A non-metallic element double-coordinated doped carbon-based material and its preparation method and application
By using carbon-based materials doped with double coordination of non-metallic elements in the anode materials of potassium ion batteries, and using bismuth sources and organic ligands to generate honeycomb carbon rods with an O-Bi-N coordination structure, the problem of potassium ion battery materials has been solved. It solves the problems of volume change and structural collapse during the electrochemical process, achieves efficient potassium ion transport and cycle stability, and simplifies the preparation process.
Patent Information
- Application Number
- CN202410288463.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing anode materials for potassium ion batteries have problems with volume changes and structural collapse during the electrochemical process. The preparation process is complex and the performance is poor, resulting in low reserves and slow kinetics.
Carbon-based materials doped with double coordination of non-metallic elements are used to generate rod-shaped Bi-MOF in a hydrothermal reaction between bismuth source and organic ligands, and then undergo pyrolysis and coordination reduction with nitrogen-containing reducing agents to form O-Bi -N coordination structure honeycomb carbon rod material, mixed with conductive materials and binders for the preparation of negative electrodes for potassium ion batteries.
The rate and cycle stability of potassium ion batteries are improved, the preparation process is simplified, the material structure is stable, the potassium ion transport channel is wide, the buffer space is large, and the electrochemical performance is enhanced.
Smart Images

Figure CN117894983B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of potassium ion batteries, and in particular relates to a carbon-based material doped with a non-metallic element in a dual coordination manner, and a preparation method and application thereof. Background Art
[0002] As the capacity of new energy equipment continues to increase, the demand for electrochemical energy storage equipment is also increasing. At present, lithium-ion batteries are widely used in various industrial products. However, problems such as low lithium-ion battery reserves and uneven lithium distribution restrict the development of lithium-ion batteries. Therefore, it is particularly necessary to develop low-cost electrochemical energy storage devices. Potassium-ion batteries, which are more abundant in resources, have attracted much attention in the research of large-scale energy storage technology in recent years.
[0003] At present, researchers have developed a series of negative electrode materials, such as selenium, sulfide, titanium-based compounds, and metal materials. However, these materials are often accompanied by significant volume changes and structural collapse during the electrochemical process. In contrast, carbon-based materials (graphite carbon, hard carbon, etc.) have the advantages of safety, economy, and high efficiency, and have become a hot topic of research. In addition, potassium ions have been proven to be effectively embedded in graphite to form KC8 compounds, with a potassium storage capacity of 279 mA h g -1 However, unmodified carbon materials still have problems such as low capacity, slow kinetics, and large volume expansion. In order to solve these problems, doping carbon materials with other atoms to coordinate and replace carbon atoms and optimizing the structure of carbon materials are effective strategies to obtain better electrochemical performance.
[0004] In the prior art, there are strategies for partial atom doping and structural optimization. For example, by mixing a nitrogen-containing mixture with graphite, after heat treatment, mixing it with a coating agent, and heat treating the obtained mixture again, the nitrogen-doped carbon-coated graphite composite material is obtained. However, the nitrogen doping and carbon coating processes of this preparation method are carried out separately, the carbon doping process has a low level of modification of the carbon layer on the surface of the graphite, and the preparation process is complicated. For another example, by subjecting a mixed solution including a carbon source, a nitrogen source, a template agent and graphite to a hydrothermal reaction and carbonization, a nitrogen-doped carbon-coated graphite negative electrode material can be obtained. However, although the preparation method is optimized, the graphite finally prepared has a high disorder, and its structural treatment inside the carbon is poor.
[0005] Therefore, how to provide a potassium ion carbon-based negative electrode material that is simple to prepare and has excellent performance is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0006] In order to solve the above technical problems, the present invention proposes a carbon-based material doped with a non-metallic element in a double coordination manner and a preparation method and application thereof.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A carbon-based material doped with a non-metallic element in a double coordination manner, wherein the carbon-based material is a honeycomb carbon rod material doped with nitrogen and oxygen double coordinated bismuth metal single atoms.
[0009] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner comprises the following steps:
[0010] The bismuth source and the organic ligand are dispersed in an organic solvent and subjected to a hydrothermal reaction to obtain a precursor, and then the precursor is subjected to a carbon reduction coordination treatment with a nitrogen-containing reducing agent to obtain the non-metallic element doped carbon-based material.
[0011] Preferably, the mass ratio of the bismuth source to the organic ligand is 1:(1-10).
[0012] Beneficial effects: During the product preparation process, under the action of high temperature and high pressure, the bismuth source and the organic ligand are coordinated in the organic solvent. Each Bi (III) cation is coordinated with nine O atoms, eight of which come from the organic ligand group and the ninth comes from the terminal water molecule, generating rod-shaped Bi-MOFs in the organic solvent.
[0013] Preferably, the bismuth source includes one of bismuth nitrate pentahydrate, bismuth trichloride, bismuth citrate, bismuth nitrite, bismuth hypophosphite, sodium bismuth carbonate or bismuth subcarbonate;
[0014] The organic ligand is one of pyridine dicarboxylic acid, heterocyclic dicarboxylic acid, trimesic acid, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, biphenyltricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene or 1,3,6,8-tetrakis(p-benzoic acid)pyrene;
[0015] The organic solvent is one or two of methanol, ethanol, N,N-dimethylformamide (DMF), acetone or ethylene glycol.
[0016] Preferably, the temperature of the hydrothermal reaction is 100-180° C. and the time is 1-24 h.
[0017] Preferably, the mass ratio of the precursor to the nitrogen-containing reducing agent is 1:(1-20);
[0018] The nitrogen-containing reducing agent is dicyandiamide.
[0019] Preferably, the reduction coordination reaction specifically comprises the following steps:
[0020] The precursor and the nitrogen-containing reducing agent are placed in two quartz boats respectively, and the temperature is raised to 900-1100° C. at a rate of 2-20° C. / min in an inert atmosphere and kept at this temperature for 1-24 hours.
[0021] Beneficial effects: The present invention simultaneously performs the pyrolysis and coordination reduction reactions of Bi MOF in an inert atmosphere. Some small molecules and adsorbed water of the rod-shaped Bi MOF are first deactivated and vaporized during the pyrolysis process in an inert atmosphere. The structure of Bi MOF collapses with increasing temperature, Bi is reduced to Bi nanoparticles, and the organic ligands are converted into carbonaceous materials. At the same time, as the temperature further increases, the Bi nanoparticles also begin to vaporize, coordinate with the vaporized nitrogen and oxygen in the nitrogen-containing reducing agent, and finally form carbon rods with an O-Bi-N coordination structure. In addition, due to the gasification and contraction of the organic components during the pyrolysis process, the generated carbonaceous material generally maintains the rod-shaped morphology of Bi MOF, but a large number of pores are harvested inside, eventually forming an internal honeycomb structure.
[0022] Application of a carbon-based material doped with a non-metallic element in a negative electrode of a potassium ion battery.
[0023] A potassium ion battery negative electrode comprises a coating material, wherein the coating material comprises the carbon-based material doped with a non-metallic element in a double coordination manner, a conductive material and a binder.
[0024] Preferably, the mass ratio of the material to the conductive material and the binder is 7-8:1-2:0.5-1, more preferably 7:2:1, 8:1:1 or 8:1.5:0.5, etc.;
[0025] Preferably, the conductive material is conductive carbon black, more preferably acetylene black;
[0026] The binder is sodium carboxymethyl cellulose.
[0027] A method for preparing a negative electrode of a potassium ion battery comprises mixing the material, a conductive material and a binder with water to form a uniform slurry, then coating the slurry on a metal foil, and drying the slurry to obtain the negative electrode of the potassium ion battery.
[0028] Preferably, the drying is carried out under vacuum conditions;
[0029] The drying temperature is 50-80° C. and the drying time is 12-48 h.
[0030] The invention discloses an application of a negative electrode of a potassium ion battery in a potassium ion battery.
[0031] A potassium ion battery comprises the potassium ion battery negative electrode.
[0032] Preferably, the electrolyte in the potassium ion battery is a potassium hexafluorophosphate (KPF6) solution with a concentration of 0.8-1 mol / L, the solvent of the electrolyte is ethylene glycol dimethyl ether (DME), or a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1; the diaphragm in the potassium ion battery is glass fiber.
[0033] Compared with the prior art, the present invention has the following advantages and technical effects:
[0034] The present invention provides a carbon-based material doped with a non-metallic element in a dual coordination manner, and a preparation method and application thereof. The negative electrode material provided by the present invention has a simple synthesis method, a stable structure, abundant active sites, a wide potassium ion transport channel, and a large buffer space, and can well improve the rate and cycle stability of potassium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0036] Figure 1 This is a scanning electron microscope photograph of the Bi-MOF precursor prepared in Example 1;
[0037] Figure 2 This is a transmission electron microscope photo of O-Bi-N@HCR prepared in Example 1;
[0038] Figure 3 Schematic diagram of the structure of O-Bi-N@HCR prepared in the present invention;
[0039] Figure 4 X-ray diffraction pattern and Raman pattern of O-Bi-N@HCR prepared in Example 1;
[0040] Figure 5 This is a rate performance diagram of the O-Bi-N@HCR negative electrode material prepared in Example 2;
[0041] Figure 6 The O-Bi-N@HCR negative electrode material prepared in Example 2 was -1 Cyclic performance diagram at current density of ;
[0042] Figure 7 The O-Bi-N@HCR negative electrode material prepared in Example 2 was -1 Cyclic performance diagram at current density of ;
[0043] Figure 8 This is a transmission electron micrograph of O-Bi-N@HCR prepared in Example 3;
[0044] Fig. 9 This is a transmission electron micrograph of O-Bi-N@HCR prepared in Example 4;
[0045] Fig.10 This is a scanning electron microscope photograph of the O-Bi-N@HCR precursor prepared in Example 5. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0048] An embodiment of the present invention provides a carbon-based material doped with a non-metallic element in a doped manner. The carbon-based material is a honeycomb carbon rod material doped with nitrogen and oxygen doped bismuth metal single atoms.
[0049] The present invention also provides a method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, comprising the following steps:
[0050] The bismuth source and the organic ligand are dispersed in an organic solvent and subjected to a hydrothermal reaction to obtain a precursor, and then the precursor is subjected to a carbon reduction coordination treatment with a nitrogen-containing reducing agent to obtain the non-metallic element doped carbon-based material.
[0051] In a preferred embodiment, the mass ratio of the bismuth source to the organic ligand is 1:(1-10).
[0052] In a preferred embodiment, the bismuth source includes one of bismuth nitrate pentahydrate, bismuth trichloride, bismuth citrate, bismuth nitrite, bismuth hypophosphite, sodium bismuth carbonate or bismuth subcarbonate;
[0053] The organic ligand is one of pyridine dicarboxylic acid, heterocyclic dicarboxylic acid, trimesic acid, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, biphenyltricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene or 1,3,6,8-tetrakis(p-benzoic acid)pyrene;
[0054] In a preferred embodiment, the temperature of the hydrothermal reaction is 100-180° C. and the time is 1-24 h.
[0055] In a preferred embodiment, the mass ratio of the precursor to the nitrogen-containing reducing agent is 1:(1-10);
[0056] The nitrogen-containing reducing agent is dicyandiamide.
[0057] In a preferred embodiment, the reduction coordination reaction specifically comprises the following steps:
[0058] The precursor and the nitrogen-containing reducing agent are placed in two quartz boats respectively, and the temperature is raised to 900-1100° C. at a rate of 2-20° C. / min in an inert atmosphere and kept at this temperature for 1-24 hours.
[0059] The embodiment of the present invention also provides an application of a carbon-based material doped with a non-metallic element in a negative electrode of a potassium ion battery.
[0060] An embodiment of the present invention further provides a potassium ion battery negative electrode, comprising a coating material, wherein the coating material comprises the carbon-based material doped with a non-metallic element in a doubly coordinated manner, a conductive material and a binder.
[0061] In a preferred embodiment, the mass ratio of the material to the conductive material and the binder is 7-8:1-2:0.5-1, more preferably 7:2:1, 8:1:1 or 8:1.5:0.5, etc.;
[0062] In a preferred embodiment, the conductive material is conductive carbon black, more preferably acetylene black;
[0063] The binder is sodium carboxymethyl cellulose.
[0064] The embodiment of the present invention also provides a method for preparing a negative electrode of a potassium ion battery, wherein the carbon-based material doped with a non-metallic element in a dual coordination manner, a conductive material and a binder are mixed with water to form a uniform slurry, which is then coated on a metal foil and dried to obtain the negative electrode of the potassium ion battery.
[0065] In a preferred embodiment, the drying is performed under vacuum conditions;
[0066] The drying temperature is 50-80° C. and the drying time is 12-48 h.
[0067] The embodiment of the present invention also provides an application of a negative electrode of a potassium ion battery in a potassium ion battery.
[0068] An embodiment of the present invention further provides a potassium ion battery, comprising the potassium ion battery negative electrode.
[0069] In a preferred embodiment, the electrolyte in the potassium ion battery is a potassium hexafluorophosphate (KPF6) solution with a concentration of 0.8-1 mol / L, and the solvent of the electrolyte is ethylene glycol dimethyl ether (DME), or a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1; the diaphragm in the potassium ion battery is glass fiber.
[0070] Unless otherwise specified, the "room temperature" in the present invention refers to 15-30°C.
[0071] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources;
[0072] Among them, bismuth sources were purchased from Shanghai MacLean Biochemical Technology Co., Ltd., with a parameter index of 99.99%;
[0073] Dicyandiamide was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. with a parameter index of ≥99.99%.
[0074] Example 1
[0075] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner comprises the following steps:
[0076] (1) Disperse 600 mg of bismuth nitrate pentahydrate and 3000 mg of organic ligand trimesic acid in 60 mL of methanol and stir for 30 min to form a transparent uniform solution;
[0077] (2) placing the transparent uniform solution in step (1) in a 100 mL hydrothermal reactor and conducting a hydrothermal reaction at 120° C. for 24 h. After the reaction is completed, the product is filtered and washed with 95% methanol, and then dried at 65° C. for 24 h to obtain a Bi-MOF precursor;
[0078] (3) 50 mg of the Bi-MOF precursor obtained in step (2) and 500 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow. The temperature was raised from room temperature to 1000°C in a nitrogen atmosphere at a rate of 2°C / min and kept at this temperature for 3 h for sufficient calcination to obtain a nitrogen-oxygen double-coordinated bismuth metal single atom doped honeycomb carbon rod material, which was labeled as O-Bi-N@HCR.
[0079] Example 2
[0080] A method for preparing a negative electrode of a potassium ion battery and a lithium ion battery comprises the following steps:
[0081] (1) The O-Bi-N@HCR obtained in Example 1 was mixed with conductive carbon black and a binder in a mass ratio of 7:2:1, and then 1.5 mL of deionized water was added to grind into a uniform slurry, and then evenly coated on a copper foil. After the surface was dry, it was transferred to a vacuum drying oven and dried at 65°C for 24 hours to obtain a potassium ion battery negative electrode sheet, which was recorded as O-Bi-N@HCR negative electrode material;
[0082] (2) The O-Bi-N@HCR negative electrode material obtained in step (1) and a potassium metal sheet (potassium metal sheet as a counter electrode and a reference electrode) are assembled into a potassium ion battery in a glove box filled with argon. The electrolyte used is a potassium hexafluorophosphate (KPF6) solution in ethylene glycol dimethyl ether (DME) with a concentration of 1 mol / L. The separator used is glass fiber.
[0083] The morphology analysis and performance test of the O-Bi-N@HCR prepared in this example were performed, and the results were as follows:
[0084] Figure 1 This is a scanning electron microscope photograph of the Bi-MOF precursor obtained in Example 1. It can be seen that the morphology of the Bi-MOF precursor is in the shape of a slender rod.
[0085] Figure 2 This is a transmission electron microscope photo of the O-Bi-N@HCR obtained in Example 1. It can be seen that the internal structure of the carbon layer presents a porous honeycomb structure.
[0086] Figure 3 Schematic diagram of the structure of O-Bi-N@HCR obtained in Example 1, wherein, from the microstructural analysis, the carbon atoms on the carbon rods are replaced by bismuth metal atoms with nitrogen and oxygen doubly coordinated to form vacancies and defects.
[0087] Figure 4 The X-ray diffraction pattern and Raman pattern of O-Bi-N@HCR obtained in Example 1 show that the carbon material has an ordered structure.
[0088] Figure 5 This is the rate performance diagram of the O-Bi-N@HCR negative electrode material obtained in Example 2. It can be seen that the rate performance of the O-Bi-N@HCR negative electrode material can reach up to 30A g -1 .
[0089] Figure 6 The O-Bi-N@HCR negative electrode material obtained in Example 2 was 1000 mA g -1 The cycling performance diagram at the current density of 1000 mA g -1 The cycle performance can reach more than 1200 cycles at a current density of .
[0090] Figure 7 The O-Bi-N@HCR negative electrode material obtained in Example 2 was -1 The cycling performance diagram under the current density of 5000 mA g -1 The cycle performance can reach more than 4200 cycles at a current density of .
[0091] Example 3
[0092] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner is different from that in Example 1 only in that step (3) is specifically as follows:
[0093] 50 mg of the Bi-MOF precursor obtained in step (2) and 100 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow, and the temperature was raised from room temperature to 1000°C in a nitrogen atmosphere at a rate of 2°C / min, and kept at this temperature for 3 hours for sufficient calcination to obtain a nitrogen-oxygen dicoordinated bismuth metal single atom doped honeycomb carbon rod material, which was labeled as O-Bi-N@HCR.
[0094] The other steps and parameters are the same as those in Example 1.
[0095] Figure 8 This is a transmission electron microscope photograph of the O-Bi-N@HCR obtained in Example 3. It can be seen that compared with the O-Bi-N@HCR prepared in Example 1, the surface of the carbon rod is smoother and has fewer holes and defects.
[0096] Example 4
[0097] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner is different from that in Example 1 in that step (3) specifically comprises the following steps:
[0098] 50 mg of the Bi-MOF precursor obtained in step (2) and 1500 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow, and the temperature was increased from room temperature to 1000°C in a nitrogen atmosphere at a heating rate of 2°C / min, and kept at this temperature for 3 hours for sufficient calcination to obtain a nitrogen-oxygen double-coordinated bismuth metal single atom doped honeycomb carbon rod material, which was labeled as O-Bi-N@HCR.
[0099] The other steps and parameters are the same as those in Example 1.
[0100] Fig. 9 This is a transmission electron microscope photograph of the O-Bi-N@HCR obtained in Example 4. It can be seen that compared with the O-Bi-N@HCR prepared in Example 1, the morphology of the carbon rods cannot be maintained.
[0101] Example 5
[0102] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, which is different from Example 1 only in that step (1) comprises the following steps:
[0103] 600 mg of bismuth nitrate pentahydrate and 3000 mg of the organic ligand trimesic acid were dispersed in a mixed solvent of methanol and ethylene glycol (the volume ratio of methanol to ethylene glycol was 4:2) with a total volume of 60 mL, and stirred for 30 minutes to form a transparent uniform solution.
[0104] The other steps and parameters are the same as those in Example 1.
[0105] Fig.10 This is a scanning electron microscope photograph of the Bi-MOF precursor obtained in Example 5. It can be seen that the morphology of the Bi-MOF precursor is a long cone.
[0106] Example 6
[0107] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, which is different from Example 1 only in that step (1) comprises the following steps:
[0108] 600 mg of bismuth nitrate pentahydrate and 3000 mg of organic ligand trimesic acid were dispersed in a total volume of 60 mL of a mixed solvent of acetone and ethylene glycol (the volume ratio of acetone to ethylene glycol was 1:4), and stirred for 30 min to form a transparent uniform solution.
[0109] The other steps and parameters are the same as those in Example 1.
[0110] Example 7
[0111] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, which is different from Example 1 only in that step (3) comprises the following steps:
[0112] 50 mg of the Bi-MOF precursor obtained in step (2) and 700 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow, and the temperature was raised from room temperature to 1000°C in a nitrogen atmosphere at a heating rate of 2°C / min, and kept warm for 3 hours for sufficient calcination to obtain a nitrogen-oxygen double-coordinated bismuth metal single atom doped honeycomb carbon rod material, marked as O-Bi-N@HCR.
[0113] The other steps and parameters are the same as those in Example 1.
[0114] Example 8
[0115] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, which is different from Example 1 only in that step (3) comprises the following steps:
[0116] 50 mg of the Bi-MOF precursor obtained in step (2) and 1000 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow, and the temperature was raised from room temperature to 1100°C in a nitrogen atmosphere at a rate of 2°C / min, and kept warm for 3 hours for sufficient calcination to obtain a nitrogen-oxygen double-coordinated bismuth metal single atom doped honeycomb carbon rod material, marked as O-Bi-N@HCR.
[0117] The other steps and parameters are the same as those in Example 1.
[0118] Comparative Example 1
[0119] A method for preparing a carbon-based material doped with a non-metallic element in a dual coordination manner, which is different from Example 1 only in that step (3) comprises the following steps:
[0120] 50 mg of the Bi-MOF precursor obtained in step (2) was placed in a quartz boat, and then placed in a tube furnace for heat treatment. The temperature was raised from room temperature to 1000°C at a heating rate of 2°C / min in a nitrogen atmosphere, and the temperature was kept for 3 hours for sufficient calcination to obtain the carbon material Bare-NC.
[0121] The other steps and parameters are the same as those in Example 1.
[0122] Compared with Example 1, Comparative Example 1 does not contain dicyandiamide, and the Bare-NC holes and defects formed are significantly reduced, which is not conducive to improving the battery capacity, fast charging and discharging, and cycle stability.
[0123] Comparative Example 2
[0124] 50 mg of glucose and 1000 mg of dicyandiamide were placed in two quartz boats respectively, and then placed in a tube furnace for heat treatment. The quartz boat containing dicyandiamide was placed above the air flow. In a nitrogen atmosphere, the temperature was increased from room temperature to 1000°C at a rate of 2°C / min and kept at this temperature for 3 hours for sufficient calcination to obtain the carbon material NC.
[0125] The other steps and parameters are the same as those in Example 1.
[0126] Compared with Example 1, in Comparative Example 2, glucose is directly used as a carbon source to be calcined with dicyandiamide, and the material structure is a carbon sheet, which is not conducive to improving the cycle stability.
[0127] The negative electrode materials prepared in Examples 3-8 and Comparative Examples 1-2 were used for potassium ion battery negative electrodes and potassium ion batteries. The preparation method was the same as that in Example 2, and the rate performance of the fifth cycle was tested at current densities of 0.2 A / g and 30 A / g. The results are shown in Table 1.
[0128] Table 1 Rate performance at current densities of 0.2 A / g and 30 A / g
[0129]
[0130] It can be seen from the test results in Table 1 that, compared with the comparative example, the potassium ion battery prepared by using the negative electrode materials obtained in Examples 1-7 of the present invention has a greatly improved rate performance under the condition of 30 A / g.
[0131] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a carbon-based material doped with a non-metallic element, characterized in that: The following steps are involved: The bismuth source and the organic ligand are dispersed in an organic solvent and subjected to a hydrothermal reaction to obtain a precursor, and then the precursor is subjected to a carbon reduction coordination treatment with a nitrogen-containing reducing agent to obtain the non-metallic element doped carbon-based material; The organic solvent is methanol; The temperature of the hydrothermal reaction is 120°C and the time is 24h; The reduction coordination treatment specifically comprises the following steps: The precursor and the nitrogen-containing reducing agent are placed in two quartz boats respectively, and the temperature is raised to 1000° C. at a rate of 2° C. / min in an inert atmosphere and kept at this temperature for 3 hours; Each Bi(III) cation in the precursor is coordinated with nine O atoms; The non-metallic element doped carbon-based material is a nitrogen-oxygen doped bismuth metal single atom doped honeycomb carbon rod material; the carbon atoms on the nitrogen-oxygen doped bismuth metal single atom are replaced by nitrogen-oxygen doped bismuth metal atoms, and the bismuth metal single atom is coordinated with two O atoms and four N atoms; The mass ratio of the bismuth source to the organic ligand is 1:
5. The bismuth source is bismuth nitrate pentahydrate; the organic ligand is trimesic acid; The mass ratio of the precursor to the nitrogen-containing reducing agent is 1:10; The nitrogen-containing reducing agent is dicyandiamide.
2. Application of the carbon-based material doped with a double coordination non-metallic element prepared by the method for preparing the carbon-based material doped with a double coordination non-metallic element as claimed in claim 1 in the negative electrode of a potassium ion battery.
3. A potassium ion battery negative electrode, characterized in that: The coating material comprises a coating material, wherein the coating material comprises a carbon-based material doped with a non-metallic element in a double coordination manner prepared by the preparation method according to claim 1, a conductive material and a binder.
4. Use of the potassium ion battery cathode electrode as claimed in claim 3 in a potassium ion battery.
5. A potassium ion battery, characterized in that: Comprising the potassium ion battery negative electrode as described in claim 3.