A method and use for continuous production of quantum dot@organic silicon light diffuser composite microspheres
By coating quantum dots with silicone materials and adopting a continuous preparation method, the agglomeration and incompatibility of quantum dots in LED packaging are solved, the lumen efficiency and stability of LED devices are improved, and high yield and automated control are achieved.
Patent Information
- Application Number
- CN202311626735.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-11-30
AI Technical Summary
Quantum dots have problems such as aggregation, solvent residue and incompatibility in LED packages, resulting in low lumen efficiency of white LED devices, limiting their large-scale applications.
The quantum dots are coated in situ by silicone material to form quantum dots @ silicone light diffuser composite microspheres, and are continuously prepared using turbulent pipeline reactors and laminar tower reactors to achieve uniform dispersion and stability of quantum dots Improved performance and adjust the refractive index to match the LED packaging material.
The preparation process of LED packaging glue is simplified, the luminous efficiency of quantum dot packaging glue and the stability of LED devices are improved, the input and temperature and pH fluctuations of reaction equipment are reduced, and high yield and automated control are achieved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a quantum dot@organic silicon light diffuser composite microsphere and a continuous preparation method thereof, belonging to the technical field of organic silicon composite materials. Technical Background
[0002] As an energy-saving and low-carbon light source, LED lighting can save 80% of lighting energy consumption each year compared to fluorescent and incandescent lighting. It has already occupied a dominant position in the lighting field and is also widely used in LCD backlighting, full-color large-screen displays, traffic lights, and landscape lighting. It is expected that in the next five years, the global LED lighting market will grow from 1,107.8 billion yuan in 2022 to 1,196 billion yuan in 2026. In LED packaging, traditional rare earth fluorescent materials are usually used as down-conversion materials. However, these fluorescent materials have disadvantages such as low fluorescence quantum efficiency and wide fluorescence emission spectrum during application. In contrast, quantum dots (QD) have the advantages of higher fluorescence quantum efficiency, extremely narrow fluorescence spectrum half-width, and high spectral color purity. Using QD to replace traditional fluorescent materials can not only achieve the regulation of emission wavelength in the visible spectrum region that is sensitive to the human eye, but also because of its extremely narrow fluorescence spectrum half-width, it can achieve high color saturation and reduce the loss of additional luminous efficiency caused by infrared light components, which greatly improves the brightness, color rendering index and color gamut of white light LEDs, thereby further promoting the development of LEDs in the direction of high-quality lighting and display.
[0003] QD is a "zero-dimensional" nanomaterial of 2-10nm. In order to avoid serious agglomeration of QD when mixed with LED encapsulation silicone, a solvent-assisted method is usually used to reduce the viscosity of the encapsulation glue / QD system and improve the dispersibility of QD in the silicone encapsulation glue. However, the subsequent solvent removal process is cumbersome and there is also a problem of solvent residue, which affects the stability of LED devices. QD usually contains sulfur, which will cause the failure of the encapsulation silicone catalyst based on silicon hydrogen / double bond addition curing, incomplete curing, etc., resulting in QD incompatibility with the existing white light LED packaging process. At the same time, QD still has problems such as agglomeration and repeated absorption, resulting in low lumen efficiency of white light LED devices. These problems have restricted the large-scale application of QD materials in LEDs to a certain extent.
[0004] In summary, the present invention in situ encapsulates quantum dots through organic silicon materials, and encapsulates the "zero-dimensional" nano QD material in larger organic silicon microspheres, so that the QD is evenly dispersed in the coated microspheres, the stability is improved, and it is compatible with the existing LED packaging process; by adjusting the refractive index of the organic silicon coating material, the organic silicon material in situ coated quantum dot material is matched with the packaging material system, thereby improving the lumen efficiency and water and oxygen stability of the QDLED. Summary of the invention
[0005] In view of the above technical problems, the present invention proposes a continuous preparation method of quantum dot@silicone light diffuser composite microspheres, that is, a turbulent pipeline reactor, a laminar flow tower reactor, and a pump and a flow meter are used to achieve the continuous preparation of quantum dot@silicone light diffuser composite microspheres. By designing and selecting the turbulent pipeline reactor, the laminar flow tower reactor, the pump and the flow meter, and the mixer, the hydrolysis and condensation process parameters are made stable and controllable, thereby achieving uniform and adjustable particle size of the quantum dot@silicone light diffuser composite microspheres, high production stability, and high yield.
[0006] A method for continuously producing quantum dot@organic silicon light diffuser composite microspheres, characterized in that it comprises the following steps:
[0007] (1) Hydrolysis: The organosilicon monomer and the acidic catalyst aqueous solution are mixed in a turbulent flow pipeline reactor, so that the organosilicon monomer fully reacts with water to hydrolyze into silanol, and the reaction obtains an organosilicon hydrolysis product;
[0008] (2) Condensation: The organic silicon hydrolyzate is mixed with a mixed solution containing quantum dots, an alkaline catalyst and a surfactant in a condensation mixer in a turbulent state, so that the organic silicon hydrolyzate, the mixed solution of quantum dots, an alkaline catalyst and a surfactant are evenly mixed in a very short time, and then enters a laminar flow tower reactor to carry out a condensation reaction to obtain a condensation reaction product;
[0009] (3) Ripening: The condensation reaction product is introduced into a heat preservation kettle, stirred and ripened to obtain quantum dot@organic silicon light diffuser composite microspheres.
[0010] The organic silicon monomer includes one or more of perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methylvinyldimethoxysilane and methylvinyldiethoxysilane.
[0011] The acidic catalyst in step (1) is one of hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid, formic acid and strong acid and weak base salts of inorganic acid such as ammonium chloride, calcium chloride, magnesium chloride and aluminum chloride, preferably hydrochloric acid, the pH value of the acidic catalyst aqueous solution is 4-6, and the mass ratio of the organosilicon monomer to water is 1:0.5-10.
[0012] In step (1), the flow rate of the organosilicon monomer is 0.01-10 m³ / h, preferably 0.1-10 m³ / h, preferably 0.1-1 m³ / h; the flow rate of the acidic catalyst aqueous solution is 0.05-50 m³ / h; the reaction temperature is -5-50°C, and the reaction time is 0.1-30 min.
[0013] The alkaline catalyst in step (2) is one of sodium hydroxide, potassium hydroxide, ammonia water, triethylamine and strong base weak acid salt sodium acetate, potassium acetate, preferably ammonia water; the surfactant is sodium dodecyl sulfate, and the quantum dots are one of CdSe / CdS / ZnS, CuInS2 / ZnS or carbon quantum dots; the mass ratio of the organosilicon monomer to the quantum dots is 1:0-10; the amount of the surfactant is 0-10 wt% of the mass of the organosilicon monomer; and the pH value of the solution is adjusted to 7-11 using an alkaline catalyst.
[0014] In step (2), the flow rate of the organosilicon hydrolyzate is 0.01-10 m³ / h, preferably 0.1-1 m³ / h; the flow rate of the mixed solution is 0.2-20 m³ / h; the reaction temperature is -5-50°C, and the reaction time is 0.1-30 min.
[0015] The aging temperature in step (3) is 0-100°C, and the aging time is 0.5-24h.
[0016] The refractive index of the continuously produced quantum dot@organic silicon light diffuser composite microspheres prepared by the method is 1.40-1.65.
[0017] The present invention provides the preparation of quantum dot@organic silicon light diffuser composite microspheres described in the above technical solution and their application in luminescent materials.
[0018] The positive effects of the present invention are:
[0019] (1) The present invention uses a continuous coating process to evenly disperse quantum dots into silicone microspheres, thereby converting quantum dots originally in a solvent-dispersed state into quantum dot@silicone light diffuser composite microspheres in the form of solid powder, greatly simplifying the preparation process of LED encapsulant and improving the luminous efficiency of the quantum dot encapsulant and the stability of the LED device.
[0020] (2) The present invention can realize the continuous synthesis of quantum dot@organic silicon light diffuser composite microspheres through the design of process and equipment, which can reduce the investment in reactor equipment and avoid the problems of unstable microsphere morphology and particle size distribution caused by large fluctuations in temperature, pH and stirring during the production process of intermittent reactors.
[0021] (3) By adjusting the type and combination of the encapsulating monomers, the refractive index of the quantum dots@silicone light diffuser composite microspheres can be adjusted according to the characteristics of the quantum dots to match the refractive index of the LED chip, thereby improving the luminous efficiency of the LED device.
[0022] (4) The continuous quantum dot@organic silicon light diffuser composite microsphere production process and device provided by the present invention can realize the automated control of the production of organosilicon microspheres, reduce the labor intensity and human influence factors, and make the production yield of organosilicon microspheres higher. DETAILED DESCRIPTION
[0023] The present invention is described in detail below in conjunction with the embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. A person skilled in the art may make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention, which still fall within the scope of protection of the present invention.
[0024] Example 1
[0025] Through the combined regulation of continuous hydrolysis process equipment: turbulent pipeline reactor, hydrolyzate storage tank, pump and flowmeter, the parameters of the hydrolysis process section are controlled as follows: the mass ratio of methyltrimethoxysilane to water is 1: 0.5, wherein methyltrimethoxysilane is 100 kg, water is 50 kg, and the pH value of water is adjusted to 4 using hydrochloric acid catalyst; the flow rate of methyltrimethoxysilane is 0.1 m³ / h, and the flow rate of acidic catalyst aqueous solution is 0.05 m³ / h; methyltrimethoxysilane and acidic catalyst aqueous solution are mixed in a turbulent pipeline reactor in a turbulent state, the residence time is 0.1 min, and the temperature control range is -5 ℃. The average molecular weight of the obtained silanol is 820 g / mol, which is a plurality of silanol polymers.
[0026] Through the combined regulation of continuous condensation process equipment: laminar flow tower reactor, condensation mixer, pump and flowmeter, the parameters are controlled as follows: the mass ratio of methyltrimethoxysilane hydrolysis product (corresponding silanol obtained by hydrolysis process of organic silicon monomer) to water is 1:2, of which hydrolyzed silanol is 100kg and water is 200kg, and the pH value of water is adjusted to 7 by ammonia catalyst; the flow rates of methyltrimethoxysilane hydrolysis product and alkaline catalyst aqueous solution are 0.05 m³ / h and 0.1 m³ / h respectively. The methyltrimethoxysilane hydrolysis product and water are first mixed evenly in turbulent state in the condensation mixer, and then enter the laminar flow tower reactor, with a residence time of 30 min and a temperature controlled at -5℃.
[0027] The organic silicon microspheres and water mixture obtained by the laminar flow tower reactor were introduced into a heat preservation kettle with stirring to further mature the organic silicon microspheres. The aging temperature and time were 0 ° C and 24 h, respectively. After the organic silicon microspheres were matured, the samples were tested by centrifugation, filtration, washing, drying and crushing. The organic silicon light diffuser prepared in this way has a particle size range of 10.6-100 microns, does not contain quantum dots, has a wide particle size distribution range, and produces a large number of non-spherical gel particles.
[0028] Example 2
[0029] The continuous hydrolysis process equipment is the same as that in Example 1, and the parameters of the hydrolysis process section are controlled as follows: the mass ratio of methyltrimethoxysilane to water is adjusted to 1:4.5, wherein methyltrimethoxysilane is 100 kg and water is 450 kg, and the pH of the water is adjusted to 5 using hydrochloric acid catalyst; the flow rate of methyltrimethoxysilane is 0.5 m³ / h, and the flow rate of the acidic catalyst aqueous solution is 2.25 m³ / h; the residence time of methyltrimethoxysilane and the acidic catalyst aqueous solution in the turbulent pipeline reactor is 15 min, and the temperature control range is 25 °C. The average molecular weight of the obtained silanol is 115 g / mol, which is a single silanol and a small amount of 2-3 silanol polymers.
[0030] The continuous condensation process equipment is the same as that in Example 1, and the parameters of the condensation process section are controlled as follows: the mass ratio of methyltrimethoxysilane hydrolyzate to water is 1:4.5, wherein the methyltrimethoxysilane hydrolyzate is 100 kg, the water is 450 kg, the water contains 2.5 kg of sodium dodecyl sulfate surfactant, and the pH is adjusted to 8.5 with ammonia water as a mixed solution of water, and the flow rates of methyltrimethoxysilane hydrolyzate and the mixed solution are 0.5 m³ / h and 2.25 m³ / h, respectively. The methyltrimethoxysilane hydrolyzate and the mixed solution are first mixed uniformly in a turbulent state in a condensation mixer, and then enter a laminar flow tower reactor, where the residence time is 15 min and the temperature is controlled at 25°C.
[0031] The mixture of organosilicon microspheres and water obtained by the laminar flow tower reactor was introduced into a heat preservation kettle with stirring to further mature the organosilicon microspheres at a temperature and time of 50 °C and 8 h, respectively. After the organosilicon microspheres were matured, the samples were tested by centrifugation, filtration, washing, drying and crushing.
[0032] The particle size of the organic silicon microspheres prepared in this way is 1.8-2.1 microns, does not contain quantum dots, has a narrow particle size distribution range, is spherical, and has no gel.
[0033] Example 3
[0034] The continuous hydrolysis process equipment is the same as that in Example 1, and the parameters of the hydrolysis process section are controlled as follows: the mass ratio of methyltrimethoxysilane to water is adjusted to 1:10, wherein methyltrimethoxysilane is 100 kg, water is 1000 kg, and the pH of water is adjusted to 6 using hydrochloric acid catalyst; the flow rate of methyltrimethoxysilane is 5 m³ / h, and the flow rate of acidic catalyst aqueous solution is 50 m³ / h; the residence time of methyltrimethoxysilane and acidic catalyst aqueous solution in the turbulent pipeline reactor is 30 min, and the temperature control range is 50 °C. The average molecular weight of the obtained silanol is 95 g / mol, which is mainly single silanol.
[0035] The continuous condensation process equipment is the same as that in Example 1, and the parameters of the condensation process section are controlled as follows: the mass ratio of methyltrimethoxysilane hydrolyzate to water is 1:10, wherein the methyltrimethoxysilane hydrolyzate is 100 kg, the water is 1000 kg, the water contains 10 kg of sodium dodecyl sulfate surfactant, and the pH is adjusted to 10.5 with ammonia water as a mixed solution of water. The flow rates of methyltrimethoxysilane hydrolyzate and the mixed solution are 3 m³ / h and 30 m³ / h, respectively. The methyltrimethoxysilane hydrolyzate and water are first mixed uniformly in a turbulent state in a condensation mixer, and then enter a laminar flow tower reactor, where the residence time is 0.1 min and the temperature is controlled at 50 °C.
[0036] The mixture of organosilicon microspheres and water obtained by the laminar flow tower reactor was introduced into a heat preservation kettle with stirring to further mature the organosilicon microspheres. The aging temperature and time were 100 °C and 0.5 h, respectively. After the aging of the organosilicon microspheres was completed, the obtained samples were tested by centrifugation, filtration, washing, drying and crushing.
[0037] The particle size of the organic silicon microspheres prepared in this way is 0.2-0.9 microns, does not contain quantum dots, has a narrow particle size distribution range, is spherical, and has no gel.
[0038] Example 4
[0039] By comparison, the particle size of the microspheres prepared by the continuous organic silicon microsphere process parameters of Example 2 is 1.8-2.1 microns, and its particle size distribution is narrow. Therefore, this embodiment prepares quantum dot@organic silicon light diffuser composite microspheres containing quantum dots based on the hydrolysis-condensation-ripening process equipment and parameters of Example 2. The parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those of Example 2, wherein the addition ratio of CdSe / CdS / ZnS quantum dots is controlled at 0.5%, that is, in the mixed solution in the condensation process section, according to the ratio of hydrolyzed silanol: quantum dot mass ratio of 1:0.005, 0.5kg of CdSe / CdS / ZnS quantum dots are added to 100kg of hydrolyzed silanol. After the ripening of the quantum dot@organic silicon light diffuser composite microspheres is completed, the obtained sample is tested by centrifugation, filtration, washing, drying and crushing. The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.7-2.0 microns, contain quantum dots, have a narrow particle size distribution range, are spherical, and have no gel.
[0040] Example 5
[0041] The parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those in Example 4, wherein the proportion of CdSe / CdS / ZnS quantum dots added is controlled at 2%, that is, in the mixed solution in the condensation process section, 2 kg of CdSe / CdS / ZnS quantum dots are added to 100 kg of hydrolyzed silanols according to a mass ratio of 1:0.02. After the ripening of the quantum dot@organic silicon light diffuser composite microspheres is completed, the obtained samples are tested by centrifugation, filtration, washing, drying and crushing. The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.55-2.05 microns, contain quantum dots, have a narrow particle size distribution range, are spherical particles, and have no gel.
[0042] Example 6
[0043] The parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those in Example 4, wherein the proportion of CdSe / CdS / ZnS quantum dots added is controlled at 10%, that is, in the mixed solution in the condensation process section, 10 kg of CdSe / CdS / ZnS quantum dots are added to 100 kg of hydrolyzed silanols according to a mass ratio of 1:0.1. After the ripening of the quantum dot@organic silicon light diffuser composite microspheres is completed, the obtained samples are tested by centrifugation, filtration, washing, drying and crushing. The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.3-2.4 microns, contain quantum dots, and have a wide particle size distribution range, but the microsphere particles are still spherical and free of gel.
[0044] Example 7
[0045] The parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those in Example 4, wherein the proportion of CuInS2 / ZnS quantum dots added is controlled at 3.5%, that is, in the mixed solution in the condensation process section, 3.5 kg of CuInS2 / ZnS quantum dots are added to 100 kg of hydrolyzed silanols according to a mass ratio of 1:0.035. After the ripening of the quantum dot@organic silicon light diffuser composite microspheres is completed, the obtained samples are tested by centrifugation, filtration, washing, drying and crushing. The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.6-2.1 microns, contain quantum dots, have a narrow particle size distribution range, and the microsphere particles are spherical and free of gel.
[0046] Example 8
[0047] The parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those in Example 4, wherein the proportion of carbon quantum dots added is controlled at 3.5%, that is, in the mixed solution in the condensation process section, 3.5 kg of carbon quantum dots are added to 100 kg of hydrolyzed silanols according to a mass ratio of 1:0.035 of hydrolyzed silanols: quantum dots. After the ripening of the quantum dot@organic silicon light diffuser composite microspheres is completed, the obtained samples are tested by centrifugation, filtration, washing, drying and crushing. The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.45-1.95 microns, contain quantum dots, have a narrow particle size distribution range, and the microsphere particles are spherical and free of gel.
[0048] Example 9
[0049] In order to compare the effects of different coating monomers (perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane) on the refractive index of organosilicon microspheres, the parameters of the hydrolysis-condensation-ripening process section in this embodiment are similar to those in Example 5, wherein the addition ratio of CdSe / CdS / ZnS quantum dots is controlled at 3%, and the coating monomers are selected to have a low refractive index monomer combination: perfluorooctyltrimethoxysilane (10 wt.%), perfluorooctyltriethoxysilane (10 wt.%), methyltrimethoxysilane (30 wt.%), methyltriethoxysilane (30 wt.%), dimethyldimethoxysilane (10 wt.%), and dimethyldiethoxysilane (10 wt.%).
[0050] The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.10-1.75 microns, contain quantum dots, have a narrow particle size distribution range, are spherical, have no gel, and have a refractive index of 1.40-1.42.
[0051] Example 10
[0052] In order to compare and study the effect of the coating monomer containing phenyl on the refractive index of the microspheres, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methylvinyldimethoxysilane, and methylvinyldiethoxysilane were selected as coating monomers in this embodiment, and the parameters of the hydrolysis-condensation-ripening process section were similar to those in Example 9, wherein the addition ratio of CdSe / CdS / ZnS quantum dots was also controlled at 3%, and the coating monomer combination ratio was: phenyltrimethoxysilane (30 wt.%), phenyltriethoxysilane (30 wt.%), diphenyldimethoxysilane (15 wt.%), diphenyldiethoxysilane (15 wt.%), methylvinyldimethoxysilane (5 wt.%), and methylvinyldiethoxysilane (5 wt.%).
[0053] The quantum dot@organic silicon light diffuser composite microspheres prepared in this way have a particle size of 1.8-2.8 microns, contain quantum dots, have a narrow particle size distribution range, are spherical, have no gel, and have a refractive index of 1.62-1.65.
[0054] In order to compare the application performance of quantum dot@silicone light diffuser composite microspheres prepared in different examples in LED packaging, the composite microspheres were mixed with a two-component silicone encapsulation adhesive with a refractive index of 1.55 in a weight ratio of 1:50, coated on the surface of the blue light LED chip, and its efficiency and yellow light ratio were tested using an integrating sphere.
[0055]
[0056] It can be seen that the quantum dot@silicone light diffuser composite microspheres prepared by CdSe / CdS / ZnS and CuInS2 / ZnS have a higher yellow light conversion efficiency in LED encapsulation glue. When the particle size of the composite microspheres is uniform and the refractive index is similar to that of the encapsulation glue, the luminous efficiency is higher and it is more suitable as a blue light conversion material.
Claims
1. A method for continuously producing quantum dot@organic silicon light diffuser composite microspheres, characterized in that: The steps include: (1) Hydrolysis: The organosilicon monomer and the acidic catalyst aqueous solution are mixed in a turbulent flow in a turbulent pipeline reactor, so that the organosilicon monomer fully reacts with water to hydrolyze into silanol, and the reaction obtains an organosilicon hydrolysis product; wherein the pH range of water is adjusted to 4-6 by using an acidic catalyst; the mass ratio of the organosilicon monomer to water is 1:0.5-10; the flow rate of the organosilicon monomer is 0.01-10 m³ / h, and the flow rate of the acidic catalyst aqueous solution is 0.05-50 m³ / h; the reaction temperature is -5-50°C, and the reaction time is 0.1-30 min; (2) Condensation: The organic silicon hydrolysate is mixed with a mixed solution containing quantum dots, an alkaline catalyst and a surfactant in a condensation mixer in a turbulent state, so that the organic silicon hydrolysate and the mixed solution of quantum dots, an alkaline catalyst and a surfactant are mixed evenly in a very short time, and then enters a laminar flow tower reactor for condensation reaction to obtain a condensation reaction product; the mass ratio of the organic silicon hydrolysate: quantum dots is 1:0-0.035, wherein the amount of quantum dots is not 0; the amount of surfactant is 0-10 wt% of the mass of the organic silicon monomer; the pH value of the solution is adjusted to 7-11 using an alkaline catalyst; the flow rate of the organic silicon hydrolysate is 0.01-10 m³ / h; the flow rate of the mixed solution is 0.2-20 m³ / h; the reaction temperature is -5-50°C, and the reaction time is 0.1-30 min; (3) Ripening: introducing the condensation reaction product into a heat preservation kettle, stirring and aging, and obtaining quantum dot@organic silicon light diffuser composite microspheres; the aging temperature is 0-100° C., and the aging time is 0.5-24 h.
2. The method for continuous production of quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The organic silicon monomer includes one or more of perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methylvinyldimethoxysilane and methylvinyldiethoxysilane.
3. The method for continuous production of quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The acidic catalyst in step (1) is one of hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid, formic acid and strong acid and weak base salts of inorganic acids such as ammonium chloride, calcium chloride, magnesium chloride and aluminum chloride.
4. The method for continuous production of quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The acidic catalyst in step (1) is hydrochloric acid.
5. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The flow rate of the organosilicon monomer in step (1) is 0.1-10 m³ / h.
6. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to claim 5, characterized in that: The flow rate of the organosilicon monomer in step (1) is 0.1-1 m³ / h.
7. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The alkaline catalyst described in step (2) is one of sodium hydroxide, potassium hydroxide, ammonia water, triethylamine and strong base weak acid salt sodium acetate, potassium acetate; the surfactant is sodium dodecyl sulfate, and the quantum dots are one of CdSe / CdS / ZnS, CuInS2 / ZnS or carbon quantum dots.
8. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to claim 7, characterized in that: The alkaline catalyst in step (2) is aqueous ammonia.
9. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to claim 1, characterized in that: The flow rate of the organosilicon hydrolyzate in step (2) is 0.1-1 m³ / h.
10. The method for continuously producing quantum dot@organic silicon light diffuser composite microspheres according to any one of claims 1 to 9, characterized in that: The refractive index of the continuously produced quantum dot@organic silicon light diffuser composite microspheres prepared by the method is 1.40-1.65.
Citation Information
Patent Citations
Method for preparing narrow-size-dispersion ultrafine polyvinyl siloxane crosslinked microspheres
CN106432733A
Preparation method for high-luminescence quantum-dot fluorescent microsphere on basis of affinity assembling
CN109705840A
Perovskite microsphere, mixed-color optical conversion film, and displayer
CN110922961A
Light diffusion particle and preparation method and application thereof
CN113897194A
Preparation method of organic silicon light diffusant microspheres
CN115873253A