improves the problem of limited capacity of negative electrode material and enhances reversible capacity and rate capacity; at the same time, it has excellent stability and good fast charging and discharging capability during charge and discharge cycles.

[0030] 2. The anode material VCu(PS3)2 / f-Mxene of the present invention combines the high capacity characteristics of sulfur phosphide anode materials with the synergistic effect between multiple metals. Its reversible capacity and rate capacity during cycling are improved compared with single metal sulfides. The introduction of f-Mxene buffers the volume expansion during charge and discharge cycles, promotes the rapid transfer of electrons / ions, and has better rate performance.

[0031] 3. This invention provides a method for synthesizing metal sulfophosphide VCu(PS3)2 nanosheets and a composite of metal sulfophosphide and carbon materials. The synthesized materials have high purity and have the potential for further verification. Attached Figure Description

[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0033] Figure 1 This is a cycle capacity diagram of the negative electrode material of Embodiment 1 and Comparative Example 1 of the present invention.

[0034] Figure 2 This is a rate capacity diagram of the negative electrode material of Example 1 and Comparative Example 1 of the present invention. Detailed Implementation

[0035] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0036] In some embodiments of the present invention, a negative electrode material is provided, comprising: metal sulfide phosphide nanosheets and carbon materials;

[0037] Metal sulfide phosphide nanosheets include VCu(PS3)2 nanosheets and / or V2PS. 10 Nanosheets;

[0038] Carbon materials include at least one of few-layer Mxene, carbon nanotubes, carbon nanofibers, hollow carbon spheres, hard carbon, and soft carbon.

[0039] Metallic sulfur phosphorus (MPS) n Polysulfides are a type of material with a layered nanostructure, used in supercapacitors, energy storage, and other fields. However, during cycling, polysulfides undergo severe volume expansion during the conversion reaction, and phosphorus undergoes a severe volume expansion during the alloying reaction, resulting in poor cycling performance.

[0040] Mxene is a two-dimensional transition metal carbide (nitride) with a layered structure similar to graphene.

[0041] This invention combines metal sulfide phosphide and carbon materials to improve the limited capacity of anode materials and enhance reversible capacity and rate capacity. At the same time, it exhibits excellent stability and good fast charging and discharging capability during charge and discharge cycles.

[0042] The introduction of carbon material into the negative electrode material of this invention can buffer volume expansion and promote rapid electron / ion transfer.

[0043] In some embodiments of the present invention, the negative electrode material includes: VCu(PS3)2 nanosheets and few-layer Mxene; the negative electrode material is named VCu(PS3)2 / f-Mxene.

[0044] Bimetallic sulfophosphorus compound VCu(PS3)2: Based on the conversion reaction mechanism, 1 mol of VCu(PS3)2 reacts with sodium ions, resulting in 18 mol of electron transfer. Based on the theoretical capacity calculation formula: 96485 × n / (M × 3.6), the theoretical specific capacity of VCu(PS3)2 as a sodium-ion battery anode material can be calculated to be 1308.12 mAh / g. -1 .

[0045] Few-layer Mxene (f-Mxene): Graphene-like two-dimensional nanomaterials with large redox active surface areas are widely used in energy storage due to their excellent conductivity. They have the following advantages: special crystal properties provide a low energy barrier for rapid electron transport within atomic layers; the layered structure generates abundant ion diffusion pathways, making the kinetic process more rapid; and excellent strength and toughness can simultaneously alleviate volumetric stress in the reaction, maintaining a strong connection between the layers.

[0046] The anode material VCu(PS3)2 / f-Mxene of this invention combines the high capacity characteristics of sulfur phosphide anode materials with the synergistic effect between multiple metals. Its reversible capacity and rate capacity during cycling are improved compared with single metal sulfides. The introduction of f-Mxene buffers the volume expansion during charge and discharge cycles, promotes the rapid transfer of electrons / ions, and has better rate performance.

[0047] In some embodiments of the present invention, the few-layer Mxene includes Ti3C2T. x Ti2CT x Ti3CNT x V2CT x and Nb4C3T x At least one of them.

[0048] In some embodiments of the present invention, the mass ratio of metal sulfophosphide nanosheets to carbon material is (82-91):(9-18); typically, but not limitingly, for example, the mass ratio of metal sulfophosphide nanosheets to carbon material can be 91:9, 90:10, 89:11, 88:12, 87:13, 86:14, 85:15, 84:16, 83:17, 82:18 or any combination thereof; preferably, the mass ratio of metal sulfophosphide nanosheets to carbon material is (84-86):(14-16).

[0049] In some embodiments of the present invention, the method for preparing metal sulfophosphide nanosheets includes the following steps:

[0050] Metal sulfide phosphide crystals were obtained by calcining metal, P and S sources; metal sulfide phosphide nanosheets were obtained by exfoliation of the metal sulfide phosphide crystals.

[0051] The metal source includes a V source and a Cu source; or, the metal source includes a V source.

[0052] When the metal source is a V source and a Cu source, the obtained metal sulfide phosphide nanosheets are VCu(PS3)2 nanosheets; when the metal source is a V source, the obtained metal sulfide phosphide nanosheets are V2PS. 10 Nanosheets.

[0053] In some embodiments of the present invention, the V source includes, but is not limited to, vanadium powder.

[0054] In some embodiments of the present invention, the Cu source includes, but is not limited to, copper powder.

[0055] In some embodiments of the present invention, the P source includes, but is not limited to, red phosphorus.

[0056] In some embodiments of the present invention, the S source includes, but is not limited to, sulfur powder.

[0057] In some embodiments of the present invention, the molar ratio of V source, Cu source, P source and S source is (0.98~1.02):(0.98~1.02):(5.98~6.02).

[0058] In some embodiments of the present invention, the molar ratio of V source, P source and S source is (1.98~2.02):(0.98~1.02):(9.98~10.02).

[0059] In some embodiments of the present invention, calcination includes: vacuum calcination at 650-750°C for 120-144 hours; preferably, calcination includes: vacuum calcination at 740-750°C for 140-144 hours.

[0060] Different crystal forms of materials have different capacities and rate performances. Vacuum calcination at 740–750℃ can synthesize metal sulfophosphide crystals with good capacity and rate performance. If the vacuum calcination temperature is too low, it will not reach the temperature required for the synthesis of sulfophosphides, and thus sulfophosphides cannot be synthesized. If the vacuum calcination temperature is too high, the sulfophosphides may decompose. The vacuum calcination time affects the purity of the metal sulfophosphides. A shorter time results in lower purity, lower capacity, and lower rate performance. A longer time may lead to side reactions during the synthesis of sulfophosphides, which can also result in low capacity and poor rate performance.

[0061] In some embodiments of the present invention, the vacuum calcination process further includes: calcining at 500–600°C for 1–3 hours under an inert atmosphere; preferably, the vacuum calcination process further includes: calcining at 580–600°C for 1.5–2.5 hours under an inert atmosphere.

[0062] The present invention involves vacuum calcination followed by calcination under an inert atmosphere to remove excess sulfur and red phosphorus.

[0063] The calcination temperature under an inert atmosphere is too low, and the boiling point of sulfur and phosphorus is not reached, so excess sulfur and phosphorus cannot be removed; if the temperature is too high, sulfur and phosphorus compounds will decompose, resulting in poor capacity and rate performance; if the calcination time under an inert atmosphere is too short, impurities cannot be completely removed, resulting in low capacity and rate performance; if the time is too long, side reactions may occur, resulting in low capacity and rate performance.

[0064] In some embodiments of the present invention, the stripping process includes: ultrasonically treating an aqueous solution of metal sulfophosphide crystals in an ice bath for 6 to 10 hours.

[0065] In some embodiments of the present invention, the peeling process further includes: freeze drying.

[0066] In some embodiments of the present invention, the method for preparing few-layer Mxene includes the following steps:

[0067] After intercalation and layering of multilayer Mxene through treatment with organic alkali and ultrasound, ammonium ions are introduced to disrupt the electrostatic balance and form flocculents. After standing, the precipitate is collected, dried, and calcined to obtain few-layer Mxene.

[0068] In some embodiments of the present invention, after mixing multilayer Mxene and an organic base aqueous solution, the mixture is subjected to solid-liquid separation and washing to obtain multilayer Mxene with inserted organic molecules; preferably, the organic base aqueous solution includes a tetramethylammonium hydroxide (TMAH) aqueous solution; the ratio of multilayer Mxene to organic base aqueous solution is 0.5-1.5g: 5-15mL.

[0069] In some embodiments of the present invention, multilayer Mxene with inserted organic molecules is dispersed in water, subjected to ultrasonic treatment, centrifuged, and the supernatant is collected; the solid precipitate obtained after centrifugation is dispersed in water again, and the above steps are repeated multiple times to obtain an Mxene solution.

[0070] In some embodiments of the present invention, ammonia and ammonium bicarbonate solution are added to disrupt the electrostatic equilibrium and form flocculent matter. The purpose of adding ammonia and ammonium bicarbonate solution here is to introduce ammonium ions, which are used to disrupt the electrostatic equilibrium. The amount of ammonium ions added is ensured to be sufficient, until flocculent matter is observed.

[0071] In some embodiments of the present invention, the preparation method of few-layer Mxene includes calcination at 150–200°C for 5–7 hours under an inert atmosphere. The calcination process transforms the Mxene condensate into few-layer Mxene.

[0072] In some embodiments of the present invention, a method for preparing the above-mentioned negative electrode material is also provided, comprising the following steps:

[0073] Metal sulfide phosphide nanosheets and carbon materials are mixed to obtain anode materials.

[0074] In some embodiments of the present invention, mixing includes: stirring an aqueous solution containing metal sulfophosphide nanosheets and carbon material for 20 to 30 hours; preferably, the stirring time is 24 to 26 hours.

[0075] This invention combines metal sulfide phosphide nanosheets with carbon materials through simple stirring, resulting in a high-purity material with potential for further verification.

[0076] In some embodiments of the present invention, a sodium-ion battery is also provided, comprising the above-described negative electrode material.

[0077] In some embodiments of the present invention, a sodium-ion battery includes a negative electrode sheet comprising the aforementioned negative electrode material, a conductive agent, and a binder in a mass ratio of (75-85):(8-12):(8-12).

[0078] The negative electrode material of this invention has high capacity, long cycle life and high rate performance. Its application in sodium-ion batteries is beneficial to improving the capacity, cycle performance and rate performance of sodium-ion batteries.

[0079] Example 1

[0080] The method for preparing the negative electrode material provided in this embodiment includes the following steps:

[0081] S1. Mix 0.051g vanadium powder, 0.063g copper powder, 0.062g phosphorus powder, and 0.192g sulfur powder evenly, seal in a quartz ampoule, and incubate at 750℃ under vacuum (~10 -6 Calcination under mb) conditions for 6 days (144h) and then calcination at 500℃ for 2h under argon atmosphere to obtain bulk VCu(PS3)2 crystals;

[0082] The above-mentioned bulk VCu(PS3)2 crystals were dispersed in 100 mL of deionized water and ultrasonically treated in an ice bath for 8 h. After freeze-drying, VCu(PS3)2 nanosheets were obtained.

[0083] S2. Add 1g of multilayer Mxene powder (Ti3C2T) x Add 10 mL of tetramethylammonium hydroxide (TMAH) aqueous solution (concentration 25 wt%), stir at room temperature for 24 h, and then centrifuge and wash three times with deionized water to obtain a solid precipitate. Disperse the solid precipitate in 50 mL of deionized water, sonicate under argon atmosphere for 1 h, centrifuge at 3500 r / min for 10 min, collect the supernatant, and repeat the above process four times to obtain about 200 mL of supernatant. Repeat the process of obtaining about 200 mL of supernatant twice to obtain about 350 mL of multilayered Mxene solution. Then add 10 mL of 28 wt% ammonia water to the above multilayered Mxene solution, and then add ammonium bicarbonate solution (prepared by dissolving 3.2 g of ammonium bicarbonate in 40 mL of deionized water) dropwise to form flocculents. After standing for 1 h, collect the flocculents. After freeze-drying the flocculents, calcine them at 180 °C for 6 h in Ar atmosphere to obtain few-layer Mxene (f-Mxene).

[0084] S3. Disperse 100 mg of VCu(PS3)2 nanosheets in 100 mL of deionized water, sonicate for 30 min to obtain a homogeneous solution, and then add 6 mL of a solution with a concentration of 3 mg / mL. -1The aqueous solution of the above few-layer Mxene was stirred for 24 h and then freeze-dried to obtain the anode material (VCu(PS3)2 / f-Mxene).

[0085] Example 2

[0086] The method for preparing the negative electrode material provided in this embodiment is the same as in Embodiment 1, except that in step S1, the negative electrode material is prepared at 650°C under vacuum (~10°C). -6 Calcination for 6 days under the conditions of mb).

[0087] Example 3

[0088] The method for preparing the negative electrode material provided in this embodiment is the same as in Embodiment 1, except that in step S1, the negative electrode material is prepared at 750°C under vacuum (~10°C). -6 Calcination for 5 days (120h) under the conditions of mb).

[0089] Example 4

[0090] The preparation method of the negative electrode material provided in this embodiment is the same as that in Embodiment 1, except that in step S1, the temperature is raised to 600°C and calcined for 2 hours under an argon atmosphere.

[0091] Example 5

[0092] The method for preparing the negative electrode material provided in this embodiment includes the following steps:

[0093] S1. Mix 0.101g vanadium powder, 0.03g red phosphorus, and 3.2g sulfur powder evenly, seal in a quartz ampoule, and incubate at 750℃ under vacuum (~10 -6 Calcination under mb) conditions for 6 days (144 h) followed by calcination at 500 °C for 2 h in an argon atmosphere yielded bulk V2PS. 10 Crystals;

[0094] The above large V2PS 10 The crystals were dispersed in 100 mL of deionized water and sonicated in an ice bath for 8 h. After freeze-drying, V2PS was obtained. 10 Nanosheets.

[0095] S2, the above V2PS 10 Nanosheets were dispersed in 100 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution. Then, 6 mL of a 3 mg / mL solution was added. -1 A few layers of Mxene aqueous solution were stirred for 24 hours and then freeze-dried to obtain the anode material (V2PS). 10 / f-Mxene);

[0096] The few-layer Mxene is the same as in Example 1.

[0097] Example 6

[0098] The preparation method of the negative electrode material provided in this embodiment is the same as that in Example 1, except that in step S3, the concentration is 3 mg / mL. -1 The volume of the aqueous solution of the few-layer Mxene is 3 mL.

[0099] Example 7

[0100] The method for preparing the negative electrode material provided in this embodiment includes the following steps:

[0101] 100 mg of VCu(PS3)2 nanosheets were dispersed in 100 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution. Then, 18 mg of carbon nanotubes (CNTs) were added and stirred for 24 h. After freeze-drying, the negative electrode material VCu(PS3)2 / CNT was obtained.

[0102] The VCu(PS3)2 nanosheets used were the same as those in Example 1.

[0103] Example 8

[0104] The method for preparing the negative electrode material provided in this embodiment includes the following steps:

[0105] 100 mg of VCu(PS3)2 nanosheets were dispersed in 100 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution. Then, 18 mg of carbon nanofibers (CNF) were added and stirred for 24 h. After freeze-drying, the negative electrode material VCu(PS3)2 / CNF was obtained.

[0106] The VCu(PS3)2 nanosheets used were the same as those in Example 1.

[0107] Example 9

[0108] The method for preparing the negative electrode material provided in this embodiment includes the following steps:

[0109] 100 mg of VCu(PS3)2 nanosheets were dispersed in 100 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution. Then, 18 mg of hard carbon was added and stirred for 24 h. After freeze-drying, the negative electrode material VCu(PS3)2 / C was obtained.

[0110] Comparative Example 1

[0111] The negative electrode material provided in this comparative example is VCu(PS3)2, and its preparation method is the same as that in Example 1.

[0112] Experimental Example 1

[0113] The method for preparing a button cell includes the following steps: grinding negative electrode material, conductive agent (super-p) and binder (sodium carboxymethyl cellulose) in a mass ratio of 80:10:10, mixing them evenly, adding deionized water, and stirring on a magnetic stirrer for 8-10 hours to obtain a slurry; uniformly coating the slurry onto copper foil and drying it in a vacuum oven at 80°C to obtain a negative electrode sheet.

[0114] Using the aforementioned negative electrode sheet, glass fiber as the battery separator material, and hand-rolled sodium sheet as the counter electrode and reference electrode in the battery, a button battery of model 2032 was obtained by assembling it in a glove box filled with Ar.

[0115] Button batteries were fabricated using the negative electrode material of Example 1 (VCu(PS3)2 / f-Mxene) and Comparative Example 1 (VCu(PS3)2) as the negative electrode material, respectively. The batteries were tested using a Land battery testing system at 0.1 A·g. -1 The results of the cyclic testing and rate capacity testing are as follows: Figure 1 and Figure 2 As shown.

[0116] from Figure 1 It can be seen that the reversible capacity of VCu(PS3)2 / f-Mxene in this invention is approximately 1290 mAh·g. -1 The capacity of VCu(PS3)2 remained relatively stable after multiple cycles; however, the capacity decay of VCu(PS3)2 was larger, indicating that the introduction of f-Mxene buffered the volume expansion of VCu(PS3)2 during charge-discharge cycles. The initial capacity of VCu(PS3)2 is higher than the theoretical capacity because a solid electrolyte interphase (SEI) film is formed during the first charge-discharge cycle, which increases the irreversible capacity during the first charge-discharge cycle, thus making its capacity higher than the theoretical capacity.

[0117] from Figure 2 It can be seen that after the introduction of f-Mxene, the capacity of VCu(PS3)2 / f-Mxene is better than that of VCu(PS3)2 at every current density, indicating that VCu(PS3)2 / f-Mxene has superior rate performance.

[0118] Button batteries were prepared using the negative electrode materials of Examples 1-9 and Comparative Example 1, respectively. Their initial discharge capacity, capacity retention after 70 cycles (compared to the second discharge capacity), and 9 A·g were measured. -1 The discharge capacity test results are shown in Table 1.

[0119] Table 1

[0120]

[0121]

[0122] As can be seen from Table 1, the anode material of the present invention exhibits excellent overall electrochemical performance.

[0123] This description is intended to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A negative electrode material, characterized in that, include: Metal sulfophosphide nanosheets and carbon materials; The metal sulfide phosphide nanosheets include VCu(PS3)2 nanosheets; The carbon material includes at least one of few-layer Mxene, carbon nanotubes, carbon nanofibers, hollow carbon spheres, hard carbon, and soft carbon; The mass ratio of the metal sulfophosphide nanosheets to the carbon material is (82~91):(9~18).

2. The negative electrode material according to claim 1, characterized in that, The preparation method of the metal sulfophosphide nanosheets includes the following steps: Metal sulfide phosphide crystals were obtained by calcining metal, P and S sources; the metal sulfide phosphide crystals were then exfoliated to obtain metal sulfide phosphide nanosheets. The metal source includes a V source and a Cu source.

3. The negative electrode material according to claim 2, characterized in that, Includes at least one of the following features (1) to (4); (1) The V source includes vanadium powder; (2) The Cu source includes copper powder; (3) The P source includes red phosphorus; (4) The S source includes sulfur powder.

4. The negative electrode material according to claim 2, characterized in that, The calcination includes vacuum calcination at 650~750℃ for 120~144h.

5. The negative electrode material according to claim 4, characterized in that, The vacuum calcination process further includes calcination at 500-600°C for 1-3 hours under an inert atmosphere.

6. The negative electrode material according to claim 2, characterized in that, The stripping process includes ultrasonically treating the aqueous solution of the metal sulfophosphide crystals in an ice bath for 6-10 hours.

7. The method for preparing the negative electrode material according to any one of claims 1 to 6, characterized in that, Includes the following steps: The negative electrode material is obtained by mixing metal sulfide phosphide nanosheets and carbon materials.

8. The method for preparing the negative electrode material according to claim 7, characterized in that, The mixing process includes stirring an aqueous solution containing the metal sulfide phosphide nanosheets and the carbon material for 20-30 hours.

9. A sodium-ion battery, characterized in that, Includes the negative electrode material as described in any one of claims 1 to 6.

Citation Information

Patent Citations

  • FePS3@MXene nano composite negative electrode material for sodium-ion battery, preparation method of FePS3-MXene nano composite negative electrode material and sodium-ion battery