Method for preparing graphite nanocapsule from lignin and graphite nanocapsule
Through the methods of liquid nitrogen freeze-drying and flash Joule heating, the problems of high preparation cost and complicated process of graphite nanocapsules in the existing technology are solved, and efficient and low-cost preparation of graphite nanocapsules is achieved, with high degree of graphitization and regularity. hollow spherical structure.
Patent Information
- Application Number
- CN202410819462.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In the existing technology, it is difficult to prepare graphite nanocapsules using lignin as the only carbon source with high efficiency and low cost, resulting in high preparation costs, complex processes, and uneven quality, which cannot satisfy the high-value utilization of lignin and the green and green properties of graphite nanocapsules. Low cost and rapid preparation requirements.
Using liquid nitrogen freeze-drying and flash Joule heating methods, the mixture of lignin and transition metal salts is slowly pyrolyzed to form hollow graphite nanocapsules. The extremely fast heating and cooling rates avoid the growth of metal particles and ensure carbon products. At the nanoscale, graphitization is achieved.
Regular hollow spherical graphite nanocapsules are prepared, which have high graphitization degree, specific surface area and pore volume, high preparation efficiency and low cost. They are suitable for a variety of industrial lignins and can flexibly control the size of carbon products and the number of graphite layers.
Smart Images

Figure CN118754116A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano-graphite carbon material preparation, relates to the application of lignin, and specifically relates to a method for preparing graphite nano-capsules from lignin and the graphite nano-capsules. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Graphite nanocapsules are nano-spherical hollow structures wrapped by graphene layers. They have excellent conductivity, high specific surface area, large pore volume and chemical stability. They have many applications in drug delivery, electronic devices, biosensors, energy storage technology and other fields. At present, the methods for preparing graphite nanocapsules mainly include template method, chemical vapor deposition method and solvent-assisted self-assembly method, but they generally have problems such as high raw material cost, complex process, high energy consumption and poor biocompatibility. Therefore, it is urgent to develop a green, low-cost and rapid method for preparing high-quality graphite nanocapsules.
[0004] Lignin is the only renewable aromatic polymer in nature, with a carbon content of up to 60%, abundant industrial reserves, low price, rich hydrophilic and hydrophobic functional groups, and the ability to self-assemble in a solution system. It is an ideal precursor for preparing carbon nanocapsules. However, most existing lignin carbon nanocapsules are amorphous carbon, which is difficult to graphitize, resulting in poor activity, stability, and conductivity. Ultra-high temperature heat treatment (>2000℃) can increase the degree of graphitization of carbon nanocapsules, but it will cause the capsule structure to collapse.
[0005] The patent application with publication number CN111285349A discloses a method for preparing highly graphitized boron-doped carbon nanocapsules. In this method, natural halloysite powder and a sugar compound are first subjected to hydrothermal treatment to obtain hydrothermal carbon; after the hydrothermal carbon is soaked in a mixed acid solution to etch a template, it is subjected to high-temperature graphitization treatment under the protection of an external boron source and a protective gas, and finally a highly graphitized boron-doped carbon nanocapsule material is obtained. The raw material cost used in this method is relatively high, the preparation efficiency is relatively low, and it is not suitable for lignin.
[0006] The patent with publication number CN107754793A discloses a method for preparing a catalyst of porous graphite nanocapsules coated with active metals. The method first synthesizes a carbon-metal precursor from an active metal precursor, an auxiliary metal precursor, and a carbon precursor including lignin, and then carbonizes it in a carbon-containing atmosphere to obtain a porous graphite-coated metal nanoparticle composite material, and further obtains porous graphite nanocapsules by acid washing. The method requires a carbon-containing atmosphere as a second carbon source, and the obtained graphite nanocapsules have a low degree of graphitization, a relatively complex preparation process, and a high cost. The acid washing process is prone to equipment corrosion and environmental pollution.
[0007] The patent with publication number CN115799499A discloses a method for preparing hollow spherical graphite particles. In this method, carbon sources including lignin are pre-carbonized to obtain carbon powder, which is then mixed with a metal catalyst to obtain composite particles. After isostatic pressing, the composite particles are carbonized at high temperature and pickled to obtain hollow spherical graphite. The hollow spherical graphite prepared by this method has a high degree of graphitization, but its size is micrometer-level, and it also has the problems of complex preparation process, high cost, and environmental unfriendliness.
[0008] In summary, it is difficult to prepare graphite nanocapsules using lignin as the sole carbon source with high efficiency and low cost in the existing technology, and it is unable to meet the high-value utilization of lignin and the green, low-cost and rapid preparation of graphite nanocapsules. Summary of the invention
[0009] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing graphite nanocapsules from lignin and graphite nanocapsules. The method of the present invention can prepare graphite nanocapsules with regular and uniform morphology, solving the problems of high preparation cost, complex process, uneven quality and narrow applicability of graphite nanocapsules in the prior art.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] In a first aspect, a method for preparing graphite nanocapsules from lignin comprises the following steps:
[0012] S1, mixing lignin, transition metal salt and water, and dispersing them evenly to obtain a lignin-metal salt mixed solution;
[0013] S2, pre-freezing the lignin-metal salt mixed solution with liquid nitrogen, and then freeze-drying to obtain a lignin-metal salt complex;
[0014] S3, heating the lignin-metal salt complex to 600-900°C at a heating rate of 5-20°C / min for slow pyrolysis to obtain metal-loaded lignin pyrolysis charcoal;
[0015] S4. The metal-loaded lignin pyrolysis carbon is subjected to flash Joule heating to obtain hollow graphite nanocapsules.
[0016] In a second aspect, a graphite nanocapsule is obtained by the method described in the first aspect of the present invention.
[0017] In a third aspect, a use of the graphite nanocapsule described in the second aspect of the present invention in drug delivery, electronic devices, biosensing or energy storage.
[0018] The beneficial effects of the present invention are:
[0019] 1. The present invention utilizes liquid nitrogen freeze drying to quickly obtain a well-dispersed nano-lignin-metal salt complex; placing the lignin-metal salt complex in a tubular furnace for slow pyrolysis can convert the metal salt into metal nanoparticles to obtain a metal-loaded lignin pyrolysis carbon with strong conductivity; flash Joule heating can instantly heat the metal-loaded lignin pyrolysis carbon to an ultra-high temperature (3000K) and rapidly cool it, so that the pyrolysis carbon is rapidly and deeply carbonized; the metal nanoparticles can undergo a dissolution-precipitation reaction with carbon atoms at this extremely high temperature to form a graphite carbon layer on the surface, while the metal particles rapidly sublimate to form a hollow graphite nanocapsule. In addition, the extremely fast heating and cooling rates can avoid the growth of metal particles, ensuring that the scale of the carbon product is at the nanometer level. The above principles make this preparation method applicable to a variety of industrial lignins, and the size and number of graphite layers of the carbon product can be flexibly regulated.
[0020] 2. The graphite nanocapsules prepared by the present invention have a regular hollow spherical structure, adjustable size and wall thickness, high graphitization degree, specific surface area and pore volume. Compared with existing graphite nanocapsule products, the preparation efficiency is higher, the cost is lower, and it is more in line with the structural characteristics of graphite nanocapsules. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0022] Figure 1 This is a flow chart of a method for preparing graphite nanocapsules from lignin according to an embodiment of the present invention;
[0023] Figure 2 This is a microscopic morphology of the graphite nanocapsules prepared in Example 1 of the present invention;
[0024] Figure 3 The XRD pattern of the graphite nanocapsules prepared in Example 1 of the present invention;
[0025] Figure 4This is a diagram of N2 isothermal adsorption and desorption of graphite nanocapsules prepared in Example 1 of the present invention;
[0026] Figure 5 This is a microscopic morphology of the graphite nanocapsules prepared in Example 2 of the present invention;
[0027] Figure 6 This is a microscopic morphology of the graphite nanocapsules prepared in Comparative Example 1 of the present invention;
[0028] Figure 7 This is a microscopic morphology of the graphite nanocapsules prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0029] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0031] The flash Joule heating (FJH) described in the present invention refers to heating in a quartz tube by discharging a high voltage (above 60V) in an instant (less than 1 second) to a high temperature of over 3000K. After heating, most of the heat is dissipated through black body radiation, so that the temperature of the quartz tube is relatively low, and rapid cooling can be achieved through the quartz tube.
[0032] In view of the fact that it is difficult to prepare graphite nanocapsules using lignin as the sole carbon source with high efficiency and low cost using existing methods, the present invention provides a method for preparing graphite nanocapsules using lignin and graphite nanocapsules.
[0033] A typical embodiment of the present invention provides a method for preparing graphite nanocapsules from lignin, comprising the following steps:
[0034] S1. Mix lignin, transition metal salt and water, and disperse them evenly to obtain a lignin-metal salt mixed solution.
[0035] S2, pre-freezing the lignin-metal salt mixed solution with liquid nitrogen, and then freeze-drying to obtain a lignin-metal salt complex;
[0036] S3, heating the lignin-metal salt complex to 600-900°C at a heating rate of 5-20°C / min for slow pyrolysis to obtain metal-loaded lignin pyrolysis charcoal;
[0037] S4. The metal-loaded lignin pyrolysis carbon is subjected to flash Joule heating to obtain hollow graphite nanocapsules.
[0038] In the present invention, liquid nitrogen freeze drying can avoid agglomeration of lignin particles and transition metal salts, thereby obtaining nano-lignin-metal composites; slow pyrolysis in a tubular furnace can convert the lignin-metal composites into lignin pyrolysis carbon loaded with nano-metal particles having strong conductivity; flash Joule heating can heat the carbon nanosheets to a temperature of about 3000 K in a very short time, and transition metals can be converted into metal nanoparticles within this temperature range, and amorphous carbon can be dissolved to precipitate graphite carbon layers, while the transition metals are quickly sublimated and removed at ultra-high temperatures, thereby finally obtaining graphite nanocapsules.
[0039] The lignin described in the present invention may be at least one of groundwood lignin, alkali lignin, Kraft lignin, organic solvent lignin, lignin sulfonate and hydrolyzed lignin.
[0040] In the transition metal salt of the present invention, the transition metal is a transition metal that can catalyze the production of graphene, such as iron, cobalt, nickel, copper, molybdenum, etc.; the salt can be an inorganic salt, such as chloride, nitrate, sulfate, phosphate, etc., or an organic salt, such as acetate, oxalate, citrate, etc. In some embodiments, the transition metal salt includes at least one of nickel acetate, nickel nitrate, nickel sulfate, nickel chloride, ferric acetate, ferric nitrate, ferric sulfate, ferric chloride, cobalt acetate, cobalt nitrate, cobalt sulfate, and cobalt chloride. The transition metal salt used in the present invention is cheap, easy to obtain, highly soluble, simple to operate, and has a wide range of applications.
[0041] In order to avoid the introduction of other impurities, the water used in the process of preparing the lignin-metal salt mixed solution of the present invention is deionized water.
[0042] In order to make lignin and transition metal salt dispersed uniformly in water, in some embodiments, the process of uniform dispersion in step S1 is: first stir uniformly, and then perform ultrasonic dispersion. Specifically, in ultrasonic dispersion, the power is 60-100W, the frequency is 40-60Hz, and the time is 10-60min. By controlling the parameters of ultrasonic treatment, it is ensured that lignin and metal salt are fully dispersed and dissolved in the aqueous solution.
[0043] In some embodiments, the concentration of lignin in the lignin-metal salt mixed solution is 5 to 20 mg / mL, and the amount of transition metal salt added is 0.2 to 5 mmol per gram of lignin, preferably 1 to 3 mmol per gram of lignin. The present invention studies and designs the amount of lignin and transition metal salt added to obtain a better mixing ratio. The above-mentioned lignin concentration can ensure that the lignin is fully dispersed in the aqueous solution to obtain nano-lignin spherical particles and reduce the drying time. The above-mentioned amount of metal salt added can ensure that the metal salt is fully dissolved in the aqueous solution and uniformly dispersed on the surface and inside of the lignin particles. When the lignin concentration is higher than the above range, the lignin particles agglomerate and nano-scale spherical lignin particles cannot be obtained. When the metal salt concentration is lower than the above range, the yield of graphite nanocapsules is low; when the metal salt concentration is higher than the above range, the metal particles aggregate and nano-scale graphite capsules cannot be formed.
[0044] When the lignin-metal salt mixed solution is pre-frozen by liquid nitrogen, the lignin metal salt can be directly placed in the liquid nitrogen for pre-freezing. In some embodiments, the lignin-metal salt mixed solution is dripped into the liquid nitrogen for pre-freezing. The dripping method can speed up the pre-freezing speed of the lignin-metal salt mixed solution by liquid nitrogen. At the same time, after pre-freezing, the specific surface area increases, the freeze-drying speed is increased, and the freeze-drying time is reduced, thereby saving costs. Specifically, the dripping speed is 5 to 20 mL / min.
[0045] In some embodiments, freeze drying parameters are: vacuum degree is 1.0×10 -5 ~2.0×10 -5 bar, the cold trap temperature is -60~-70℃, the drying temperature is 15~25℃, and the drying time is 48~72h. By controlling the freeze-drying parameters, the pretreated lignin-metal salt composite powder is ensured to be fully dried.
[0046] The slow pyrolysis of the present invention is achieved by a relatively low heating rate, and its main purpose is to convert metal salts into metal nanoparticles. The size of the metal nanoparticles and the resistivity of the pyrolytic carbon can be adjusted by the heating parameters of the slow pyrolysis. When the heating rate is higher than 20°C / min or the pyrolysis temperature is lower than 600°C, the metal has a low crystallinity, the volatile matter is not fully released, and the conductivity of the lignin pyrolytic carbon is poor; when the heating rate is lower than 5°C / min or the pyrolysis temperature is higher than 900°C, the metal particles are too large to form nanoscale graphite capsules. In some embodiments, the holding time of the slow pyrolysis is 1 to 5 hours. The present invention can better prepare the lignin-metal salt complex into metal-loaded lignin pyrolytic carbon that meets the requirements of flash Joule heating for preparing graphite nanocapsules by adjusting the holding time of the slow pyrolysis. Specifically, the slow pyrolysis is carried out in a tubular furnace.
[0047] In some embodiments, in step S4, the metal-loaded pyrolytic carbon of lignin is loaded with 50 to 200 mg, the voltage during flash Joule heating is 70 to 150 V, the initial resistance is 5 to 20 Ω, and the power-on time is 0.5 to 2 s. The present invention studies and designs the flash Joule heating process to obtain optimal process parameters to ensure that the pyrolytic carbon of lignin is heated to the temperature required to form graphite nanocapsules at a sufficiently high heating rate. Otherwise, when the mixture loading and resistance are higher than this range, or the voltage and power-on time are lower than this range, the temperature or heating rate will be lower, thereby making the success rate of obtaining graphite nanocapsule products lower. The adjustment of the initial resistance is mainly achieved by the compression density of the metal-loaded pyrolytic carbon of lignin. The voltage of the present invention is directly provided by a DC power supply after voltage regulation.
[0048] A second embodiment of the present invention provides a graphite nanocapsule obtained by the above method.
[0049] A third embodiment of the present invention provides an application of the above-mentioned graphite nanocapsule in drug delivery, electronic devices, biosensors or energy storage.
[0050] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0051] Example 1
[0052] A method for preparing graphite nanocapsules from lignin, such as Figure 1 As shown, the following steps are included:
[0053] S1: Kraft lignin and ferric acetate are dissolved in deionized water according to a preset mass ratio, stirred evenly and subjected to ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 5 mg, the amount of ferric acetate added is 3 mmol per gram of lignin, the power of ultrasonic treatment is 100 W, the frequency is 60 Hz, and the time is 60 min.
[0054] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 5 mL / min, and the vacuum degree of the freeze dryer is 1.0×10 -5 bar, cold trap temperature is -70℃, drying temperature is 15℃, and drying time is 72h.
[0055] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 900° C., the heating rate is 5° C. / min, and the holding time is 5 h.
[0056] S4: flash Joule heating the metal-loaded lignin pyrolysis carbon to obtain graphite nanocapsules coated with a small amount of metal impurities. Specifically, the metal-loaded lignin pyrolysis carbon has a loading of 50 mg, a flash Joule heating voltage of 150 V, an initial resistance of 5 Ω, and a power-on time of 2 s.
[0057] The microscopic morphology of the graphite nanocapsules prepared in this embodiment is as follows: Figure 2 As shown. It can be seen that the graphite nanocapsules present a regular hollow spherical structure with an average diameter of 140.31nm, an outer wall of a multilayer graphene structure with an average wall thickness of 23.36nm, a large space inside the capsule, and no obvious metal particles are found to remain. The XRD and N2 adsorption-desorption curves of the graphite nanocapsules prepared in this embodiment are shown in Figure 3 and Figure 4 As shown in Figure 2, the graphitization degree of graphite nanocapsules is as high as 90.1%, and the specific surface area reaches 294.23 m 2 / g, and the pore volume reaches 0.58cc / g.
[0058] Example 2
[0059] A method for preparing graphite nanocapsules from lignin, such as Figure 1 As shown, the following steps are included:
[0060] S1: Alkali lignin and nickel acetate are dissolved in deionized water according to a preset mass ratio, stirred evenly and subjected to ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 10 mg, the amount of nickel acetate added is 2 mmol per gram of lignin, the power of ultrasonic treatment is 90 W, the frequency is 50 Hz, and the time is 30 min.
[0061] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 10 mL / min, and the vacuum degree of the freeze dryer is 1.5×10 -5 bar, cold trap temperature is -60℃, drying temperature is 25℃, and drying time is 72h.
[0062] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 800° C., the heating rate is 10° C. / min, and the holding time is 3 h.
[0063] S4: flash Joule heating the metal-loaded lignin pyrolysis carbon to obtain graphite nanocapsules coated with a small amount of metal impurities. Specifically, the metal-loaded lignin pyrolysis carbon has a loading of 100 mg, a flash Joule heating voltage of 100 V, an initial resistance of 10 Ω, and a power-on time of 0.5 s.
[0064] The microscopic morphology of the graphite nanocapsules obtained in Example 2 is as follows: Figure 5 The corresponding structural parameters are listed in Table 1. It can be seen that the graphite nanocapsules present a regular hollow spherical structure with an average diameter of 86.47nm, a multilayer graphene structure on the outer wall, an average wall thickness of 15.78nm, a small space inside the capsule, and no obvious metal particles are found. The degree of graphitization is 83.2%, and the specific surface area is 306.38m 2 / g, and the pore volume is 0.49cc / g.
[0065] Example 3
[0066] A method for preparing graphite nanocapsules from lignin, such as Figure 1 As shown, the following steps are included:
[0067] S1: dissolving the organic solvent lignin and cobalt acetate in deionized water according to a preset mass ratio, stirring evenly and performing ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 20 mg, the amount of nickel acetate added is 1 mmol per gram of lignin, the power of ultrasonic treatment is 60 W, the frequency is 40 Hz, and the time is 10 min.
[0068] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 20 mL / min, and the vacuum degree of the freeze dryer is 2.0×10 -5 bar, cold trap temperature is -60℃, drying temperature is 25℃, and drying time is 48h.
[0069] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 600° C., the heating rate is 20° C. / min, and the holding time is 1 hour.
[0070] S4: flash Joule heating the metal-loaded lignin pyrolysis carbon to obtain graphite nanocapsules coated with a small amount of metal impurities. Specifically, the metal-loaded lignin pyrolysis carbon has a loading of 200 mg, a flash Joule heating voltage of 70 V, an initial resistance of 20 Ω, and a power-on time of 0.5 s.
[0071] The structural parameters of the graphite nanocapsules prepared in Example 3 are listed in Table 1. The average diameter is 42.84 nm, the outer wall is a multilayer graphene structure, the average wall thickness is 6.01 nm, the internal space of the capsule is small, and no obvious metal particles are found. The degree of graphitization is 74.3%, and the specific surface area is 425.82 m 2 / g, and the pore volume is 0.33cc / g.
[0072] Example 4
[0073] A method for preparing graphite nanocapsules from lignin, such as Figure 1 As shown, the following steps are included:
[0074] S1: dissolving lignin sulfonate and ferric nitrate in deionized water according to a preset mass ratio, stirring evenly and performing ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 15 mg, the amount of nickel acetate added is 2.5 mmol per gram of lignin, the power of ultrasonic treatment is 60 W, the frequency is 40 Hz, and the time is 30 minutes.
[0075] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 20 mL / min, and the vacuum degree of the freeze dryer is 2.0×10 -5 bar, cold trap temperature is -70℃, drying temperature is 25℃, and drying time is 48h.
[0076] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 700° C., the heating rate is 10° C. / min, and the holding time is 4 hours.
[0077] S4: flash Joule heating the metal-loaded lignin pyrolysis carbon to obtain graphite nanocapsules coated with a small amount of metal impurities. Specifically, the metal-loaded lignin pyrolysis carbon has a loading of 150 mg, a flash Joule heating voltage of 120 V, an initial resistance of 10 Ω, and a power-on time of 1 s.
[0078] The structural parameters of the graphite nanocapsules prepared in Example 4 are listed in Table 1. The average diameter is 53.54 nm, the outer wall is a multilayer graphene structure, the average wall thickness is 10.39 nm, the internal space of the capsule is small, and no obvious metal particles are found. The degree of graphitization is 84.6%, and the specific surface area is 321.73 m 2 / g, and the pore volume is 0.41cc / g.
[0079] Table 1 Structural parameters of graphite nanocapsules prepared in Examples 1 to 4
[0080]
[0081]
[0082] Comparative Example 1
[0083] The difference between this comparative example and Example 1 is that the metal-loaded lignin pyrolysis carbon is not subjected to flash Joule heat treatment.
[0084] S1: Kraft lignin and ferric acetate are dissolved in deionized water according to a preset mass ratio, stirred evenly and subjected to ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 5 mg, the amount of ferric acetate added is 3 mmol per gram of lignin, the power of ultrasonic treatment is 100 W, the frequency is 60 Hz, and the time is 60 min.
[0085] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 5 mL / min, and the vacuum degree of the freeze dryer is 1.0×10 -5 bar, cold trap temperature is -70℃, drying temperature is 15℃, and drying time is 72h.
[0086] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 900° C., the heating rate is 5° C. / min, and the holding time is 5 h.
[0087] The microscopic morphology of the carbon material obtained in Comparative Example 1 is as follows Figure 6 As shown, no graphite nanocapsule structure is formed, the metal particles are wrapped by amorphous carbon, and no graphene layer is formed, which indicates that the flash Joule heating treatment is crucial for the formation of the graphite nanocapsule structure.
[0088] Comparative Example 2
[0089] The difference between this comparative example and Example 2 is that the flash Joule heating voltage and the initial resistance are lower than the claimed range.
[0090] S1: Alkali lignin and nickel acetate are dissolved in deionized water according to a preset mass ratio, stirred evenly and subjected to ultrasonic treatment to obtain a mixed solution. Specifically, the mass of lignin added per milliliter of water is 10 mg, the amount of nickel acetate added is 2 mmol per gram of lignin, the power of ultrasonic treatment is 90 W, the frequency is 50 Hz, and the time is 30 min.
[0091] S2: Drop the lignin-metal salt mixed solution into liquid nitrogen and freeze it quickly, then put it into a freeze dryer and dry it under vacuum to obtain a lignin-metal salt complex. Specifically, the dropping speed of the lignin-metal salt mixed solution is 10 mL / min, and the vacuum degree of the freeze dryer is 1.5×10 -5 bar, cold trap temperature is -60℃, drying temperature is 25℃, and drying time is 72h.
[0092] S3: slowly pyrolyzing the lignin-metal salt complex in a tubular furnace to obtain metal-loaded lignin pyrolysis carbon. Specifically, the pyrolysis temperature is 800° C., the heating rate is 10° C. / min, and the holding time is 3 h.
[0093] S4: flash Joule heating the metal-loaded lignin pyrolysis carbon to obtain graphite nanocapsules coated with a small amount of metal impurities. Specifically, the metal-loaded lignin pyrolysis carbon has a loading of 100 mg, a flash Joule heating voltage of 60 V, an initial resistance of 30 Ω, and a power-on time of 0.5 s.
[0094] The microscopic morphology of the graphite nanocapsules obtained in Comparative Example 2 is as follows: Figure 7 As shown in the figure, it can be seen that the graphite nanocapsules present a regular hollow spherical structure with a multilayer graphene structure on the outer wall, but there are obvious metal particles remaining inside the capsules. This shows that the flash Joule heating condition is crucial for the sublimation removal of metal impurities.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing graphite nanocapsules from lignin, characterized in that: The following steps are involved: S1, mixing lignin, transition metal salt and water, and dispersing them evenly to obtain a lignin-metal salt mixed solution; S2, pre-freezing the lignin-metal salt mixed solution with liquid nitrogen, and then freeze-drying to obtain a lignin-metal salt complex; S3, heating the lignin-metal salt complex to 600-900°C at a heating rate of 5-20°C / min for slow pyrolysis to obtain metal-loaded lignin pyrolysis charcoal; S4. The metal-loaded lignin pyrolysis carbon is subjected to flash Joule heating to obtain hollow graphite nanocapsules.
2. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The transition metal salt includes at least one of nickel acetate, nickel nitrate, nickel sulfate, nickel chloride, ferric acetate, ferric nitrate, ferric sulfate, ferric chloride, cobalt acetate, cobalt nitrate, cobalt sulfate, and cobalt chloride.
3. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The process of uniform dispersion in step S1 is: first stirring uniformly, and then ultrasonic dispersion; preferably, in the ultrasonic dispersion, the power is 60 to 100 W, the frequency is 40 to 60 Hz, and the time is 10 to 60 min.
4. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The concentration of lignin in the lignin-metal salt mixed solution is 5-20 mg / mL, and the addition amount of the transition metal salt is 0.2-5 mmol per gram of lignin, preferably 1-3 mmol per gram of lignin.
5. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The lignin-metal salt mixed solution is dripped into liquid nitrogen for pre-freezing; preferably, the dripping speed is 5 to 20 mL / min.
6. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The parameters of freeze drying were: vacuum degree was 1.0×10 -5 ~2.0×10 -5 bar, cold trap temperature is -60~-70℃, drying temperature is 15~25℃, and drying time is 48~72h.
7. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: The holding time for slow pyrolysis is 1 to 5 hours.
8. The method for preparing graphite nanocapsules from lignin as claimed in claim 1, characterized in that: In step S4, the loading amount of the metal-loaded lignin pyrolysis carbon is 50-200 mg, the flash Joule heating is performed, the voltage is 70-150 V, the initial resistance is 5-20 Ω, and the power-on time is 0.5-2 s.
9. A graphite nanocapsule, characterized in that: Obtained by the method according to any one of claims 1 to 8.
10. Use of the graphite nanocapsule according to claim 9 in drug delivery, electronic devices, biosensing or energy storage.
Citation Information
Patent Citations
Lignin microcapsule and method of producing the same
CN105566929A
Porous carbon supported Fischer-Tropsch synthesis catalyst as well as preparation method and application thereof
CN107754793A
Method for preparing boron-doped porous graphene from lignin and product
CN117285035A
Laser pyrolysis method for producing carbon nano-spheres
US20060137487A1
Methods for Synthesizing Graphene from a Lignin Source
US20150307356A1
Cited By
Method for preparing porous boron-doped carbon and co-producing acetovanillone by oxidative depolymerization of lignin
CN122212128A