A high temperature resistant coil and preparation method thereof
The high-temperature-resistant coil with a pure inorganic insulation layer is formed through thermo-electrochemical oxidation treatment and high-temperature baking, which solves the problems of fragile ceramic insulation materials and aging at high temperatures, and realizes a high-temperature-resistant and widely used inorganic insulation layer.
Patent Information
- Application Number
- CN202311668341.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-07
AI Technical Summary
Existing ceramic insulation materials are fragile and prone to cracking at high temperatures, and the processing technology is complex and costly, which limits the heat resistance and application scope of the windings.
Thermal electrochemical oxidation treatment is used to generate Al2O3 ceramic coated aluminum wires, and the surface is coated with high-temperature resistant insulating paint containing organic and inorganic components. It is cured through high-temperature baking to remove the organic components and form a pure inorganic insulating layer.
A high-temperature resistant coil with simple process, low cost and inorganic insulation layer has been realized, which can withstand up to 400°C. The heat dissipation performance of the inorganic insulation layer is better than that of organic materials, overcoming the high temperature intolerance and radiation defects of organic insulation materials.
Smart Images

Figure CN117877883B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of winding electromagnetic wires, and in particular to a high temperature resistant coil and a preparation method thereof. Background Art
[0002] The heat resistance of the winding is mainly limited by the temperature tolerance of its electromagnetic wire insulation material. The heat resistance level of existing organic insulation electromagnetic wire is generally around 200°C, and organic insulation materials age quickly in high temperature or radiation environments. In order to improve the heat resistance of the winding and overcome the problem of rapid aging and decomposition of organic insulation materials at high temperatures, inorganic insulation materials based on ceramics have been developed at home and abroad, which greatly improve the heat resistance of the winding, see references 1-3. However, the processing technology of such inorganic insulation materials based on ceramics is complex, difficult to make, and expensive, and sometimes difficult to purchase due to non-market factors.
[0003] Another difficulty is that ceramic insulating materials have an insurmountable brittleness. When winding the winding, the ceramic layer on the surface of the electromagnetic wire is easy to crack or fall off, resulting in tiny cracks and pores, which leads to the deterioration of insulation performance. In order to overcome the problem that ceramic insulating materials are relatively fragile and easy to crack and fall off, Chinese invention patent CN115295304A discloses a method for preparing ceramic aluminum wire windings, in which the aluminum wire is first wound into shape and then subjected to thermoelectrochemical oxidation treatment, so that a ceramic insulating film layer is generated on the surface of the aluminum wire in the formed winding. Patent CN115274294A discloses a method for preparing ceramic insulated aluminum windings, in which the aluminum wire is oxidized while being bent. Patent CN116707248A discloses a method for manufacturing prefabricated aluminum coils, which are actually a method of pre-bending and then coating a ceramic insulating film layer to avoid the problem of the fragile ceramic film layer being easy to crack and fall off. However, this method of pre-bending and then coating the ceramic insulating film layer has certain limitations on the stator structure. The stator must be designed with rectangular open teeth for assembly, and the harmonic magnetic field is high, so the application range is limited.
[0004] References:
[0005] [1] Malec D, Roger D, Duchesne S. An electrical machine made within organic rigid coils: a breakthrough toward high temperature motors designed for aeronautics[C]. IEEE Electrical Insulation Conference, San Antonio, USA, 2018.
[0006] [2] Babicz S, Vélu G. Improving insulation quality of ceramic insulated conductors by dip coating with boron oxide[J]. IEEE Transactions on Dielectrics and Electrical Insulation, 2019, 26(01): 51-55.
[0007] [3] Wang Z, Freer R, Fang L, et al. Development of low temperature co-fired ceramic (LTCC) coatings for electrical conductor wires[J]. IEEE Transactions on Dielectrics and Electrical Insulation, 2016, 23(01): 158-164. Summary of the invention
[0008] The object of the present invention is to provide a high temperature resistant coil with simple process, low cost, easy winding and pure inorganic insulation and a preparation method thereof.
[0009] To achieve the above-mentioned purpose, the technical solution of the present invention is as follows:
[0010] A method for preparing a high temperature resistant coil comprises the following steps:
[0011] (1) Immerse the aluminum wire in an electrolyte for thermal electrochemical oxidation treatment to obtain a surface with Al 2 O 3 Ceramic aluminum conductor with ceramic coating;
[0012] (2) coating the surface of the ceramic aluminum conductor with a high temperature resistant insulating coating, and winding the ceramic aluminum conductor into an aluminum coil before the high temperature resistant insulating coating dries;
[0013] (3) Place the aluminum coil in an oven and bake it for 0.5-2 hours. Set the oven temperature at 280℃-400℃ to solidify the high-temperature resistant insulating coating. Take it out to obtain the high-temperature resistant coil.
[0014] Furthermore, the high temperature resistant insulating coating includes organic components and inorganic components. The heat treatment process cures the high temperature resistant insulating coating while removing the organic components in the high temperature resistant insulating coating, leaving only Al on the surface of the aluminum wire. 2 O 3The inorganic components of the ceramic coating and the high temperature resistant insulating coating can obtain a pure inorganic insulating high temperature resistant aluminum coil.
[0015] The present invention also provides a high temperature resistant coil prepared by the method.
[0016] The present invention also provides an electromagnetic pump, comprising a pump core, wherein the coil on the pump core adopts the above-mentioned high temperature resistant coil.
[0017] The present invention also provides a method for preparing the electromagnetic pump, comprising:
[0018] (1) Immersing the aluminum wire in an electrolyte for thermal electrochemical oxidation treatment to obtain a ceramic aluminum wire with a ceramic coating on the surface;
[0019] (2) Coating a high temperature resistant insulating coating on the surface of the ceramic aluminum conductor, and winding the ceramic aluminum conductor on the pump core into an aluminum coil before the high temperature resistant insulating coating dries;
[0020] (3) Place the pump core in an oven and bake it for a period of time to solidify the high-temperature resistant insulating coating. Take out the pump core and assemble it into an electromagnetic pump.
[0021] Compared with the prior art, the beneficial technical effects of the present invention are:
[0022] The preparation method of the high temperature resistant coil of the present invention is simple in process and low in cost. The winding of the high temperature resistant coil is not limited by the stator tooth shape and has a wider application range. The insulation layer of the high temperature resistant coil of the present invention is an inorganic material, which can work in harsh environments such as high temperature and radiation, and can withstand a high temperature of up to 400°C. The heat dissipation performance of the inorganic insulation layer is better than that of the organic insulation material, which overcomes the defects of the organic insulation material that is not resistant to high temperature, radiation, and has difficulty in heat dissipation. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a physical photo of the pump core of the electromagnetic pump made in Example 1 of the present invention.
[0024] Figure 2 This is a physical photo of the electromagnetic pump core produced in Example 1.
[0025] Figure 3 This is a photograph of the burnt-out part of the pump core coil of Comparative Example 1 in the comparative experiment of Example 1.
[0026] Figure 4 This is the comparative analysis result picture in Example 1 (1 mm scale), where: Figure 4 The left is a microscopic photo of the surface of ceramic aluminum flat wire. Figure 4 On the right is a microscopic photograph of the surface film layer of the ceramic aluminum flat wire after being coated with high-temperature resistant insulating coating and cured at high temperature.
[0027] Figure 5This is a comparative analysis result picture in Example 1 (20 μm scale), where: Figure 5 The left is a microscopic photo of the surface of ceramic aluminum flat wire. Figure 5 On the right is a microscopic photograph of the surface film layer of the ceramic aluminum flat wire after being coated with high-temperature resistant insulating coating and cured at high temperature. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.
[0029] Example 1
[0030] A method for manufacturing a high temperature resistant electromagnetic pump core, comprising the steps of:
[0031] (1) Immerse the aluminum flat wire in an electrolyte for micro-arc oxidation / thermal electrochemical oxidation treatment to generate Al 2 O 3 Ceramic coating, ceramic aluminum flat wire, a section is cut off as a sample for analysis;
[0032] (2) Winding the ceramic aluminum flat wire on the axial core of the pump core, coating the surface of the ceramic aluminum flat wire with a high temperature resistant insulating coating (purchased from Beijing Zhisheng Weihua Chemical, model ZS-1091) before winding, and completing the winding before the high temperature resistant insulating coating dries;
[0033] (3) Place the wound pump core in a muffle furnace and bake it for 2 hours at a temperature of 400°C. High-temperature baking solidifies the high-temperature resistant insulating coating in the coil and removes the organic components in the coating.
[0034] After baking, remove the pump core ( Figure 1 ), and then naturally cool to room temperature and can be used for the assembly of electromagnetic pump.
[0035] Comparative Example 1: The pump core is wound according to the method of Example 1, except that the ceramic aluminum flat wire is not coated with high temperature resistant insulating coating ( Figure 2 ).
[0036] The pump cores made in Example 1 and Comparative Example 1 were assembled into electromagnetic pumps for comparative tests. The experimental conditions were to extract aluminum liquid, and the electromagnetic pump was fed with low voltage and high current (30V, 50A) to keep the pump core temperature at 350°C for 2 hours. The experimental results showed that the coil in the pump core of Comparative Example 1 was burned out ( Figure 3 ), the pump core made in Example 1 can work continuously. A section of the coil on the pump core was cut as a sample and compared with the sample obtained in step (1) of Example 1. The analysis results are as follows Figure 4 and 5 As shown. Figure 4 and 5It can be seen that the surface roughness of the ceramic aluminum flat wire is greatly reduced after being coated with high-temperature resistant insulating coating. The surface roughness tester measured that the average surface roughness of the ceramic aluminum flat wire to the aluminum flat wire coated with high-temperature resistant insulating coating dropped from 2.36μm to 0.96μm. After applying the high-temperature resistant insulating coating, the friction force generated when the surface of the aluminum flat wire is rubbed is greatly reduced, enhancing its anti-friction and wear performance. In addition, before the high-temperature resistant insulating coating is cured at high temperature, the organic components in it have excellent flexibility. When it is covered on the surface of the ceramic aluminum flat wire, it can be filled into the pores of the ceramic layer under capillary action, fully absorbing the energy generated by the stress deformation of the ceramic aluminum flat wire during winding, so that the stress on the ceramic layer of the ceramic aluminum flat wire is greatly reduced, avoiding the cracking and falling off of the ceramic layer of the ceramic aluminum flat wire when it is directly subjected to stress deformation.
[0037] Comparative Example 2: The pump core was wound according to the method of Example 1. The bare aluminum flat wire was directly wound without thermoelectrochemical / micro-arc oxidation treatment. The high temperature resistant insulating coating was applied before winding. However, the coating needed to be repeated 7-8 times to make the high temperature resistant insulating coating evenly hung on the surface of the bare aluminum flat wire. In the high temperature curing stage of step (3), after the pump core was taken out and cooled, it was found that the inorganic insulating layer on the surface of the aluminum flat wire fell off over a large area.
[0038] The possible reason for this situation is that the ceramic coating on the surface of the aluminum flat wire treated by micro-arc oxidation / thermal electrochemical oxidation is a loose, porous and rough structure, which has a grinding and roughening effect, making it easier for the high-temperature resistant insulating coating to hang on the surface of the aluminum flat wire. At the same time, the ceramic coating on the surface of the aluminum flat wire treated by micro-arc oxidation / thermal electrochemical oxidation is in situ generated on the surface of the aluminum substrate, and has a better bonding degree with the aluminum substrate and is not easy to fall off. The ceramic coating acts as a transition layer to make the high-temperature resistant insulating coating solidified on the surface of the ceramic coating firmly adhere to the surface of the aluminum flat wire. Example 2
[0039] The pump core was wound according to the method of Example 1, except that the high temperature resistant insulating coating was replaced with another one (Guangzhou Yina New Materials, model GN-203AW), the baking temperature was set to 280°C, and the baking time was 30 minutes.
Claims
1. A method for preparing a high temperature resistant coil, characterized in that: Includes steps: (1) Immersing the aluminum wire in an electrolyte for thermal electrochemical oxidation treatment to obtain a ceramic aluminum wire with a ceramic coating on the surface; (2) coating a high temperature resistant insulating coating on the surface of the ceramic aluminum conductor, and winding the ceramic aluminum conductor into an aluminum coil before the high temperature resistant insulating coating dries; the high temperature resistant insulating coating includes an organic component and an inorganic component; (3) The aluminum coil is heat-treated for a period of time to solidify the high-temperature resistant insulating coating and remove organic components in the high-temperature resistant insulating coating, and the high-temperature resistant coil is obtained after it is taken out.
2. The method according to claim 1, characterized in that The heat treatment method is to place the product in an oven for baking, the heat treatment temperature is 280° C.-400° C., and the heat treatment time is 0.5-2 hours.
3. A high temperature resistant coil prepared by the method according to claim 1 or 2.
4. An electromagnetic pump, comprising a pump core, the pump core having a coil, characterized in that: The coil is the high temperature resistant coil described in claim 3.
5. The method for preparing the electromagnetic pump according to claim 4, characterized in that: include: (1) Immersing the aluminum wire in an electrolyte for thermal electrochemical oxidation treatment to obtain a ceramic aluminum wire with a ceramic coating on the surface; (2) Coating a high temperature resistant insulating coating on the surface of the ceramic aluminum conductor, and winding the ceramic aluminum conductor on the pump core into an aluminum coil before the high temperature resistant insulating coating dries; (3) Place the pump core in an oven and bake it for a period of time to solidify the high-temperature resistant insulating coating. Take out the pump core and assemble it into an electromagnetic pump.