A method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation step by step
Through the electrochemical oxidation method, a mixed solution of electrolyte, thiosulfate and alkali is used for electrochemical leaching, which solves the problem of simultaneous leaching of Au and Ag, achieves efficient extraction and separation of precious metals, simplifies the process, and reduces environmental pollution. contamination risk.
Patent Information
- Application Number
- CN202410050623.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-12
AI Technical Summary
In the existing hydrometallurgical process, the simultaneous leaching of Au and Ag leads to the formation of alloys. The back-end separation and purification process is complex and inefficient, and the strong acid leaching agent used poses environmental pollution risks.
The electrochemical oxidation method is used to perform electrochemical leaching using a mixed solution composed of salt electrolyte, thiosulfate and alkali that does not contain thiosulfate. Silver and gold are extracted through primary and secondary electrochemical leaching respectively, using voltage and time control to achieve selective step-by-step leaching.
It achieves efficient green selective extraction of precious metals Au and Ag, simplifies the separation and purification process, improves efficiency, avoids environmental pollution, and promotes the efficient use of precious metal resources.
Smart Images

Figure CN117887977B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation in steps. Background Art
[0002] Electronic waste is a typical representative of "urban mineral" resources. It is rich in precious metals such as gold, silver, and platinum, and its grade can reach dozens or even hundreds of times that of natural minerals, with significant resource advantages. For example, the gold and silver grades in waste circuit boards (PCBs) are about 120 and 320g / t, respectively, which are more than 60 times higher than those in natural ores. Against the backdrop of the increasing scarcity of natural precious metal mineral resources in China, strengthening the extraction and utilization of precious metals in domestic "urban mineral" resources is of great significance to the high-quality development of my country's economy and science and technology.
[0003] At present, the extraction of precious metals from electronic waste is divided into two methods: pyrometallurgy and hydrometallurgy. Compared with pyrometallurgy, hydrometallurgy is more environmentally friendly. It usually uses aqua regia, cyanide, thiourea and halide as leaching agents to leach precious metals from electronic waste, and then enriches the precious metal ions in the leachate by solvent extraction or adsorption, and finally reduces and recovers the precious metal ions by replacement or electrodeposition. Due to the poor selectivity of commonly used leaching agents, Au and Ag in electronic waste are leached simultaneously, resulting in the formation of gold-silver alloys in the product. The alloy also needs to be wet-leached again using NaClO3, Na2SO3, HNO3 and other agents, and the separation of Au and Ag can be achieved through zinc powder and iron powder replacement, resulting in a complex process flow for the separation and purification of Au and Ag at the back end, low separation efficiency, and the strong acid leaching agent used has an environmental pollution risk.
[0004] Therefore, in order to avoid the simultaneous leaching of gold and silver and simplify the separation and purification process of Au and Ag, it is urgent to develop a technology for the selective step-by-step leaching of Au and Ag in electronic waste. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for selectively leaching Au and Ag from electronic waste in steps by electrochemical oxidation, so as to solve the problem that in the traditional hydrometallurgical process, Au and Ag are simultaneously leached to form an alloy, the back-end Au and Ag separation and purification process is complicated and the separation efficiency is low.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation in steps, comprising the following steps:
[0008] S1: A mixed solution consisting of an electrolyte, thiosulfate and alkali solution is used as an electrolyte, wherein the electrolyte is a salt that does not contain thiosulfate; the electrolyte and the electronic waste are placed in an electrolytic cell, and an electrode system provided in the electrolytic cell is used for electrochemical leaching, and a silver leaching solution and slag are obtained after solid-liquid separation;
[0009] S2: Add electrolyte to the electrolytic cell, perform secondary electrochemical leaching on the slag, and obtain gold leaching solution and waste slag after solid-liquid separation.
[0010] S3: Recovering silver and gold from the silver leaching solution and the gold leaching solution respectively.
[0011] Preferably, the voltage of one electrochemical leaching is 0.1-0.5V, and the electrolysis time is 10-60min.
[0012] Preferably, the voltage of one electrochemical leaching is 0.3 V and the electrolysis time is 30 min.
[0013] Preferably, the voltage of the secondary electrochemical leaching is 0.6-3V, and the electrolysis time is 4-24h.
[0014] Preferably, the concentration of thiosulfate in the electrolyte is 0.05-0.5M, the concentration of the electrolyte is 0.1-0.5M, and the concentration of the alkali solution is 0.1-2.5M.
[0015] Preferably, the pH of the electrolyte is 8-10.
[0016] Preferably, the thiosulfate is one or more of sodium thiosulfate, ammonium thiosulfate, and potassium thiosulfate; and the alkali solution is one or more of ammonia water, sodium hydroxide, and potassium hydroxide.
[0017] Preferably, the electrolyte is one or two of chloride, sulfate and carbonate.
[0018] Preferably, the cathode of the electrolysis system is a titanium plate, a stainless steel plate or a copper plate, and the anode is one of platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, a graphite electrode and graphite felt.
[0019] Preferably, a cation exchange membrane is provided in the electrolytic cell, and the cation exchange membrane divides the electrolytic cell into a cathode chamber and an anode chamber.
[0020] The beneficial effects of the present invention are:
[0021] 1. The present invention can realize the efficient green selective extraction of precious metals Au and Ag, and realize 100% leaching of Ag in waste circuit boards within 30 minutes under low voltage. After solid-liquid separation, the slag is subjected to secondary leaching by changing the voltage. The Au in the slag can be leached 100% within 24 hours, and the selectivity is far superior to the traditional copper ammonia technology;
[0022] 2. The present invention helps to recover and extract high-purity precious metals, avoids the problem of gold and silver separation and purification at the back end, simplifies the precious metal extraction process, improves efficiency, and promotes the green and efficient utilization of precious metal resources in electronic waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of a method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation in steps according to the present invention;
[0024] Figure 2 Example 1 S2O3 2- -KCl-NH3 system leaching effect diagram of Ag and Au in PCBs;
[0025] Figure 3 Comparative Example 1S2O3 2- -Cu 2+ -NH3 system leaching effect diagram of Ag and Au in PCBs;
[0026] Figure 4 Example 2S2O3 2- -KCl-NH3 system leaching effect diagram of Ag and Au in PCBs;
[0027] Figure 5 Example 3S2O3 2- -KCl-NH3 system selectively leaching Ag and Au from PCBs in steps;
[0028] Figure 6 Example 4S2O3 2- -KCl-NH3 system selectively leaching Ag and Au from PCBs in steps;
[0029] Figure 7 Example 5S2O3 2- -KCl-NH3 system selectively leaching Ag and Au from PCBs in steps;
[0030] Figure 8 Example 6S2O3 2- -KCl-NH3 system selectively leaching Ag and Au from PCBs in steps. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The essence of precious metal leaching is an oxidation reaction, that is, precious metals such as Au and Ag lose electrons and are oxidized into ions and enter the solution. In systems such as cyanide and thiosulfate, the redox potential of Au and Ag is close to E θ (Au(CN)2 - / Au)=-0.6eV,E θ (Ag(CN)2 - / Ag)=-0.31eV; E θ (Au(S2O3)2 3- / Au)=0.153eV,E θ (Ag(S2O3))2 - / Ag)=-0.269eV, which results in the leaching rates of gold and silver being close, and the two cannot achieve selective step-by-step leaching.
[0033] The present invention proposes a method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation step by step, that is, based on the thiosulfate electrochemical system, electrochemical anodic oxidation is used to replace the traditional copper ammonium ion catalysis to selectively leach Au and Ag from electronic waste. In this method, the anodic oxidation potential can be precisely controlled by changing the external voltage. When the anodic oxidation potential is adjusted to E θ (Au(S2O3)2 3- / Au) and E θ (Ag(S2O3)2 3- / Ag), the Ag in the electronic waste is rapidly oxidized and leached, while Au cannot be leached; after the Ag is completely leached, solid-liquid separation is performed, and then the electronic waste material is added to the new leaching solution, and the anodic oxidation potential is adjusted to E θ (Au(S2O3)2 3- / Au) or more, so that Au in the material is oxidized and leached, and finally the selective step-by-step leaching of Au and Ag in electronic waste is achieved.
[0034] Specifically, the electrochemical oxidation selective step-by-step leaching method of Au and Ag in electronic waste provided by the present invention is as follows: Figure 1 As shown, the following steps are included:
[0035] S1: A mixed solution consisting of electrolyte, thiosulfate and alkali solution is used as the electrolyte; the concentration of thiosulfate in the electrolyte is 0.05-0.5M, the concentration of electrolyte is 0.1-0.5M, the concentration of alkali solution is 0.1-2.5M, and the initial pH is adjusted to 8-10 with NaOH. Among them, thiosulfate is used as a leaching agent, and its type is not limited, and it can be one or more of sodium thiosulfate, ammonium thiosulfate, and potassium thiosulfate; the alkali solution can be one or more of ammonia water, sodium hydroxide, and potassium hydroxide; the electrolyte is a salt that does not contain thiosulfate, for example, it can be chloride, sulfate or carbonate.
[0036] S2: placing the electrolyte and the electronic waste in an electrolytic cell, performing a first electrolysis operation using an electrode system disposed in the electrolytic cell, and obtaining a silver leaching solution and slag after solid-liquid separation; the voltage of the first electrolysis operation is 0.1-0.5V, preferably 0.3V; and the electrolysis time is 10-60min, preferably 30min.
[0037] S3: Add electrolyte to the electrolytic cell, perform a second electrolysis operation on the slag, and obtain gold leaching solution and waste slag after solid-liquid separation. The voltage of the second electrolysis operation is 0.6-3V, and the electrolysis time is 4-24h.
[0038] S4: Recovering silver and gold from the silver leaching solution and the gold leaching solution respectively.
[0039] The types of cathode materials and anode materials of the electrolysis system of the present invention are not limited. For example, the cathode can be a metal with good conductivity such as a titanium plate, a stainless steel plate or a copper plate, and the anode can be a material with strong conductivity such as platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, graphite electrode and graphite felt. Preferably, a cation exchange membrane is also provided in the electrolytic cell, and the cation exchange membrane divides the electrolytic cell into a cathode chamber and an anode chamber to prevent the noble metal complex anions generated in the anode chamber from reaching the cathode.
[0040] The present invention is described in detail below with reference to specific embodiments.
[0041] Example 1
[0042] The electrolyte composition is 0.15M S2O3 2- , 0.25M KCl, 0.4M NH3, adjust pH 0=10 with NaOH to obtain S2O3 2- -KCl-NH3 system reaction electrolyte.
[0043] A cation exchange membrane is set in a rectangular assembled electrolytic cell, and the electrolytic cell is divided into a cathode chamber and an anode chamber. The prepared electrolyte is poured into the electrolytic cell and the liquid levels of the cation and anode chambers are leveled. Pretreated electronic waste PCBs (200-600 mesh) are added to the anode chamber, and an anode graphite felt (GF) is fixed in the anode chamber. The cathode is a titanium plate of the same size fixed in the cathode chamber. Then a DC power supply is connected, and the voltage is adjusted to 0.3V to react, and the rotation speed is adjusted to 800rpm. Samples are taken at different times, and the concentrations of Au and Ag are determined by atomic absorption spectroscopy. The effect of electrochemical oxidation leaching to extract precious metals in electronic waste is evaluated by the concentrations of Au and Ag. The results are as follows: Figure 1 As shown, it can be seen that the Ag leaching rate of the system is 100% at 30 min, the Au leaching rate is 10.5%, and the Au leaching rate is 58% at 24 h, indicating that the selective step-by-step leaching of Au and Ag can be achieved by controlling the voltage and reaction time.
[0044] Comparative Example 1
[0045] The electrolyte composition is 0.15M S2O3 2- , 0.25M KCl, 1.5mM Cu 2+ , 0.4M NH3, adjust pH to 0 = 10 with NaOH to obtain S2O3 2- Cu 2+ -NH3 system reaction electrolyte.
[0046] A cation exchange membrane was set in a rectangular assembled electrolytic cell, and the electrolytic cell was divided into a cathode chamber and an anode chamber. The prepared electrolyte was poured into the electrolytic cell and the liquid levels of the cation and anode chambers were leveled. Pretreated electronic waste PCBs (200-600 mesh) were added to the anode chamber, and the reaction was carried out without electricity, and the rotation speed was adjusted to 800rpm. Samples were taken at different times, and the Au and Ag concentrations were determined by atomic absorption spectroscopy. The effect of traditional copper ammonia system ion catalytic leaching to extract precious metals from electronic waste was evaluated by Au and Ag concentrations. The results are shown in Figure 2. Figure 2 As shown, it can be seen that the Ag leaching rate of this system is 47% and the Au leaching rate is 38.5% at 30 min, and the selective step-by-step leaching of gold and silver cannot be achieved.
[0047] Example 2
[0048] The electrolyte composition is 0.15M S2O3 2- , 0.25M KCl, 0.4M NH3, adjust pH 0=10 with NaOH to obtain S2O3 2- -KCl-NH3 system reaction electrolyte.
[0049] A cation exchange membrane is set in a rectangular assembled electrolytic cell, and the electrolytic cell is divided into a cathode chamber and an anode chamber. The prepared electrolyte is poured into the electrolytic cell and the liquid levels of the cation and anode chambers are made level. Pretreated electronic waste PCBs (200-600 mesh) are added to the anode chamber, and an anode graphite felt (GF) is fixed in the anode chamber. The cathode is a titanium plate of the same size fixed in the cathode chamber. Then a DC power supply is connected, and the voltage is adjusted to 0.6V to react, and the speed is adjusted to 800rpm. Samples are taken at different times, and the concentrations of Au and Ag are determined by atomic absorption spectroscopy. The effect of electrochemical oxidation leaching to extract precious metals in electronic waste is evaluated by the concentrations of Au and Ag. The results are as follows: Figure 3 As shown, it can be seen that the Ag leaching rate of the system is 100% at 30 min, the Au leaching rate is 30.4%, and the Au leaching rate is 58% at 24 h, indicating that the selective step-by-step leaching of Au and Ag can be achieved by controlling the voltage and reaction time.
[0050] Example 3
[0051] The electrolyte composition is 0.15M S2O3 2- , 0.25M KCl, 0.4M NH3, adjust pH 0=10 with NaOH to obtain S2O3 2- -KCl-NH3 system reaction electrolyte.
[0052] A cation exchange membrane is set in a rectangular assembled electrolytic cell, and the electrolytic cell is divided into a cathode chamber and an anode chamber. The prepared electrolyte is poured into the electrolytic cell and the liquid levels of the cation and positive chambers are leveled. Pretreated electronic waste PCBs (200-600 mesh) are added to the anode chamber, and the anode graphite felt (GF) is fixed in the anode chamber. The cathode is a titanium plate of the same size fixed in the cathode chamber. Then, a DC power supply is connected, the voltage is adjusted to 0.3V for a primary leaching, and the rotation speed is adjusted to 800rpm. After the reaction for 30 minutes, the power supply is stopped, and the mixture in the anode chamber is separated from the solid and liquid to obtain a silver leachate. Then, the leaching electrolyte is added to the anode chamber, the voltage is adjusted to 0.6V, and the slag after silver extraction is leached for a second time. The reaction time is 24 hours, and the gold leachate and waste slag are obtained after solid-liquid separation. The concentrations of Ag and Au in the silver leachate and the gold leachate were determined by atomic absorption spectrometry, respectively, and the results are as follows: Figure 4 As shown, it can be seen that after the first leaching, the Ag leaching rate is 100%, and the Au leaching rate is 10.5%; after the second leaching, there is no Ag leaching when stirring, and the Au leaching rate is 100%.
[0053] Example 4
[0054] The method of electrochemical oxidation selective step-by-step leaching of Au and Ag in electronic waste in this embodiment is basically the same as that in Example 3, except that the voltage of one leaching is 0.1 V. After solid-liquid separation, the Ag concentration in the silver leaching solution is measured, and the result is as follows: Figure 5 As shown, it can be seen that the Ag leaching rate is 96.8%.
[0055] Example 5
[0056] The method of electrochemical oxidation selective step-by-step leaching of Au and Ag in electronic waste in this embodiment is basically the same as that in Example 3, except that the voltage of one leaching is 0.5 V. After solid-liquid separation, the Ag concentration in the silver leachate is measured, and the result is as follows: Figure 6 As shown, it can be seen that the Ag leaching rate is 100%.
[0057] Example 6
[0058] The method of electrochemical oxidation selective stepwise leaching of Au and Ag from electronic waste in this embodiment is basically the same as that in Example 3, except that the voltage of the secondary leaching is 1.2 V. After solid-liquid separation, the Au concentration in the gold leaching solution is measured, and the results are as follows: Figure 7 As shown, it can be seen that the Au leaching rate is 100%.
[0059] In summary, the present invention uses S2O3 2- -KCl-NH3 system is used as the reaction electrolyte. By controlling the voltage of the first leaching to 0.1-0.5V, 100% of the Ag in the waste circuit board can be leached out within 30 minutes, realizing the selective leaching of Ag; by controlling the voltage to 0.6-3V for the secondary leaching of slag, 100% of Au can be leached out within 24 hours. This method has the advantages of selectivity, high efficiency, no pollution, low cost, high purity of precious metal extraction, etc., and promotes the green and efficient utilization of precious metal resources in electronic waste.
[0060] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0061] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation step by step. It is characterized in that The steps include: S1: A mixed solution consisting of an electrolyte, thiosulfate and alkali solution is used as an electrolyte, wherein the electrolyte is a salt that does not contain thiosulfate; the electrolyte and electronic waste are placed in an electrolytic cell, and an electrode system provided in the electrolytic cell is used for electrochemical leaching, and a silver leaching solution and slag are obtained after solid-liquid separation; the voltage of the electrochemical leaching is 0.1-0.5V, and the electrolysis time is 10-60min; the pH of the electrolyte is 8-10; S2: adding electrolyte to the electrolytic cell, performing secondary electrochemical leaching on the slag, and obtaining gold leaching solution and waste slag after solid-liquid separation; S3: Recovering silver and gold from the silver leaching solution and the gold leaching solution respectively.
2. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The voltage of the electrochemical leaching is 0.3V, and the electrolysis time is 30min.
3. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The voltage of the secondary electrochemical leaching is 0.6-3V, and the electrolysis time is 4-24h.
4. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The concentration of thiosulfate in the electrolyte is 0.05-0.5 M, the concentration of the electrolyte is 0.1-0.5 M, and the concentration of the alkali solution is 0.1-2.5 M.
5. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The thiosulfate is one or more of sodium thiosulfate, ammonium thiosulfate, and potassium thiosulfate; the alkali solution is one or more of ammonia water, sodium hydroxide, and potassium hydroxide.
6. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The electrolyte is one or two of chloride, sulfate and carbonate.
7. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that The cathode of the electrode system is a titanium plate, a stainless steel plate or a copper plate, and the anode is one of platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, graphite electrode and graphite felt.
8. The method for selectively leaching Au and Ag from electronic waste by electrochemical oxidation according to claim 1, It is characterized in that A cation exchange membrane is arranged in the electrolytic cell, and the cation exchange membrane divides the electrolytic cell into a cathode chamber and an anode chamber.
Citation Information
Patent Citations
Method for efficiently decomposing and leaching gold of noble metal in waste circuit board
CN108203762A
Valuable metal recovery process for oxidizing and leaching copper anode slime based on Fenton reagent
CN116479253A
Process for extraction of noble metal from anode mud by method of controlling potential
CN85106670A
Leaching process
CN86106986A