Polybenzoxazole precursor and preparation method thereof, photosensitive resin composition
By introducing cyclohexyl-containing diamine monomers to form polybenzoxazole precursors, the problems of warping of polyimide and polybenzoxazole during high-temperature thermal curing are solved, and rapid at lower temperatures are achieved Curing and performance-keeping, suitable for microelectronic packaging.
Patent Information
- Application Number
- CN202311742221.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Polyimide and polybenzoxazole cause wafer warping and solder joint cracking during high-temperature thermal curing. Their high-temperature curing temperature limits the performance of the device and requires rapid curing at lower temperatures without loss. Mechanics and thermal properties.
By introducing cyclohexyl-containing diamine monomers, polybenzoxazole precursors are formed, reducing their thermal curing temperature, improving mechanical and thermal properties, and a six-membered ring side is prepared through specific polymerization and capping steps. A polybenzoxazole precursor based on a photosensitive resin composition.
It realizes rapid curing of polybenzoxazole at lower temperatures, maintains excellent mechanical, thermal and chemical corrosion resistance, and is suitable for microelectronic packaging fields, especially fan-out wafer-level packaging and flat-plate-level packaging.
Smart Images

Figure CN117866200B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of photosensitive polymers, and in particular to a polybenzoxazole precursor, a preparation method of the polybenzoxazole precursor, and a photosensitive resin composition. Background Art
[0002] Due to their excellent thermal, mechanical and electrical properties and good chemical corrosion resistance, polyimide (PI) and polybenzoxazole (PBO) have been widely used as stress buffer coatings and cover coating films for wafer-level chip scale packages with copper redistribution layers (RDL) to improve the reliability of semiconductor devices and provide precise bump height uniformity and bump shape control for the most complex wafer layouts while maintaining low deposition internal stress. Advanced packaging technologies such as multi-layer RDL, 3D stacking and heterogeneous integration (HI) enable various chips and chiplets with different functions, capabilities, sizes and sources to work together in the system, connected on substrates ranging from silicon and fan-out to organic and glass.
[0003] Photosensitive polybenzoxazole (PBO) has photosensitive properties. Through coating, exposure, and development to show patterns, it has been widely used as an insulating protective layer in the field of microelectronic packaging. The curing temperature of PBO is generally above 300°C. In the high-temperature thermal curing process of fan-out wafer-level packaging (FOWLP) and fan-out flat-panel packaging (FOPLP), the wafer may warp, and the solder joints of the low-melting solder of the plastic-encapsulated circuit may crack, fall off, and recrystallize, which seriously damages the performance of the plastic-encapsulated device. Therefore, considering the fan-shaped external stress and the need to transition to full Cu interconnection, the high-temperature thermal curing temperature of PBO is limited to 250°C. Therefore, PBO must be able to cure faster at a lower temperature, and at the same time, it should not lose its adhesion to the copper substrate, mechanical properties, thermal properties and other properties.
[0004] Compared with high-temperature curing PBO, low-temperature curing PBO can solve the problems such as wafer warping that may be caused by high-temperature curing, while maintaining mechanical properties and thermal properties. Therefore, low-temperature curing PBO has become the focus of research in recent years. Summary of the invention
[0005] The purpose of the present application is to provide a polybenzoxazole precursor that can effectively reduce the thermal curing temperature while also having good mechanical properties, thermal properties, photolithography properties and chemical corrosion resistance.
[0006] To achieve the above object, the technical solution of the present application provides a polybenzoxazole precursor, which is formed by reacting a diamine monomer and a dicarboxylic acid monomer; wherein the diamine monomer comprises a diamine compound represented by formula (1) and / or formula (2):
[0007]
[0008] The dicarboxylic acid monomer has a structure shown in formula (3):
[0009]
[0010] In formula (3), X is a divalent organic group, which is an aliphatic group or an aromatic group; and Z is selected from a hydroxyl group or a halogen group.
[0011] In some embodiments of the present application, the monovalent organic group is selected from C1-C12 alkyl, C1-C12 alkoxy, C6-C10 aromatic, C6-C10 phenoxy, C6-C10 benzyl and C6-C10 benzyloxy; in R1-R5 and in R 11 ~R 51 There are 0 to 3 groups independently selected from the monovalent organic groups in each of R1 to R5 and in R 11 ~R 51 wherein one group is independently selected from the monovalent organic group, and the remaining groups are hydrogen, or R1 to R5 and R 11 ~R 51 All are hydrogen.
[0012] In some embodiments of the present application, X is a C6-C48 aromatic group; preferably, X is a C6-C24 aromatic group; further preferably, X is Wherein A is selected from a single bond, an alkylene group, -O-, -S-, -C(CF3)2- and -C(CH3)2-, * represents the linking portion to the carbonyl group in the formula (3).
[0013] In some embodiments of the present application, the dicarboxylic acid monomer is selected from at least one of an aromatic dicarboxylic acid, an aliphatic dicarboxylic acid, a dihalide or dicarboxylic acid ester of the aromatic dicarboxylic acid, and a dihalide or dicarboxylic acid ester of the aliphatic dicarboxylic acid; preferably, the aromatic dicarboxylic acid is selected from isophthalic acid, terephthalic acid, 5-tert-butylisophthalic acid, 5-bromoisophthalic acid, 5-fluoroisophthalic acid, 5-chloroisophthalic acid, 2,6-naphthalene dicarboxylic acid, 4,4 At least one of '-dicarboxybiphenyl, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxytetraphenylsilane, bis(4-carboxyphenyl)sulfone, 2,2-bis(p-carboxyphenyl)propane and 2,2-bis(4-carboxyphenyl)-1,1,1,3,3,3-hexafluoropropane; preferably, the aliphatic dicarboxylic acid is selected from at least one of oxalic acid, malonic acid, succinic acid, 1,2-cyclobutanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid and 1,3-cyclopentanedicarboxylic acid.
[0014] In some embodiments of the present application, the diamine monomer further comprises a diamine compound represented by formula (4):
[0015]
[0016] In formula (4), Y is a tetravalent organic group having at least two hydroxyl groups, and the tetravalent organic group is an aliphatic group or an aromatic group; preferably, the tetravalent organic group is an aromatic group.
[0017] In some embodiments of the present application, Y is selected from the following tetravalent organic groups:
[0018]
[0019] Among them, one of 1* and 2* represents the connection part with the amino group in formula (4), and the other represents the connection part with the hydroxyl group in Y in formula (4).
[0020] In some embodiments of the present application, the structural formula of the polybenzoxazole precursor is as shown in formula (I) or formula (II):
[0021]
[0022] In formula (I) and formula (II), X is Y is
[0023] n and n1 are 1-100, m and m1 are 0-100; preferably, n and n1 are 1-40, m and m1 are 15-40.
[0024] The present application also provides a method for preparing a polybenzoxazole precursor, comprising the following steps: S1: dissolving a diamine monomer in a first solvent to obtain a diamine monomer solution, wherein the molar percentage of the diamine compound represented by formula (1) and / or formula (2) in the diamine monomer is 10% to 100%; S2: adding a dicarboxylic acid monomer represented by formula (3) to the diamine monomer solution to cause a polymerization reaction to obtain a polybenzoxazole precursor solution.
[0025] In some embodiments of the present application, the first solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, tetrahydrofuran, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate;
[0026] And / or, step S2 satisfies one of the following conditions: 1) adding the dicarboxylic acid monomer represented by formula (3) under ice bath conditions of 0 to 10° C., and the polymerization reaction temperature is 0 to 35° C., and the polymerization reaction time is 2 hours to 10 hours; 2) the molar ratio of the diamine monomer to the dicarboxylic acid monomer represented by formula (3) is 1:(0.5 to 1);
[0027] And / or, the preparation method further comprises step S3: adding a capping agent to the polybenzoxazole precursor solution to carry out a capping reaction to obtain a capped polybenzoxazole precursor solution, wherein the molar ratio of the capping agent to the diamine monomer is (0.02-0.2):1, the temperature of the capping reaction is 10°C-35°C, and the time is 1 hour-4 hours; preferably, the capping agent is selected from at least one of phthalic anhydride, maleic anhydride, succinic anhydride, 2,3-pyrazine dianhydride, tetrafluorophthalic anhydride, 2,3-naphthalene dicarboxylic anhydride, hexahydrophthalic anhydride, nadic anhydride, tetrahydrophthalic anhydride, 4-phenylalkynylphthalic anhydride, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, phenylsuccinic anhydride, and 2,2'-biphenyl dicarboxylic anhydride;
[0028] And / or, the preparation method further comprises step S4: dropping the polybenzoxazole precursor solution or the blocked polybenzoxazole precursor solution into deionized water, and washing and drying the precipitate to obtain a dry polybenzoxazole precursor.
[0029] The present application also provides a photosensitive resin composition, which comprises the following components by weight: 100 parts of the polybenzoxazole precursor described in any one of the above items, 5 to 40 parts of a photosensitive agent, and 30 to 10,000 parts of a second solvent; preferably, the photosensitive agent comprises at least one of a photoacid generator, a photobase generator, a crosslinking agent, a thermal acid generator, a sensitizer, a sealing agent, a surfactant, a leveling agent, and fine particles; preferably, the second solvent comprises at least one of N,N'-dimethylformamide, N-methylpyrrolidone, N-ethyl-2-pyrrolidone, N,N'-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, γ-butyrolactone and diethylene glycol monomethyl ether.
[0030] In the present application, a cyclohexyl-containing diamine monomer is introduced so that the prepared polybenzoxazole precursor contains a six-membered ring side group. The large steric hindrance limits the close arrangement of the polybenzoxazole precursor molecular chain, so that the energy required for the polybenzoxazole precursor in the heating ring closing process is reduced, so that the polybenzoxazole precursor can achieve closed-loop curing at a lower curing temperature, improve the cyclization rate, and have better mechanical properties, thermal properties, lithography properties and chemical corrosion resistance, effectively avoiding the problem that the low heat resistance devices may be damaged during the high-temperature thermal curing process in the fields of fan-out wafer-level packaging and fan-out flat-panel packaging.
[0031] The photosensitive resin composition containing the polybenzoxazole precursor can be used as a positive photoresist developed by alkaline water, can form a high-resolution pattern during photolithography, and has excellent mechanical and thermal properties. When applied to a black matrix, the relevant properties of the black matrix can be improved.
[0032] The preparation method of the polybenzoxazole precursor of the present application has readily available raw materials, simple preparation steps and process conditions and is easy to control, and is convenient for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them:
[0034] Figure 1 is a structural formula of a polybenzoxazole precursor of an embodiment of the present application;
[0035] Figure 2 is another structural formula of the polybenzoxazole precursor of the embodiment of the present application;
[0036] Figure 3 FT-IR image of the polybenzoxazole film prepared in Example 7 of the present application;
[0037] Figure 4 This is a test chart of the lithography performance of the photosensitive resin composition prepared in Example 1 of the present application;
[0038] Figure 5 This is a test diagram of the lithography performance of the photosensitive resin composition prepared in Example 2 of the present application;
[0039] Figure 6 This is a 3D image of the film surface after the cured film of Example 16 of the present application was soaked in N-methylpyrrolidone. DETAILED DESCRIPTION
[0040] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.
[0041] Based on the problem that high-temperature thermal curing may cause damage to devices with low heat resistance in fields such as fan-out wafer-level packaging and fan-out flat-panel packaging, the present application improves polybenzoxazole by introducing six-membered ring side groups into the molecular chain of the polybenzoxazole precursor, thereby reducing its thermal curing temperature while maintaining other properties to meet the requirements.
[0042] Specifically, the present invention provides a polybenzoxazole precursor, which is formed by reacting a diamine monomer and a dicarboxylic acid monomer. The diamine monomer includes a diamine compound represented by formula (1) and / or formula (2):
[0043]
[0044] In the formula (1) and the formula (2), R1 to R5, R 11 ~R 51 are independently selected from hydrogen or a monovalent organic group.
[0045] In some preferred embodiments, the monovalent organic group is selected from C1-C12 alkyl, C1-C12 alkoxy, C6-C10 aromatic group, C6-C10 phenoxy, C6-C10 benzyl and C6-C10 benzyloxy. The C1-C12 alkyl groups include, for example, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl and hexyl groups; the C1-C12 alkoxy groups include, for example, methoxy, ethoxy, propoxy, butoxy and pentyloxy groups; the C6-C10 aromatic groups include, for example, phenyl, tolyl, methylphenyl, dimethylphenyl, ethylphenyl, diethylphenyl, propylphenyl, butylphenyl, fluorophenyl, pentafluorophenyl, chlorophenyl, bromophenyl, methoxyphenyl, dimethoxyphenyl, ethoxyphenyl, diethoxyphenyl, methoxybenzyl, dimethoxybenzyl, ethoxybenzyl, diethoxybenzyl, aminophenyl, aminobenzyl, nitrophenyl, nitrobenzyl and cyanophenyl groups. , cyanobenzyl, phenethyl, phenylpropyl, phenylamino, diphenylamino, biphenyl and naphthyl, etc.; the C6~C10 phenoxy group is, for example, methylphenoxy, ethylphenoxy, propylphenoxy, dimethylphenoxy, diethylphenoxy, methoxyphenoxy, ethoxyphenoxy and dimethoxyphenoxy, etc.; the C6~C10 benzyl group is, for example, benzyl, methylbenzyl, ethylbenzyl, propylbenzyl, dimethylbenzyl, methoxybenzyl, ethoxybenzyl and methoxybenzyl, etc.; the C6~C10 benzyl group is, for example, methylbenzyl, ethylbenzyl, propylbenzyl, dimethylbenzyl, methoxybenzyl, ethoxybenzyl and methoxybenzyl, etc.
[0046] In order to further reduce the curing temperature of the photosensitive resin composition and improve the heat resistance and chemical corrosion resistance of the cured film, 11 ~R 51 There are 0 to 3 groups independently selected from the monovalent organic groups in each of R1 to R5 and in R 11 ~R 51 In each of them, there is a group independently selected from the monovalent organic group, and the remaining groups are hydrogen, that is, in R1 to R5, there is a group selected from the monovalent organic group, and the remaining groups are hydrogen, and in R 11 ~R 51 There is one group selected from the monovalent organic group, and the remaining groups are hydrogen; or, R1 to R5 and R 11 ~R 51 All are hydrogen.
[0047] The dicarboxylic acid monomer has a structure shown in formula (3):
[0048]
[0049] In formula (3), X is a divalent organic group, which is an aliphatic group or an aromatic group, preferably an aromatic group of C6 to C48, and more preferably an aromatic group of C6 to C24. More preferably, X is Wherein A is selected from a single bond, an alkylene group, -O-, -S-, -C(CF3)2- and -C(CH3)2-, * represents the carbonyl group in formula (2) The connection part.
[0050] In order to further improve the developability of the photosensitive resin composition and the mechanical properties of the cured film, A is -O-, and X is
[0051] In formula (3), Z is selected from a hydroxyl group or a halogen group. In order to further improve the yield, Z is preferably a halogen group.
[0052] In some embodiments, the dicarboxylic acid monomer is selected from at least one of aromatic dicarboxylic acids, aliphatic dicarboxylic acids, dihalides of the aromatic dicarboxylic acids, dicarboxylic acid esters of the aromatic dicarboxylic acids, dihalides of the aliphatic dicarboxylic acids, and dicarboxylic acid esters of the aliphatic dicarboxylic acids. Preferably, the aromatic dicarboxylic acid is selected from at least one of isophthalic acid, terephthalic acid, 5-tert-butylisophthalic acid, 5-bromoisophthalic acid, 5-fluoroisophthalic acid, 5-chloroisophthalic acid, 2,6-naphthalene dicarboxylic acid, 4,4'-dicarboxybiphenyl, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxytetraphenylsilane, bis(4-carboxyphenyl)sulfone, 2,2-bis(p-carboxyphenyl)propane, and 2,2-bis(4-carboxyphenyl)-1,1,1,3,3,3-hexafluoropropane. Preferably, the aliphatic dicarboxylic acid is at least one selected from oxalic acid, malonic acid, succinic acid, 1,2-cyclobutanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid and 1,3-cyclopentanedicarboxylic acid.
[0053] In order to further improve the developability of the photosensitive resin composition and the mechanical properties of the cured film, the dicarboxylic acid monomer is preferably 4,4'-dicarboxyl diphenyl ether (ie, 4,4'-diphenyl ether dicarboxylic acid) and its dihalide (eg, 4,4'-diacyl chloride diphenyl ether).
[0054] In some embodiments, the diamine monomer further comprises a diamine compound represented by formula (4): In formula (4), Y is a tetravalent organic group having at least two hydroxyl groups. The tetravalent organic group may be an aliphatic group or an aromatic group, preferably an aromatic group. The positional relationship between the hydroxyl group in Y and the amino group in formula (4) is preferably ortho. The number of carbon atoms in Y is preferably 6 to 48, more preferably 6 to 24.
[0055] In some preferred embodiments, Y is selected from the following tetravalent organic groups:
[0056]
[0057] In the above-mentioned tetravalent organic group, one of 1* and 2* represents a linking portion to the amino group (-NH2) in formula (4), and the other represents a linking portion to the hydroxyl group.
[0058] In order to further improve the solubility and photosensitivity of the polybenzoxazole precursor in the alkaline developer, Y is In this case, the diamine compound represented by formula (4) is 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, and its structural formula is as follows:
[0059]
[0060] In some preferred embodiments, Y is The diamine compound represented by formula (4) is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, and its structural formula is as follows:
[0061]
[0062] In some embodiments, the polybenzoxazole precursor has a structural formula as follows: Figure 1 Formula I shown or Figure 2 In formula (I) and formula (II), X is Y is n and n1 are 1 to 100, and m and m1 are 0 to 100. More preferably, n and n1 are 1 to 40, and m and m1 are 15 to 40.
[0063] In order to further improve the solubility of the photosensitive resin composition in the alkaline developer, the number average molecular weight (Mn) of the polybenzoxazole precursor is preferably 2000-40000, more preferably 3000-20000; the weight average molecular weight (Mw) of the polybenzoxazole precursor is preferably 4000-80000, more preferably 6000-40000. The Mw / Mn of the polybenzoxazole precursor is preferably 1-5, more preferably 1-3. In the embodiments of the present application, the number average molecular weight and the weight average molecular weight are both measured by gel permeation chromatography (GPC).
[0064] In order to further improve the photolithography performance and low temperature curing performance of the polybenzoxazole precursor, in formula (I) and formula (II), n / (m+n)×100%≥0.1%, n1 / (m1+n1)×100%≥0.1%. More preferably, n / (m+n)×100%≥0.5%, n1 / (m1+n1)×100%≥5%. Among them, n / (m+n)×100% also represents the length ratio of the polymer chain segment formed by the polymerization of the diamine compound shown in formula (1) and the dicarboxylic acid monomer in the total molecular chain of the polybenzoxazole precursor, and also represents the molar percentage of the diamine compound shown in formula (1) in the diamine monomer. Similarly, n1 / (m1+n1)×100% also represents the length ratio of the polymer chain segment formed by the polymerization of the diamine compound represented by formula (2) and the dicarboxylic acid monomer in the total molecular chain of the polybenzoxazole precursor, and also represents the molar percentage of the diamine compound represented by formula (2) in the diamine monomer.
[0065] In some embodiments, the diamine monomer may include, in addition to the diamine compound represented by formula (1) and / or formula (2) and the diamine compound represented by formula (4), at least one of the following diamine compounds: 4,4'-bis(3-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, m-aminobenzylamine, p-aminobenzylamine, 3, 3'-Diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, bis[4-(4-aminophenoxy)phenyl]methane, 1,1-bis[4-(4 1,2-bis[4-(4-aminophenoxy)phenyl]ethane, 1,1-bis[4-(4-aminophenoxy)phenyl]propane, 1,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,1-bis[4-(4-aminophenoxy)phenyl]butane, 1,3-bis[4-(4-aminophenoxy)phenyl]butane, 1,4-bis[4-(4-aminophenoxy)phenyl]butane, 2,2-bis[4-(4-aminophenoxy)phenyl]butane, 2,3-bis[4-(4-aminophenoxy)phenyl ] butane, 2-[4-(4-aminophenoxy)phenyl]-2-[4-(4-aminophenoxy)-3-methylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)-3-methylphenyl]propane, 2-[4-(4-aminophenoxy)phenyl]-2-[4-(4-aminophenoxy)-3,5-dimethylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)-3,5-dimethylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfoxide, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(3-aminophenoxy)benzoyl]benzene, 4,4'-bis[(3-aminophenoxy)benzoyl]benzene, 1,1-bis[4-(3-aminophenoxy)phenyl]propane, 1,3-bis [4-(3-aminophenoxy)phenyl]propane, 3,4'-diaminodiphenyl sulfide, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, bis[4-(3-aminophenoxy)phenyl]methane, 1,1-bis[4-(3-aminophenoxy)phenyl]ethane, 1,2-bis[4-(3-aminophenoxy)phenyl]ethane, bis[4-(3-aminophenoxy)phenyl]sulfoxide, 4,4'-bis[3-(4-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[3-(3-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, 4,4'-bis[ 4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, bis[4-{4-(4-aminophenoxy)phenoxy}phenyl]sulfone, 1,4-bis[4-(4-aminophenoxy)phenoxy-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-aminophenoxy)phenoxy-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-trifluoromethylphenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-fluorophenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-methylphenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-cyanopheneoxy)-α, α-dimethylbenzyl]benzene, 3,3'-diamino-4,4'-diphenoxybenzophenone, 4,4'-diamino-5,5'-diphenoxybenzophenone, 3,4'-diamino-4,5'-diphenoxybenzophenone, 3,3'-diamino-4-phenoxybenzophenone, 4,4'-diamino-5-phenoxybenzophenone, 3,4'-diamino -4-phenoxybenzophenone, 3,4'-diamino-5'-phenoxybenzophenone, 3,3'-diamino-4,4'-diphenyloxybenzophenone, 4,4'-diamino-5,5'-diphenyloxybenzophenone, 3,4'-diamino-4,5'-diphenyloxybenzophenone, 3,3'-diamino-4-biphenyloxybenzophenone, 4,4'-Diamino-5-biphenyloxybenzophenone, 3,4'-diamino-4-biphenyloxybenzophenone, 3,4'-diamino-5'-biphenyloxybenzophenone, 1,3-bis(3-amino-4-phenoxybenzoyl)benzene, 1,4-bis(3-amino-4-phenoxybenzoyl)benzene, 1,3-bis(4-amino-5-phenoxybenzoyl)benzene, 1,4-bis(4-amino-5-phenoxybenzoyl)benzene, 1,3-bis(3-amino-4-phenoxybenzoyl)benzene 1,4-bis(3-amino-4-biphenyloxybenzoyl)benzene, 1,3-bis(4-amino-5-biphenyloxybenzoyl)benzene, 1,4-bis(4-amino-5-biphenyloxybenzoyl)benzene, 2,6-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzonitrile and all or part of the hydrogen atoms on the aromatic ring of the above aromatic diamines are replaced by halogen atoms, alkyl or alkoxy groups having 1 to 3 carbon atoms , cyano, or aromatic diamines in which all or part of the hydrogen atoms of an alkyl or alkoxy group are replaced by halogen atoms and the number of carbon atoms is 1 to 3; 4,4'-methylenebis(cyclohexylamine), isophoronediamine, trans-1,4-diaminocyclohexane, cis-1,4-diaminocyclohexane, 1,4-cyclohexanebis(methylamine), 2,5-bis(aminomethyl)bicyclo[2,2,1]heptane, 2,6-bis(aminomethyl)bicyclo[ aliphatic diamines such as 1,3-diaminoadamantane, 2,2-bis(4-aminocyclohexyl)propane, 2,2-bis(4-aminocyclohexyl)hexafluoropropane, 1,3-propylenediamine, 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, and 1,9-nonamethylenediamine.
[0066] The present application also provides a method for preparing the polybenzoxazole precursor, comprising the following steps:
[0067] S1: dissolving a diamine monomer in a first solvent to obtain a diamine monomer solution, wherein the molar percentage of the diamine compound represented by formula (1) and / or formula (2) in the diamine monomer is 10% to 100%;
[0068] S2: adding the dicarboxylic acid monomer represented by formula (3) to the diamine monomer solution to cause a polymerization reaction to obtain a polybenzoxazole precursor solution.
[0069] In some embodiments, in step S1, the first solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, tetrahydrofuran, 1,3-dimethyl-2-imidazolidinone (DMI), γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate.
[0070] In some preferred embodiments, step S2 satisfies one of the following conditions: 1) adding the dicarboxylic acid monomer represented by formula (3) under ice bath conditions of 0 to 10° C., and the polymerization reaction temperature is 0 to 35° C., and the polymerization reaction time is 2 hours to 10 hours; 2) the molar ratio of the diamine monomer to the dicarboxylic acid monomer represented by formula (3) is 1:(0.5 to 1).
[0071] In some embodiments, the preparation method further includes step S3: adding a capping agent to the polybenzoxazole precursor solution to carry out a capping reaction to obtain a capped polybenzoxazole precursor solution, wherein the molar ratio of the capping agent to the diamine monomer is (0.02-0.2):1, and the temperature of the capping reaction is 10°C-35°C, and the time is 1 hour-4 hours; preferably, the capping agent is selected from at least one of phthalic anhydride, maleic anhydride, succinic anhydride, 2,3-pyrazine dianhydride, tetrafluorophthalic anhydride, 2,3-naphthalene dicarboxylic anhydride, hexahydrophthalic anhydride, naphthalene dianhydride, tetrahydrophthalic anhydride, 4-phenylalkynylphthalic anhydride, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, phenylsuccinic anhydride, and 2,2'-biphenyl dicarboxylic anhydride.
[0072] In some embodiments, the preparation method further comprises step S4: dropping the polybenzoxazole precursor solution or the blocked polybenzoxazole precursor solution into deionized water, and washing and drying the precipitate to obtain a dried polybenzoxazole precursor. In some embodiments, the cleaning liquid for washing the solid resin can be selected from at least one of distilled water, methanol, ethanol, isopropanol, etc. During drying, at least one of a blast oven, a vacuum oven, a freeze dryer, a fluidized dryer, etc. can be used.
[0073] The embodiment of the present application also provides a photosensitive resin composition, comprising the above-mentioned polybenzoxazole precursor having cyclohexyl side groups and a photosensitizer. The use of the above-mentioned polybenzoxazole precursor having cyclohexyl side groups as a photosensitive polymer can significantly reduce the curing temperature of the photosensitive resin composition. When the photosensitive resin composition is applied to a black matrix, the relevant properties of the black matrix can be improved.
[0074] In some embodiments, in addition to the above-mentioned polybenzoxazole precursor having a cyclohexyl side group, the photosensitive resin composition may further include other polybenzoxazole precursors.
[0075] In some preferred embodiments, in the photosensitive resin composition, the polybenzoxazole precursor having cyclohexyl side groups accounts for 50% to 99% of the total mass of the non-volatile components, and more preferably, 60% to 99%.
[0076] In some embodiments, in the photosensitive resin composition, the polybenzoxazole precursor having cyclohexyl side groups is 100 parts by weight, and the photosensitizer is preferably 5 to 40 parts by weight, and more preferably 10 to 30 parts by weight.
[0077] In some embodiments, the photosensitizer includes a photoacid generator and / or a photobase generator, etc. In order to further improve the resolution, the photosensitizer is preferably a photoacid generator. The photoacid generator is a compound that generates acid by light irradiation of ultraviolet light, visible light, etc. As an example, the photoacid generator includes at least one of naphthoquinone diazide compounds, diaryl sulfonium salts, triaryl sulfonium salts, dialkylbenzylmethyl sulfonium salts, diaryl iodonium salts, aryl diazonium salts, aromatic tetracarboxylic acid esters, aromatic sulfonates, nitrobenzyl esters, aromatic N-oxyimide sulfonates, aromatic sulfonamides and benzoquinone diazonium sulfonates. Further preferably, the photoacid generator is a naphthoquinone diazide compound. The naphthoquinone diazide compound can be selected from, for example, naphthoquinone diazide adducts of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene (e.g., TS533, TS567, TS583, TS593 manufactured by Sampo Chemical Research Institute Co., Ltd.), naphthoquinone diazide adducts of tetrahydroxybenzophenone (e.g., BS550, BS570, BS599 manufactured by Sampo Chemical Research Institute Co., Ltd.), and naphthoquinone diazide adducts of 4-{4-[1,1-bis(4-hydroxyphenyl)ethyl]-α,α-dimethylbenzyl}phenol (e.g., TKF-428, TKF-528 manufactured by Sampo Chemical Research Institute Co., Ltd.).
[0078] The photobase generator is a compound that changes its molecular structure or breaks down its molecules by irradiation with ultraviolet light, visible light, etc., thereby generating one or more basic substances (secondary amines and tertiary amines, etc.). As the photobase generator, it can be an ionic photobase generator or a non-ionic photobase generator. In order to further improve the sensitivity of the photosensitive resin composition, the photobase generator is preferably an ionic photobase generator. As an ionic photobase generator, for example, salts of carboxylic acids and tertiary amines containing aromatic components can be cited, and as its commercial products, WPBG-082, WPBG-167, WPBG-168, WPBG-266 and WPBG-300 of ionic PBG manufactured by Wako Pure Chemical Industries, Ltd. can be cited. As a non-ionic photobase generator, for example, it can be an α-aminoacetophenone compound, an oxime ester compound, a compound having a substituent such as an N-formylated aromatic amino group, an N-acylated aromatic amino group, a nitrobenzyl carbamate group and an alkoxybenzyl carbamate group, etc. As other photobase generators, WPBG-018 (trade name: 9-anthrylmethyl N,N'-diethylcarbamate), WPBG-027 (trade name: (E)-1-[3-(2-hydroxyphenyl)-2-propenoyl]piperidine), WPBG-140 (trade name: 1-(anthraquinon-2-yl)ethyl imidazolecarboxylate) and WPBG-165 manufactured by Wako Pure Chemical Industries, Ltd. can be mentioned.
[0079] In some embodiments, the photosensitive resin composition may further include a crosslinking agent. The addition of the crosslinking agent can further enable the photosensitive resin composition to be fully cured under low temperature curing conditions. In some preferred embodiments, in the photosensitive resin composition, the polybenzoxazole precursor having cyclohexyl side groups is 100 parts by weight, and the crosslinking agent is preferably 0.1 to 30 parts by weight, and more preferably 0.1 to 20 parts by weight.
[0080] The crosslinking agent is preferably a compound that can react with the phenolic hydroxyl group in the polybenzoxazole precursor to form a crosslinked structure, for example, a crosslinking agent having a cyclic ether group such as an epoxy group, a cyclic thioether group such as an episulfide group, a crosslinking agent having an alcoholic hydroxyl group formed by bonding an alkylene group having 1 to 12 carbon atoms such as a hydroxymethyl group to a hydroxyl group, a compound having an ether bond such as an alkoxymethyl group, a crosslinking agent having a triazine ring structure, a urea crosslinking agent, etc. More preferably, the crosslinking agent is at least one of a crosslinking agent having a cyclic ether group, especially an epoxy group, and a crosslinking agent having an alcoholic hydroxyl group, especially a hydroxymethyl group bonded to a hydroxyl group.
[0081] In some preferred embodiments, the crosslinking agent includes a crosslinking agent having an epoxy group, and the crosslinking agent having an epoxy group undergoes a thermal reaction with the hydroxyl group of the polybenzoxazole precursor to form a crosslinked structure. The number of functional groups of the crosslinking agent having an epoxy group is preferably 2 to 4. The photosensitive resin composition can further reduce the curing temperature by including a crosslinking agent having an epoxy group. Among the crosslinking agents having an epoxy group, epoxy compounds having a functional group number of two or more of a naphthalene skeleton are preferred, which can not only obtain an insulating film with better flexibility and chemical corrosion resistance, but also can achieve a low CTE that is in an opposite relationship to flexibility, which can suppress the occurrence of warping and cracking of the insulating film. In addition, from the perspective of flexibility, bisphenol A type epoxy compounds can also be used as crosslinking agents.
[0082] In some preferred embodiments, the cross-linking agent includes a cross-linking agent having a hydroxymethyl group, preferably having 2 or more hydroxymethyl groups.
[0083] In some preferred embodiments, in order to further promote the cyclization reaction of the polybenzoxazole precursor, the photosensitive resin composition may further include a thermal acid generator. In some preferred embodiments, in order to improve photosensitivity, the photosensitive resin composition may further include a sensitizer. In some preferred embodiments, in order to further improve the adhesion to the substrate, the photosensitive resin composition may further include a silane coupling agent and other adhesion agents. In some preferred embodiments, in order to further improve the processing characteristics and various functionalities of the photosensitive resin composition, various organic or inorganic low-molecular or high-molecular compounds may also be added. For example, surfactants, leveling agents, fine particles, etc. may be used. The fine particles include organic fine particles of polystyrene, polytetrafluoroethylene, etc. and inorganic fine particles of silicon dioxide, carbon, layered silicates, etc. In addition, various colorants and fibers may also be mixed in the photosensitive resin composition.
[0084] In some embodiments, the photosensitive resin composition further includes a second solvent. The type of the second solvent is not limited, as long as the components can be dissolved, for example, at least one of N,N'-dimethylformamide, N-methylpyrrolidone, N-ethyl-2-pyrrolidone, N,N'-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, γ-butyrolactone and diethylene glycol monomethyl ether.
[0085] In some embodiments, in the photosensitive resin composition, the polybenzoxazole precursor having a cyclohexyl side group is 100 parts by weight, and the second solvent is 30 parts by weight to 10,000 parts by weight.
[0086] The photosensitive resin composition can be used to prepare photoresist.
[0087] The embodiment of the present application also provides a dry film, which is a resin layer formed by drying the above-mentioned photosensitive resin composition. The thickness is not particularly limited and is determined according to the actual use. For example, it can be set to 0.1μm to 150μm. The coating method is not limited, for example, a spin coater, a rod coater, a blade coater, a curtain coater and a screen printer are used for coating, or a spray coater is used for spray coating or inkjet method. The drying method can be air drying, heat drying using an oven or a hot plate, vacuum drying, etc. In addition, it is preferably dried under conditions that do not cause the closed loop of the polybenzoxazole precursor in the photosensitive resin composition. In some preferred embodiments, natural drying, air drying, or heating drying is performed at 70°C to 140°C and 1 minute to 30 minutes. In order to simplify the operating method, it is preferred to use a hot plate and dry for 1 minute to 20 minutes. In addition, vacuum drying can also be performed and dried at room temperature for 20 minutes to 1 hour.
[0088] The present application also provides a cured film, and a method for preparing the cured film includes:
[0089] S10: exposing and developing the dry film to form a pattern film;
[0090] S20: heating and curing the pattern film.
[0091] In step S10, the wavelength of the light source used for exposure can be the wavelength at which the photoacid generator is activated. Preferably, the light source has a maximum wavelength of 350nm to 450nm. The exposure dose is determined according to the film thickness, etc., and can usually be set to 10mJ / cm 2 ~10000mJ / cm 2 , preferably can be set to 50mJ / cm 2 ~3000mJ / cm 2 The exposure machine used for exposure can be any device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, etc., and irradiates ultraviolet rays in the range of 350nm to 450nm.
[0092] During development, known photoresist development methods can be used, such as rotary spraying, paddle method, immersion method with ultrasonic treatment, etc. The developer can be selected from inorganic bases such as sodium hydroxide, sodium carbonate, sodium silicate, ammonia, or organic amines such as ethylamine, diethylamine, triethylamine, triethanolamine, or aqueous solutions of quaternary ammonium salts such as tetramethylammonium hydroxide and tetrabutylammonium hydroxide. In addition, appropriate amounts of water-soluble organic solvents such as methanol, ethanol, isopropanol, and surfactants can be added to the aqueous solution as needed.
[0093] After the pattern film is formed, the pattern film may be cleaned with a rinse liquid, which is at least one selected from distilled water, methanol, ethanol, isopropanol, and the like.
[0094] In step S20, the polybenzoxazole precursor is subjected to a cyclization reaction by heating to form polybenzoxazole. The heating conditions may be 220° C. to 350° C. for 5 to 120 minutes. A hot plate, an oven, or a temperature-programmable heating oven may be used for heating, preferably under an inert gas such as nitrogen or argon.
[0095] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Unless otherwise specified, the reagents and raw materials used can be purchased through commercial channels. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications.
[0096] Example 1
[0097] Preparation of polybenzoxazole precursor:
[0098] (1) 12.600 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 1.4900 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 103.8900 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0099] (2) pouring 11.0625 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0100] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0101] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0102] Preparation of photosensitive resin composition:
[0103] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0104] Example 2
[0105] Polybenzoxazole precursor preparation:
[0106] (1) 12.600 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 1.4900 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 106.8400 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0107] (2) pouring 11.8000 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0108] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0109] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0110] Preparation of photosensitive resin composition:
[0111] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0112] Example 3
[0113] Polybenzoxazole precursor preparation:
[0114] (1) 12.600 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 1.4900 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 109.7900 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0115] (2) pouring 12.5375 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0116] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0117] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0118] Preparation of photosensitive resin composition:
[0119] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0120] Example 4
[0121] Preparation of polybenzoxazole precursor:
[0122] (1) 11.200 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 2.9800 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 104.2500 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0123] (2) pouring 11.0625 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0124] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0125] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0126] Preparation of photosensitive resin composition:
[0127] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0128] Example 5
[0129] Polybenzoxazole precursor preparation:
[0130] (1) 11.200 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 2.9800 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 107.2000 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0131] (2) pouring 11.8000 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0132] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0133] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0134] Preparation of photosensitive resin composition:
[0135] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0136] Example 6
[0137] Polybenzoxazole precursor preparation:
[0138] (1) 11.200 g of 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone and 2.9800 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 110.1500 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0139] (2) pouring 12.5375 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0140] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0141] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0142] Preparation of photosensitive resin composition:
[0143] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0144] Example 7
[0145] Polybenzoxazole precursor preparation:
[0146] (1) 12.8100 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 4.4700 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 116.6500 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0147] (2) pouring 11.0625 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0148] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0149] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0150] Preparation of photosensitive resin composition:
[0151] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0152] The photosensitive resin composition prepared in Example 7 was coated and baked to form a dry film, and low-temperature cured for 1 hour in an oxygen-free environment at 250°C and an oxygen content of less than 100 ppm to obtain a cured PBO film. The PBO film was tested by Fourier transform infrared spectroscopy (FT-IR): The sample was tested using a Nicolet iS5 Fourier infrared spectrometer from ThermoFisher Technology Co., Ltd., with a test range of 4000 to 500 cm -1 The number of tests was set to 32. During the test, the sample was directly placed on the ATR component to obtain the following Figure 3 The FT-IR graph shown. Figure 3 As shown, 1052cm -1 The stretching vibration peak of the CO bond on the oxazole ring appears at 1539 cm -1 The peak of the amide bond at has disappeared, proving that the PBO membrane has been basically cyclized.
[0153] Example 8
[0154] Preparation of polybenzoxazole precursor:
[0155] (1) 12.8100 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 4.4700 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 119.6000 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0156] (2) pouring 11.8000 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0157] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0158] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0159] Preparation of photosensitive resin composition:
[0160] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0161] Example 9
[0162] Preparation of polybenzoxazole precursor:
[0163] (1) 12.8100 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 4.4700 g of 2,2'-diamino-4,4'-(cyclohexyl-1,1-diyl)diphenol were completely dissolved in 122.5500 g of N,N-dimethylacetamide to obtain a diamine monomer solution;
[0164] (2) pouring 12.5375 g of 4,4'-diacyl chloride diphenyl ether solid into the diamine monomer solution under a nitrogen atmosphere and an ice bath at 5° C., removing the ice bath after pouring, and reacting for 4 hours under a nitrogen atmosphere at 25° C. to obtain a polybenzoxazole precursor solution;
[0165] (3) In a nitrogen atmosphere at 25° C., 0.8200 g of solid nadic anhydride was poured into the polybenzoxazole precursor solution and reacted for 2 hours to perform a capping reaction;
[0166] (4) The blocked product system is evenly dropped into deionized water, filtered and replaced with deionized water, soaked and washed again, filtered, and repeated for multiple times, and dried to obtain a dry polybenzoxazole precursor containing cyclohexyl side groups.
[0167] Preparation of photosensitive resin composition:
[0168] Take 10g of the polybenzoxazole precursor prepared in this example, 2g of TS533 (naphthoquinone diazide adduct of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, Sanbao Chemical), 0.5g of γ-glycidyloxypropyltrimethoxysilane and 18g of N-methylpyrrolidone, stir and mix well to obtain a photosensitive resin composition.
[0169] Weight average molecular weight (Mw) and molecular weight distribution index (PDI) determination
[0170] Gel permeation chromatography (GPC) was used to detect the weight average molecular weight (Mw) and molecular weight distribution index (PDI) of the polybenzoxazole precursor prepared in Examples 1 to 9. The test method is: fill the chromatographic column with DMAc to occupy all the gaps between the carrier particles and the cavities inside the particles, then add the sample solution prepared with the same solvent from the column head, elute with the same solvent, collect the elution at the micro end of the chromatographic column, calculate the volume and concentration of the elution, and the total volume of the elution received is called the elution volume. The elution volume of the solute is related to its molecular weight, and the larger the molecular weight, the smaller its elution volume. If the sample is polydisperse, a series of fractions with molecular weights from large to small can be collected in the order of elution. The test results are shown in Table 1.
[0171] Table 1 Mw and PDI of polybenzoxazole precursors prepared in Examples 1 to 9
[0172] Group M PDI Example 1 10159 1.47 Example 2 13229 1.66 Example 3 16795 1.78 Example 4 10942 1.49 Example 5 14117 1.68 Example 6 18096 1.85 Example 7 11439 1.54 Example 8 14796 1.70 Example 9 19007 1.89
[0173] Lithography performance test
[0174] The photosensitive resin compositions prepared in Example 1 and Example 2 were filtered under pressure to remove insoluble matter, and degassed under vacuum to obtain a photosensitive resin composition solution. The photosensitive resin composition was spin-coated on a silicon wafer and placed on a 120°C hot plate for 180 seconds to volatilize most of the solvent to obtain a dry film. The dry film was exposed using a stepper photolithography machine (SSB320) at an exposure dose of 400 to 1200 mJ / cm 2 , a TMAH (tetramethylammonium hydroxide) aqueous solution with a mass fraction of 2.38% was used for development, the development time was 30s*2 times, and the pattern was observed under a microscope.
[0175] The patterns after exposure and development of the photosensitive resin compositions of Example 1 and Example 2 are respectively as follows: Figure 4 and Figure 5 As shown in the figure, it can be seen that the photosensitive resin composition prepared by using Example 1 and Example 2 can prepare a high-resolution pattern (10μm@10μm, that is, the film thickness is 10μm and the opening is 10μm).
[0176] Example 10
[0177] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at 220° C. and an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0178] Embodiment 11
[0179] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at 250° C. with an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0180] Example 12
[0181] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at 280° C. and an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0182] Embodiment 13
[0183] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at 300° C. and an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0184] Embodiment 14
[0185] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at 320° C. and an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0186] Comparative Example 1
[0187] The photosensitive resin composition prepared in Example 1 was coated, baked, exposed, and developed to form dumbbell-shaped specimens, and low-temperature cured for 1 hour in an oxygen-free environment at a high temperature of 350° C. and an oxygen content of less than 100 ppm to obtain a cured PBO specimen.
[0188] The PBO strips of Examples 10 to 15 and Comparative Example 1 were tested using a Nicolet iS5 Fourier transform infrared spectrometer from ThermoFisher Technology Co., Ltd. in attenuated total reflection mode to verify the degree of cyclization. -1 The cyclization rate of the PBO film was monitored by the signal intensity of the CO bond on the oxazole ring at , and the signal intensity of Comparative Example 1 was taken as 100% to obtain the cyclization rate shown in Table 2. The cyclization rate results show that the cyclization degree of the examples of the present application is close to complete curing.
[0189] Mechanical properties test
[0190] The tensile properties, thermal expansion coefficients and dynamic mechanical properties (DMA) of the PBO splines of Examples 10 to 14 and Comparative Example 1 were tested. The test results are shown in Table 2.
[0191] Tensile performance test: The tensile strength, Young's modulus and elongation at break of the specimen were characterized by using a CMT-1104 universal tensile testing machine from Zhuhai Sansi Taijie Electrical Equipment Co., Ltd. The test was carried out in accordance with the "Standard Test Method for Tensile Properties of Plastics" (ASTM-D638), with a tensile speed of 5 mm / min until the specimen broke. The final data was the average of 5 measurement results.
[0192] TMA test: The coefficient of thermal expansion (CTE) of the specimens was characterized using a Q400 static thermomechanical analyzer from TA Instruments, USA, to determine its dimensional stability within the normal operating temperature range. In the tensile mode, the temperature was raised to 300°C in a nitrogen atmosphere at a heating rate of 30°C / min and stayed for 5 minutes to eliminate the residual thermal potential, then cooled to room temperature at the same rate, and then heated to 390°C for the second time at a heating rate of 5°C / min. The static force was set to 0.05N, and the final CTE value was taken in the 50-150°C range.
[0193] DMA test: The glass transition temperature (Tg) of the sample was characterized by a Q800 dynamic thermal mechanical analyzer from TA Instruments, USA, to determine its upper limit of normal operating temperature. In the dynamic pull-up mode, the temperature was raised to 500°C in a nitrogen atmosphere at a heating rate of 5°C / min, and the test frequency was set to 1Hz.
[0194] Table 2 Mechanical properties test results of Examples 10 to 14 and Comparative Example 1
[0195]
[0196] As shown in 2, the mechanical properties of the polymers in the embodiments of the present application when cured at low temperatures (220°C to 300°C) are similar to those when cured at high temperatures (350°C), indicating that the polymers in the embodiments of the present application can be cured at low temperatures and have excellent mechanical properties. The Tg of the polymers in the embodiments of the present application increases with the increase of the curing temperature, and all exceed 250°C, meeting the use requirements.
[0197] Thermal performance test
[0198] The PBO specimens of Examples 10 to 14 and Comparative Example 1 were subjected to thermogravimetric testing. The specific testing method is as follows:
[0199] The stability of the material was characterized using a Discovery TGA55 thermogravimetric analyzer from TA Instruments, Inc., USA. 10-15 mg of the sample was weighed and carefully placed in an alumina high-temperature crucible. The temperature was raised to 120°C at a heating rate of 20°C / min in a nitrogen atmosphere, maintained for 10 minutes to remove trace moisture contained in the sample, then cooled to room temperature, and then heated again to 800°C at a heating rate of 10°C / min, with a nitrogen pressure of no more than 0.1 MPa. The test results are shown in Table 3.
[0200] Table 3 Thermal performance test results of Examples 10 to 14 and Comparative Example 1
[0201] project Curing temperature Td1%(℃) Td3%(℃) Td5%(℃) Example 10 220℃ 259.44 285.52 341.15 Embodiment 11 250℃ 288.57 324.12 371.12 Example 12 280℃ 311.41 361.78 405.88 Embodiment 13 300℃ 335.58 395.47 429.43 Embodiment 14 320℃ 363.91 414.80 447.73 Comparative Example 1 350℃ 401.07 445.29 476.71
[0202] Table 3 shows the thermal properties test results of the polybenzoxazole precursor containing cyclohexyl side groups prepared in Example 1 at different curing temperatures. When the curing temperature is 220°C to 350°C, the Td of the polybenzoxazole precursor increases with the increase of the curing temperature, and all exceed 250°C. Therefore, the polybenzoxazole precursor prepared in the embodiment of the present application has excellent thermal properties and meets the use requirements.
[0203] Chemical corrosion resistance test
[0204] Embodiment 15
[0205] The photosensitive resin composition of Example 1 was spin-coated on a silicon wafer and placed on a 120°C hot plate for 180 seconds to volatilize most of the solvent to obtain a dry film. The dry film was exposed using a stepper lithography machine (SSB320) with an exposure dose of 400 to 1200 mJ / cm 2 , using a 2.38% mass fraction of TMAH (tetramethylammonium hydroxide) aqueous solution for development, the development time is 30s*2 times, and after rinsing with a rinse solution, an uncured positive resin pattern is obtained. The silicon wafer with the uncured positive resin pattern is placed in a nitrogen-protected blast oven (oxygen concentration below 100ppm) and first cured at 150°C for 30min, then heated to 220°C for 1h to obtain a cured film.
[0206] Example 16
[0207] The silicon wafer with the uncured positive resin pattern of Example 15 was placed in a nitrogen-protected blast oven (oxygen concentration below 100 ppm) and cured at 150° C. for 30 min, then heated to 250° C. for 1 h to obtain a cured film.
[0208] Embodiment 17
[0209] The silicon wafer with the uncured positive resin pattern of Example 15 was placed in a nitrogen-protected blast oven (oxygen concentration below 100 ppm) and cured at 150° C. for 30 min, then heated to 280° C. for 1 h to obtain a cured film.
[0210] Embodiment 18
[0211] The silicon wafer with the uncured positive resin pattern of Example 15 was placed in a nitrogen-protected blast oven (oxygen concentration below 100 ppm) and cured at 150° C. for 30 min, then heated to 300° C. for 1 h to obtain a cured film.
[0212] Embodiment 19
[0213] The silicon wafer with the uncured positive resin pattern of Example 15 was placed in a nitrogen-protected blast oven (oxygen concentration below 100 ppm) and cured at 150° C. for 30 min, then heated to 320° C. for 1 h to obtain a cured film.
[0214] The silicon wafers with cured films obtained in Examples 15 to 19 and the PBO specimens of Comparative Example 1 were immersed in organic reagents such as acetone (25°C, 60s), ammonia water (25°C, 60s), HCl (25°C, 60s), a mixed solution of H2SO4 and H2O2 (25°C, 180s), and N-methylpyrrolidone (25°C, 30min), respectively. Then, they were washed with water and dried by air. The changes in film thickness of the silicon wafers with cured films before and after immersion were measured with a film thickness meter. The patterns were observed under an optical microscope to evaluate their resistance to chemical corrosion.
[0215] The chemical resistance when the film thickness change before and after immersion does not exceed 5% is evaluated as A, the chemical resistance when the film thickness change before and after immersion exceeds 5% is evaluated as B, and the chemical resistance when cracks appear on the film surface, cracks occur at the corners of the pattern, the agent penetrates into the edge of the pattern, or the cured film peels off from the substrate is evaluated as C. The test results can be found in Table 4.
[0216] Table 4 Chemical corrosion resistance test results of Examples 15 to 19 and Comparative Example 1
[0217] project Curing temperature acetone ammonia HCl <![CDATA[H2SO4 / H2O2]]> N-Methylpyrrolidone Embodiment 15 220℃ A A A A A Example 16 250℃ A A A A A Embodiment 17 280℃ A A A A A Embodiment 18 300℃ A A A A A Embodiment 19 320℃ A A A A A Comparative Example 1 350℃ A A A A A
[0218] It can be seen from Table 4 that the polybenzoxazole precursor containing cyclohexyl side groups prepared in the examples of the present application has good chemical corrosion resistance.
[0219] Figure 6 The 3D image of the film surface after the cured film of Example 16 was soaked in N-methylpyrrolidone (25°C, 30 min) is shown. Figure 6 It can be seen that the film surface is flat and has no cracks, which proves that the cured film has excellent chemical resistance.
[0220] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.
Claims
1. A polybenzoxazole precursor, It is characterized in that The structural formula of the polybenzoxazole precursor is shown in formula (I) or formula (II): ; ; In formula (I) and formula (II), X is , Y is or ; n and n1 are 1~100, m and m1 are 0~100.
2. The polybenzoxazole precursor according to claim 1, It is characterized in that The n and n1 are 1-40, and the m and m1 are 15-40.
3. A method for preparing a polybenzoxazole precursor as claimed in claim 1 or 2, It is characterized in that The polybenzoxazole precursor is formed by reacting a diamine monomer and a dicarboxylic acid monomer; wherein the diamine monomer comprises a diamine compound represented by formula (1) and / or formula (2) and a diamine compound represented by formula (4): ; ; ; In the formula (1) and the formula (2), R 1 ~R 5 , R 11 ~R 51 All are hydrogen; In the formula (4), Y is or ; wherein, one of 1* and 2* represents the connection part with the amino group in formula (4), and the other represents the connection part with the hydroxyl group; The dicarboxylic acid monomer has a structure shown in formula (3): ; In formula (3), X is ; Z is selected from a hydroxyl group or a halogen group; The preparation method comprises the following steps: S1: dissolving a diamine monomer in a first solvent to obtain a diamine monomer solution, wherein the molar percentage of the diamine compound represented by formula (1) and / or formula (2) in the diamine monomer is greater than or equal to 10% and less than 100%; S2: adding the dicarboxylic acid monomer represented by formula (3) to the diamine monomer solution to cause a polymerization reaction to obtain a polybenzoxazole precursor solution.
4. The preparation method according to claim 3, It is characterized in that The first solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, tetrahydrofuran, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate; And / or, step S2 satisfies one of the following conditions: 1) adding the dicarboxylic acid monomer represented by formula (3) under ice bath conditions of 0-10°C, and the polymerization reaction temperature is 0-35°C, and the polymerization reaction time is 2 hours to 10 hours; 2) the molar ratio of the diamine monomer to the dicarboxylic acid monomer represented by formula (3) is 1:(0.5-1); And / or, the preparation method further comprises step S3: adding a capping agent to the polybenzoxazole precursor solution to carry out a capping reaction to obtain a capped polybenzoxazole precursor solution, wherein the molar ratio of the capping agent to the diamine monomer is (0.02-0.2):1, the temperature of the capping reaction is 10°C-35°C, and the time is 1 hour-4 hours; the capping agent is selected from at least one of phthalic anhydride, maleic anhydride, succinic anhydride, 2,3-pyrazine dianhydride, tetrafluorophthalic anhydride, 2,3-naphthalene dicarboxylic anhydride, hexahydrophthalic anhydride, nadic anhydride, tetrahydrophthalic anhydride, 4-phenylalkynylphthalic anhydride, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, phenylsuccinic anhydride, and 2,2'-biphenyl dicarboxylic anhydride; And / or, the preparation method further comprises step S4: dropping the polybenzoxazole precursor solution or the blocked polybenzoxazole precursor solution into deionized water, and washing and drying the precipitate to obtain a dry polybenzoxazole precursor.
5. A photosensitive resin composition, It is characterized in that The following components are included by weight: 100 parts of the polybenzoxazole precursor according to claim 1 or 2, 5 to 40 parts of a photosensitizer, and 30 to 10,000 parts of a second solvent.
6. The photosensitive resin composition according to claim 5, It is characterized in that The photosensitizer includes at least one of a photoacid generator, a photobase generator, a crosslinking agent, a thermal acid generator, a sensitizer, a bonding agent, a surfactant, a leveling agent, and fine particles.
7. The photosensitive resin composition according to claim 5, It is characterized in that The second solvent includes at least one of N,N-dimethylformamide, N-methylpyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine and diethylene glycol monomethyl ether.