A method for preparing a carbon-based composite material gradient oxygen barrier protective coating

By using a borosilicate glass composite coating on the surface of carbon-based composite materials, the problems of coating self-damage and structural deterioration of carbon-based composite materials in high-temperature oxidizing environments are solved, achieving more efficient oxidation protection and extending the coating life. service life and temperature range.

CN117843401BActive Publication Date: 2024-10-08HENAN ACAD OF SCI CARBON MATRIX COMPOSITES RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311827693.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-08
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Existing carbon-based composite materials are rapidly oxidized in high-temperature oxidizing environments, resulting in a decrease in mechanical properties. The coating is self-destructive due to oxidation, resulting in an unstable oxygen barrier structure. There are self-destructive film formation and structural deterioration problems, which limit its use in aerospace. application.

Method used

Using borosilicate glass powder and hafnium dioxide as slurry powder, and silica sol as solvent, a non-destructive prefabricated oxygen barrier film is formed on the surface of HfB2-SiC by spin coating to form a borosilicate glass composite coating, reducing the number of coatings loss, improve adhesion, improve the fluidity of SiO2, heal cracks and holes caused by thermal stress and oxidation reactions.

Benefits of technology

It effectively avoids the film-forming loss of the coating, improves the initial oxidation protection capability, extends the oxidation protection time, improves the protective aging and temperature range of the coating, and significantly improves the oxygen barrier performance of carbon-based composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117843401B_ABST
    Figure CN117843401B_ABST
Patent Text Reader

Abstract

The invention relates to a carbon-based composite gradient oxygen barrier protective coating and a preparation method thereof. Firstly, a graphite@HfB2-SiC carbon-based composite material is prepared by a spark plasma sintering method according to a ratio; secondly, hafnium dioxide, borosilicate glass powder and silica sol are mixed in proportion to form a white suspension slurry; thirdly, the prepared slurry is spin-coated on the surface of the graphite@HfB2-SiC; the graphite@HfB2-SiC carbon-based composite material is double-sided spin-coated by the same process until it is completely covered; finally, the spin-coated composite coating is dried at a low temperature in an oven, and the dried sample is placed in a vacuum tube furnace for non-destructive film forming treatment; the invention overcomes the problems of film self-damage and deterioration of coating structure in the existing low-loss film forming technology, and has the characteristics of simple process, non-destructive film forming and significant oxygen barrier protection effect; the film forming loss of the coating is avoided, the self-healing ability of cracks and holes generated on the surface during the oxidation protection process is improved, the oxidation protection temperature is increased, and the oxidation protection time is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-temperature oxygen barrier protection, and in particular to a method for preparing a carbon-based composite material gradient oxygen barrier protective coating. Background Art

[0002] Carbon materials are promising candidate materials in the aerospace field due to their low density, high strength and excellent mechanical properties. However, rapid oxidation in high-temperature aerobic environments causes a significant decrease in their mechanical properties, greatly limiting their practical applications in aerospace. In order to protect carbon-based composites from high-temperature oxidation, preparing an ultra-high temperature oxygen barrier coating on the surface is the best choice at this stage.

[0003] Transition metal borides are often used as the main components of ultra-high temperature ceramics (UHTCs) due to their extremely high melting temperatures. However, single forms of borides are not suitable for ultra-high temperature applications due to their inherent brittleness under thermal shock conditions and limited sintering properties. The oxidation behavior of SiC with ZrB2 and HfB2 ceramics at high temperatures, that is, the interaction between silicide and boride in the reaction process with oxygen will generate fluid SiO2, which can fill the defects in the thermal erosion process and block the oxygen diffusion channel. This not only improves the oxygen barrier properties of carbon-based composites, but also improves the density of the material at ultra-high temperatures. Therefore, the SiO2 layer generated during the oxidation process plays a vital role in the oxidation protection of carbon-based composites. However, the generation of the self-generated SiO2 layer with oxygen barrier ability is often accompanied by the oxidation self-damage of the coating, which greatly destroys the stability of the oxygen barrier structure of the coating.

[0004] Wu Binbin et al. (Wu Binbin. Construction and performance research of HfB2-SiC high oxygen barrier coating based on low-temperature hot pressing and rapid sintering [D]. China University of Mining and Technology, 2023) prepared a SiO2 glass film with low oxygen permeability through film formation regulation and treatment with low film formation loss, which improved the comprehensive oxygen barrier effect of the coating to a certain extent and extended the working life of the coating. Despite this, there is still a low self-damage, which is bound to cause degradation to the coating structure. Therefore, there is an urgent need for a coating preparation technology to solve the problems of film self-damage and coating structure degradation during film formation in the existing technology, so as to improve the protective effect and protective time of the coating. Summary of the invention

[0005] The present invention aims to provide a carbon-based composite material gradient oxygen barrier protective coating and a preparation method thereof to solve the drawbacks of the above-mentioned prior art:

[0006] The present invention uses borosilicate glass powder and hafnium dioxide as slurry powder, silica sol as solvent, HfB2-SiC carbon-based composite material as matrix, and adopts spin coating method to non-destructively preform an oxygen barrier film on the surface of HfB2-SiC. By preforming the oxygen barrier film non-destructively, the boride and silicide in the coating are protected in the early stage of oxidation, the loss of the coating is reduced, and the performance of the coating is retained to the maximum extent; when forming the film, silica sol is used as a solvent to improve the adhesion of the slurry and reduce cracking caused by solvent evaporation. At the same time, the complex phase oxide in the borosilicate glass powder will improve the fluidity of SiO2, heal the cracks and holes caused by thermal stress and oxidation reaction during the oxidation process, reduce the pore size and porosity of the coating defects, and improve the working temperature range of the coating.

[0007] Specifically, the present invention adopts the following technical solutions:

[0008] A method for preparing a carbon-based composite gradient oxygen barrier protective coating, specifically a surface coating of a graphite@HfB2-SiC carbon-based composite material and a non-destructive film forming method thereof, is carried out according to the following steps, including:

[0009] (1) preparing graphite@HfB2-SiC carbon-based composite materials by spark plasma sintering according to the ratio;

[0010] (2) mixing hafnium dioxide, borosilicate glass powder and silica sol in proportion to form a white suspension slurry;

[0011] (3) Spin coating the slurry prepared in step (2) on the surface of graphite@HfB2-SiC, taking an appropriate amount of the slurry and performing spin coating three times; spin coating the graphite@HfB2-SiC carbon-based composite material on both sides using the same process until it is fully covered;

[0012] (4) Drying the borosilicate glass composite coating in step (3) at low temperature in an oven, and placing the dried borosilicate glass composite coating sample in a vacuum tube furnace for non-destructive film forming treatment; taking it out after the treatment is completed to obtain a sample with non-destructive film forming on the surface of the carbon-based composite material.

[0013] Preferably, in step (1), HfB2 powder and SiC powder are used to prepare graphite@HfB2-SiC carbon-based composite material, wherein the volume ratio of HfB2 powder to SiC powder is 60vol%HfB2-40vol%SiC.

[0014] Preferably, in step (2), the mass ratio of hafnium dioxide, borosilicate glass powder and silica sol is in the range of 1:9:18 to 6:9:18.

[0015] Preferably, in step (3), the amount of slurry used is in the range of 0.5 g to 2 g.

[0016] Preferably, in the step (4), the low-temperature drying temperature of the spin-coated borosilicate glass composite coating glass layer is 40-60° C., and the processing time is 4 h to 6 h.

[0017] Preferably, in the step (4), the heat treatment temperature of the spin-coated borosilicate glass composite coating glass layer is 1200-1300° C., and the treatment time is 4 h to 6 h.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The non-destructive film-forming method adopted in the present invention has a simple process and overcomes the problem of self-damage consumption during the film-forming process of the oxygen barrier coating, fundamentally avoiding the film-forming loss of the coating and improving the protective ability of the material in the early stage of oxidation.

[0020] (2) As an effective coating preparation method, the non-destructive film-forming technology involved in the present invention avoids self-damage of the film formation compared with conventional oxygen barrier coating protection technology and existing pre-oxidation film-forming technology, effectively prevents the degradation of the coating structure caused by oxidation self-damage, avoids the formation of oxygen diffusion channels in the intrinsic structure, and improves the protective effectiveness of the coating.

[0021] (3) Through the synergistic effect of hafnium dioxide powder and borosilicate glass powder, the fluidity of the glass film SiO2 formed on the surface of the carbon-based composite material is improved, the self-healing ability of cracks and holes generated on the surface during the oxidation protection process is improved, the oxidation protection temperature is increased, and the oxidation protection time is extended.

[0022] In summary, the present invention overcomes the problems of self-damage of film formation and deterioration of coating structure in the existing low-loss film-forming technology, and has the characteristics of simple process, lossless film formation, and significant oxygen barrier protection effect; it avoids coating film loss, improves the self-healing ability of cracks and holes generated on the surface during the oxidation protection process, increases the oxidation protection temperature, and prolongs the oxidation protection time. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a macroscopic surface image of the oxygen barrier protective coating of the carbon-based composite material in an embodiment of the present invention.

[0024] Figure 2 This is a SEM cross-sectional view of the carbon-based composite material oxygen barrier protective coating obtained in Example 1 of the present invention.

[0025] Figure 3 This is a SEM cross-sectional view of the carbon-based composite material oxygen barrier protective coating obtained in Example 2 of the present invention.

[0026] Figure 4 This is a SEM cross-sectional view of the carbon-based composite material oxygen barrier protective coating obtained in Example 3 of the present invention.

[0027] Figure 5 This is a SEM cross-sectional view of the carbon-based composite material oxygen barrier protective coating obtained in Comparative Example 1 of the present invention.

[0028] Figure 6 This is a SEM cross-sectional view of the carbon-based composite material oxygen barrier protective coating obtained in Comparative Example 2 of the present invention.

[0029] Figure 7 The oxidation weight gain curves of the carbon-based composite oxygen barrier protective coatings obtained in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2 are shown. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0031] Embodiment 1:

[0032] A method for preparing a carbon-based composite material gradient oxygen barrier protective coating is carried out according to the following steps, including:

[0033] (1) According to the ratio, the graphite @ HfB2-SiC carbon-based composite material is prepared by spark plasma sintering. Specifically, HfB2 powder and SiC powder are used to prepare the graphite @ HfB2-SiC carbon-based composite material, and according to the volume ratio of 60 vol% HfB2-40 vol% SiC, the graphite @ HfB2-SiC carbon-based composite material is prepared by spark plasma sintering at 1500°C;

[0034] (2) mixing hafnium dioxide, borosilicate glass powder and silica sol in a mass ratio of 1:9:18 to form a white suspension slurry;

[0035] (3) Spin-coat the slurry prepared in step (2) on the surface of graphite@HfB2-SiC, take 0.5g of the slurry, and spin-coat it three times. Spin-coat the graphite@HfB2-SiC carbon-based composite material on both sides in the same process until it is completely covered;

[0036] (4) The borosilicate glass composite coating in step (3) is dried in an oven at low temperature (drying temperature 40°C, treatment time 4h), and after drying, the borosilicate glass composite coating sample is placed in a vacuum tube furnace for non-destructive film forming treatment (treatment temperature 1200°C, treatment time 4h). After the treatment is completed, the sample is taken out to obtain a sample with non-destructive film formation on the surface of the carbon-based composite material.

[0037] The cross-sectional microstructure of the obtained carbon-based composite material oxygen barrier protective coating is as follows: Figure 2 As shown, the weight gain results of 1700℃ constant temperature oxidation are as follows Figure 7 shown.

[0038] Embodiment 2:

[0039] A method for preparing a carbon-based composite material gradient oxygen barrier protective coating is carried out according to the following steps, including:

[0040] (1) According to the ratio, a graphite@HfB2-SiC carbon-based composite material was prepared by spark plasma sintering; the details were the same as in Example 1;

[0041] (2) mixing hafnium dioxide, borosilicate glass powder and silica sol in a certain proportion (mass ratio 3:9:18) to form a white suspension slurry;

[0042] (3) Spin-coat the slurry prepared in step (2) on the surface of graphite@HfB2-SiC, take 1g of the slurry, and spin-coat it three times. Spin-coat the graphite@HfB2-SiC carbon-based composite material on both sides in the same process until it is completely covered;

[0043] (4) The borosilicate glass composite coating in step (3) is dried in an oven at low temperature (drying temperature 50°C, treatment time 5h), and after drying, the borosilicate glass composite coating sample is placed in a vacuum tube furnace for non-destructive film forming treatment (treatment temperature 1250°C, treatment time 5h). After the treatment is completed, the sample is taken out to obtain a sample with non-destructive film formation on the surface of the carbon-based composite material.

[0044] The cross-sectional microstructure of the obtained carbon-based composite material oxygen barrier protective coating is as follows: Figure 3 As shown, the weight gain results of 1700℃ constant temperature oxidation are as follows Figure 7 shown.

[0045] Embodiment 3:

[0046] A method for preparing a carbon-based composite material gradient oxygen barrier protective coating is carried out according to the following steps, including:

[0047] (1) According to the ratio, a graphite@HfB2-SiC carbon-based composite material was prepared by spark plasma sintering; the details were the same as in Example 1;

[0048] (2) mixing hafnium dioxide, borosilicate glass powder and silica sol in a certain proportion (mass ratio 6:9:18) to form a white suspension slurry;

[0049] (3) Spin-coat the slurry prepared in step (2) onto the surface of graphite@HfB2-SiC, take 2g of the slurry, and spin-coat it three times. Spin-coat the graphite@HfB2-SiC carbon-based composite material on both sides in the same process until it is completely covered;

[0050] (4) The borosilicate glass composite coating in step (3) is dried in an oven at low temperature (drying temperature 60°C, treatment time 6h), and the dried borosilicate glass composite coating sample is placed in a vacuum tube furnace for non-destructive film forming treatment (treatment temperature 1300°C, treatment time 6h). After the treatment is completed, the sample is taken out to obtain a sample with non-destructive film formation on the surface of the carbon-based composite material.

[0051] The cross-sectional microstructure of the obtained carbon-based composite material oxygen barrier protective coating is as follows: Figure 4 As shown, the weight gain results of 1700℃ constant temperature oxidation are as follows Figure 7 shown.

[0052] Comparative Example 1:

[0053] (1) According to the ratio, the graphite @ HfB2-SiC carbon-based composite material is prepared by spark plasma sintering. Specifically: according to the volume ratio of 60 vol% HfB2-40 vol% SiC, the graphite @ HfB2-SiC carbon-based composite material is prepared by spark plasma sintering at 1500°C;

[0054] Comparative Example 1 Cross-sectional microstructure Figure 5 As shown, the weight gain results of 1700℃ constant temperature oxidation are as follows Figure 7 shown.

[0055] It can be found that:

[0056] Compared with Examples 1 to 3, Comparative Example 1 did not perform any film-forming treatment on the HfB2-SiC coating. Since it relied solely on the coating structure to block oxygen and lacked the protection of the composite glass layer, Comparative Example 1 had an obvious rapid weight gain stage 10 minutes before oxidation (indicating that the coating was oxidized and lost drastically). In addition, Comparative Example 1 was most severely oxidized at 1700°C, with the largest oxidation weight gain and the worst protection effect.

[0057] Comparative Example 2:

[0058] (1) According to the ratio, the graphite@HfB2-SiC carbon-based composite material is prepared by spark plasma sintering;

[0059] (2) The HfB2-SiC carbon-based composite material was subjected to a pre-oxidation film-forming treatment in a muffle furnace (film-forming temperature 1300°C, film-forming time 6h) to obtain a pre-oxidation film-forming HfB2-SiC coating.

[0060] Compared with Examples 1 to 3, Comparative Example 2 uses traditional pre-oxidation film-forming treatment. Since the essence of the coating in the traditional pre-oxidation film-forming treatment is low-loss film-forming, that is, the coating itself produces loss, the coating structure is damaged, and the working life itself is shortened. At the same time, the low-loss film-forming of the coating causes internal defects and oxygen diffusion channels. The weight gain per unit area after the same oxidation conditions (oxidation temperature, oxidation time) is greater than that of the examples, indicating that the degree of oxidation and loss are more serious, highlighting that the lossless film-forming technology in the present invention has a more excellent protection effect and protection timeliness.

[0061] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A method for preparing a carbon-based composite gradient oxygen barrier protective coating, specifically a surface coating of a graphite@HfB2-SiC carbon-based composite material and a non-destructive film forming method thereof, characterized in that: Follow these steps, including: (1) Preparing graphite@HfB2-SiC carbon-based composite materials by spark plasma sintering according to the ratio; (2) mixing hafnium dioxide, borosilicate glass powder and silica sol in proportion to form a white suspension slurry; (3) Spin-coating the slurry prepared in step (2) onto the surface of graphite@HfB2-SiC, taking an appropriate amount of the slurry and performing spin coating three times; spin-coating the graphite@HfB2-SiC carbon-based composite material on both sides using the same process until it is completely covered; (4) drying the borosilicate glass composite coating in step (3) in an oven at low temperature, and placing the dried borosilicate glass composite coating sample in a vacuum tube furnace for non-destructive film forming treatment; taking it out after the treatment is completed to obtain a sample with non-destructive film forming on the surface of the carbon-based composite material; In the step (2), the mass ratio of hafnium dioxide, borosilicate glass powder and silica sol is in the range of 1:9:18 to 6:9:18; In the step (4), the non-destructive film forming treatment temperature is 1200-1300° C., and the treatment time is 4 h-6 h.

2. The method for preparing a carbon-based composite material gradient oxygen barrier protective coating according to claim 1, characterized in that: In the step (1), HfB2 powder and SiC powder are used to prepare a graphite@HfB2-SiC carbon-based composite material, wherein the volume ratio of HfB2 powder to SiC powder is 60 vol% HfB2-40 vol% SiC.

3. The method for preparing a carbon-based composite material gradient oxygen barrier protective coating according to claim 1, characterized in that: In the step (3), the amount of slurry used is in the range of 0.5 g to 2 g.

4. The method for preparing a carbon-based composite material gradient oxygen barrier protective coating according to claim 1, characterized in that: In the step (4), the low-temperature drying temperature of the spin-coated borosilicate glass composite coating is 40-60° C., and the processing time is 4 h to 6 h.