Method for photocatalytic treatment of hexavalent chromium in water, chromium-containing hydrotalcite and application thereof
The loaded polyacid@zeolite imidazolate framework material reduces hexavalent chromium in water to trivalent chromium under light conditions to form stable chromium-containing hydrotalcite, which solves the problem of low removal rate of hexavalent chromium and dielectric dichloride in the existing technology. To solve the problem of secondary pollution, efficient and environmentally friendly water purification has been achieved.
Patent Information
- Application Number
- CN202410037990.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-10
AI Technical Summary
The existing technology has problems of low removal rate and secondary pollution when treating hexavalent chromium pollution in water bodies. In particular, the chromium-containing sludge produced is easy to cause environmental pollution. The equipment is complicated and it is easy to produce a large amount of acid-base waste liquid.
The supported polyacid@zeolite imidazolate framework material is used as a catalyst to perform light reduction treatment on chromium-containing water with a pH of 5-9, converting hexavalent chromium into trivalent chromium and forming chromium-containing hydrotalcite to avoid secondary pollution.
It achieves efficient removal of hexavalent chromium in water, and the generated chromium-containing hydrotalcite has high stability, avoids secondary pollution, and provides a simple and effective treatment method.
Smart Images

Figure CN117902670B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic functional materials and heavy metal removal, and in particular to a method for photocatalytically treating hexavalent chromium in water, chromium-containing hydrotalcite and applications thereof. Background Art
[0002] Heavy metal pollutants in water are toxic to organisms and cannot be naturally degraded. Heavy metal pollutants will also gradually accumulate in the ecosystem and enter the human body through the food chain, causing irreversible damage to the human body. Among them, hexavalent chromium (Cr(VI)) has the characteristics of high toxicity, high solubility and difficulty in degradation. Its existence form in water changes with the change of pH, mainly in the form of Cr2O7 2- With HCrO4 - Stable existence.
[0003] The main sources of acidic wastewater containing hexavalent chromium are electroplating, leather tanning, wood preservation, paint and pigment production and other industries; the main source of alkaline wastewater containing hexavalent chromium is the leaching liquid containing a large amount of hexavalent chromium that flows out from the land contaminated by alkaline chromium slag after being soaked in rainwater.
[0004] At present, the commonly used hexavalent chromium treatment technologies in industry mainly include: sulfite reduction method, ferrous sulfate-lime treatment method, micro-electrolysis treatment method and ion exchange treatment method, etc. The above methods have obvious disadvantages, such as the chromium-containing sludge produced is easy to cause secondary pollution, the equipment is complicated and it is easy to produce a large amount of acid and alkali waste liquid.
[0005] Therefore, there is an urgent need to develop a method for treating chromium-containing wastewater with high hexavalent chromium and total chromium removal rates and without causing secondary pollution. Summary of the invention
[0006] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a method for photocatalytically treating hexavalent chromium in water, chromium-containing hydrotalcite and application thereof.
[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for photocatalytic treatment of hexavalent chromium in water, wherein the method comprises: using a supported polyacid@zeolite imidazolate framework material as a catalyst to perform photoreduction treatment on a chromium-containing water body with a pH of 5-9.
[0008] The second aspect of the present invention provides a chromium-containing hydrotalcite obtained by the method described in the first aspect.
[0009] The third aspect of the present invention provides the use of the chromium-containing hydrotalcite described in the second aspect as a catalyst in photocatalytic water decomposition to produce hydrogen, photocatalytic organic matter degradation and electrochemical sensors.
[0010] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0011] (1) The present invention uses a supported polyacid @ zeolite imidazolate framework material as a catalyst to photocatalytically reduce hexavalent chromium to trivalent chromium under light conditions and form chromium-containing hydrotalcite for fixation. The hexavalent chromium is completely converted and the removal rate is high; the chromium-containing hydrotalcite K produced by the reduction sp Low, stable structure, can avoid secondary pollution.
[0012] (2) The present invention provides an effective way to degrade hexavalent chromium, which can effectively solve the problem of secondary pollution easily caused by hexavalent chromium pollution treatment in water bodies.
[0013] (3) The method of the present invention is technically feasible and easy to operate, and can effectively treat hexavalent chromium ions present in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The PW prepared in Preparation Example 1 of the present invention 12 @TEM image of ZIF-8;
[0015] Figure 2 PW is generated after the reaction of Example 1 of the present invention 12 @TEM image of ZnCr-LDH;
[0016] Figure 3 This is a time-resolved XRD pattern during the treatment process of Example 1 of the present invention;
[0017] Figure 4 The nitrogen adsorption-desorption curves of the material before and after treatment in Example 1 of the present invention;
[0018] Figure 5 PW is generated after the reaction of Example 1 of the present invention 12 @XPS full spectrum of ZnCr-LDH;
[0019] Figure 6 PW is generated after the reaction of Example 1 of the present invention 12 @X-ray absorption spectrum of Zn in ZnCr-LDH;
[0020] Figure 7 The removal kinetic curves of hexavalent chromium and total chromium at different initial pH values in Examples 1 and 4 of the present invention are shown. DETAILED DESCRIPTION
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] The first aspect of the present invention provides a method for photocatalytic treatment of hexavalent chromium in water, wherein the method comprises: using a supported polyacid @ zeolite imidazolate framework material as a catalyst to perform photoreduction treatment on a chromium-containing water body with a pH of 5-9.
[0023] The present invention uses a supported polyacid @ zeolite imidazolate skeleton material as a catalyst to perform light reduction treatment on a chromium-containing water body with a pH of 5-9. After the reduction reaction is completed, the hexavalent chromium in the water is completely converted into trivalent chromium and decomposes and releases the M released by the supported polyacid @ zeolite imidazolate skeleton material. 2+ (For example, Zn 2+ 、Co 2+ ) is combined to form chromium-containing hydrotalcite, thereby achieving the purpose of treating hexavalent chromium in water. The treatment method of the present invention has a high removal rate for hexavalent chromium, and the final product is chromium-containing hydrotalcite. According to literature reports, due to the multiple interactions in the structure of hydrotalcite, its solubility product constant is lower than that of the corresponding hydroxide, so the removed product has the characteristics of stable structure, which can avoid secondary pollution of trivalent chromium.
[0024] The present invention is a method for removing hexavalent chromium from wastewater with a clear and stable product structure, thereby avoiding secondary pollution, and is also a method for constructing a chromium-containing hydrotalcite (such as PW 12 @ZnCr-LDH) functional material method, the processed product can be reused.
[0025] The water after reduction (degradation) in the present invention usually contains hexavalent chromium and trivalent chromium at the same time, wherein the concentration of hexavalent chromium before and after the reaction can be measured by UV-visible spectrophotometer, and the concentration of total chromium before and after the reaction can be measured by ICP.
[0026] The invention can directly treat water bodies containing hexavalent chromium pollutants, including acidic electroplating waste liquid and alkaline chromium slag leaching liquid containing hexavalent chromium.
[0027] In some embodiments of the present invention, the initial concentration of hexavalent chromium ions in the chromium-containing water is 1-300 ppm, preferably 1-100 ppm.
[0028] In some embodiments of the present invention, the pH is 6 to 9. The pH value of the water body can be adjusted by using commonly used acids and bases, such as hydrochloric acid, nitric acid and other acids or ammonia water, sodium hydroxide and other bases.
[0029] In some embodiments of the present invention, the wavelength band of the illumination is the full wavelength band or the ultraviolet wavelength band. The present invention reduces hexavalent chromium by illumination, and the illumination wavelength band can be determined according to actual needs, and the preferred wavelength band is the full wavelength band.
[0030] In some embodiments of the present invention, the light reduction treatment time is 30 min-24 h, preferably 12-24 h. The treatment time used in the present invention varies with the initial concentration of hexavalent chromium, the type and amount of the supported polyacid @ zeolite imidazolate framework material, the light intensity and wavelength.
[0031] In some embodiments of the present invention, the temperature of the light reduction treatment is 20-60° C., preferably 25° C. The treatment process of the present invention is simple, and can usually be carried out under normal temperature and pressure. The reaction temperature can also be adjusted appropriately, such as within the range of 40-60° C. to achieve the purpose of the present invention.
[0032] In some embodiments of the present invention, the amount of the supported polyacid@zeolite imidazolate framework material is 0.1-5 mg / mL, preferably 0.5-3 mg / mL, based on the volume of the chromium-containing water. In the present invention, too little amount of the catalyst will reduce the removal rate of chromium.
[0033] In some embodiments of the present invention, the supported polyacid@zeolite imidazolate framework material is prepared by encapsulating the polyacid in the zeolite imidazolate framework material through an in-situ encapsulation method.
[0034] For example, the polyacid and the metal salt are first dissolved in a methanol solution, and then the methanol solution of 2-methylimidazole is dripped into the generated supported polyacid@zeolite imidazole framework material. The polyacid used is selected from at least one of phosphotungstic acid, phosphomolybdic acid, phosphomolybdicvanadic polyacid and the potassium salt or sodium salt of the aforementioned polyacid, preferably phosphotungstic acid or phosphomolybdic acid, and the metal salt is generally nitrate or chloride. The prepared supported polyacid@zeolite imidazole framework material is dried for standby use.
[0035] In some embodiments of the present invention, the polyacid in the supported polyacid@zeolite imidazolate framework material is selected from at least one of phosphotungstic acid, phosphomolybdic acid and phosphomolybdicvanadic acid, preferably phosphotungstic acid or phosphomolybdic acid.
[0036] In some embodiments of the present invention, the zeolite imidazolate framework material in the supported polyacid@zeolite imidazolate framework material is selected from at least one of ZIF-8, ZIF-65, ZIF-67, ZIF-71 and ZIF-90, preferably ZIF-8.
[0037] In some embodiments of the present invention, the loading amount of the polyacid in the supported polyacid@zeolite imidazolate framework material is 4.8-15%, preferably 6.7%.
[0038] In some embodiments of the present invention, the product obtained by the method is separated into solid and liquid and then dried to obtain chromium-containing hydrotalcite.
[0039] The second aspect of the present invention provides a chromium-containing hydrotalcite obtained by the method described in the first aspect.
[0040] In some embodiments of the present invention, the molar ratio of the divalent metal ions to Cr(III) in the chromium-containing hydrotalcite is 1:4-4:1, preferably 1:1-3.
[0041] In some embodiments of the present invention, the divalent metal ion is Zn 2+ and / or Co 2+ .
[0042] In some embodiments of the present invention, the chromium-containing hydrotalcite is loaded with a polyacid and has a hollow shell structure, wherein the polyacid is phosphotungstic acid or phosphomolybdic acid.
[0043] The third aspect of the present invention provides the use of the chromium-containing hydrotalcite as a catalyst in photocatalytic water decomposition to produce hydrogen, photocatalytic organic matter degradation and electrochemical sensors.
[0044] The method for photocatalytic degradation of hexavalent chromium in water proposed by the present invention shows a significant degradation effect, has a high removal efficiency for hexavalent chromium, and the chromium-containing hydrotalcite generated after the removal of hexavalent chromium has stable properties. The method of the present invention is technically feasible, simple to operate, and easy to implement. The method of the present invention is used to remove hexavalent chromium pollution in water and has good economic and environmental benefits.
[0045] The present invention will be described in detail below through examples.
[0046] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.
[0047] In the following examples or comparative examples, the removal rate refers to the ratio of the hexavalent chromium or total chromium content removed by reduction (degradation) to the hexavalent chromium or total chromium content in the initial water body.
[0048] Preparation Example 1
[0049] 0.582g zinc nitrate hexahydrate was dissolved in 25mL methanol to form solution 1, 50mg phosphotungstic acid was dissolved in 25mL methanol to form solution 2, and 0.6568g 2-methylimidazole was dissolved in 25mL methanol to form solution 3. Solution 2 was first added to solution 1 and stirred for 30min, and then solution 3 was added to the above mixed solution and stirred for 3h. After solid-liquid separation of the obtained product, the solid part was washed and dried to obtain the supported polyacid @ zeolite imidazole ester framework material PW 12 @ZIF-8, in which the loading amount of phosphotungstic acid is 6.7%.
[0050] Figure 1The prepared PW 12 TEM image of @ZIF-8. It can be seen that the prepared PW 12 @ZIF-8 has a rhombic dodecahedron morphology and a particle size of about 400 nm.
[0051] Preparation Example 2
[0052] 0.582g zinc nitrate hexahydrate was dissolved in 25mL methanol to form solution 1, 25mg phosphotungstic acid was dissolved in 25mL methanol to form solution 2, and 0.6568g 2-methylimidazole was dissolved in 25mL methanol to form solution 3. Solution 2 was first added to solution 1 and stirred for 30min, and then solution 3 was added to the above mixed solution and stirred for 3h. After solid-liquid separation of the obtained product, the solid part was washed and dried to obtain the supported polyacid @ zeolite imidazole ester framework material PW 12 @ZIF-8, in which the loading amount of phosphotungstic acid is 4.8%.
[0053] Preparation Example 3
[0054] 0.582g zinc nitrate hexahydrate was dissolved in 25mL methanol to form solution 1, 50mg phosphomolybdic acid was dissolved in 25mL methanol to form solution 2, and 0.6568g 2-methylimidazole was dissolved in 25mL methanol to form solution 3. Solution 2 was first added to solution 1 and stirred for 30min, and then solution 3 was added to the above mixed solution and stirred for 3h. After solid-liquid separation of the obtained product, the solid part was washed and dried to obtain the supported polyacid @ zeolite imidazole ester framework material PMo 12 @ZIF-8, in which the loading amount of phosphomolybdic acid is 1.8%.
[0055] Preparation Example 4
[0056] 0.25g PVP and 0.24g 2-formyl imidazole were dissolved in a mixed solution of 10mL water and 2.5mL methanol to form solution 1, 5mg phosphotungstic acid was dissolved in 2mL water to form solution 2, and solution 2 was added to solution 1 to form mixed solution 1, and the mixed solution 1 was heated to 70°C and maintained for 5min, and then the temperature was reduced to 42°C. 0.25g zinc nitrate hexahydrate was dissolved in 2mL methanol to form solution 3, and solution 3 was dropped into mixed solution 1 and reacted for 5min. After solid-liquid separation of the obtained product, the solid part was washed and dried to obtain the supported polyacid @ zeolite imidazole ester framework material PW 12 @ZIF-90, in which the loading amount of phosphotungstic acid is 3.6%.
[0057] Comparative Preparation Example 1
[0058] 0.582 g of zinc nitrate hexahydrate was dissolved in 25 mL of methanol to form solution 1, and 0.6568 g of 2-methylimidazole was dissolved in 25 mL of methanol to form solution 2. Solution 2 was added to the above-mentioned mixed solution and stirred for 3 hours. After solid-liquid separation of the obtained product, the solid part was washed and dried to obtain the zeolite imidazole ester framework material ZIF-8.
[0059] Example 1
[0060] The PW with a phosphotungstic acid loading of 6.7% in Preparation Example 1 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 6. The initial concentration of hexavalent chromium ions in the chromium-containing water was 60 ppm, the catalyst dosage was 1 mg / mL, the light wavelength was full-band, and the reaction was carried out at room temperature for 24 hours. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, its TEM image is as follows Figure 2 As shown. Among them, Zn 2+ The molar ratio to Cr(III) is 1:2.5.
[0061] It was calculated that the hexavalent chromium removal rate was 100% and the total chromium removal rate was 99.8%.
[0062] Figure 3 The time-resolved XRD pattern during the treatment process shows that the characteristic diffraction peaks at 7.3°, 10.4° and 12.7° belonging to ZIF-8 weakened with the extension of reaction time, while the characteristic peaks at 34.5° and 59.8° belonging to hydrotalcite strengthened, proving that ZIF-8 was continuously converted into ZnCr-LDH as the reaction proceeded.
[0063] Figure 4 The nitrogen adsorption-desorption curves of the materials before and after treatment are shown in Figure 2. 12 @ZIF-8 isotherm is a type I isotherm, indicating that the material has a microporous structure. 12 The isotherm of @ZnCr-LDH shows an H3 hysteresis loop formed by the lamellar stacking of LDH, and the overall isotherm presents a type IV isotherm, indicating a mesoporous structure.
[0064] Figure 5 PW is generated after the reaction 12 @The full XPS spectrum of ZnCr-LDH shows the presence of Zn, Cr, P and W elements, proving that the polyacid is loaded on ZnCr-LDH.
[0065] Figure 6 PW is generated after the reaction 12The X-ray absorption spectrum of Zn in @ZnCr-LDH shows that Zn has the same oscillation as that of hydrotalcite ZnCr-LDH in the X-ray absorption fine structure region, proving that the coordination structure of Zn is the same as that of hydrotalcite.
[0066] Example 2
[0067] The PW with a phosphotungstic acid loading of 6.7% in Preparation Example 1 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 6. The initial concentration of hexavalent chromium ions in the chromium-containing water was 60 ppm, the catalyst dosage was 1 mg / mL, the light wavelength was full-band, and the reaction was carried out at room temperature for 18 hours. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, where Zn 2+ The molar ratio to Cr(III) is 1:2.5.
[0068] According to calculation, the hexavalent chromium removal rate is 100% and the total chromium removal rate is 99.7%.
[0069] Example 3
[0070] The PW with a phosphotungstic acid loading of 4.8% in Preparation Example 2 was used. 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 6. The initial concentration of hexavalent chromium ions in the chromium-containing water was 60 ppm, the catalyst dosage was 3 mg / mL, the illumination wavelength was full-band, and the reaction was carried out at room temperature for 24 hours. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, where Zn 2+ The molar ratio with Cr(III) is 1:1.
[0071] After calculation, the hexavalent chromium removal rate is 100% and the total chromium removal rate is 100%.
[0072] Example 4
[0073] The PW with a phosphotungstic acid loading of 6.7% in Preparation Example 1 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 8. The initial concentration of hexavalent chromium ions in the chromium-containing water was 60ppm, the catalyst dosage was 1mg / mL, the wavelength of light was full-band, and the reaction was carried out at room temperature for 24h. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, where Zn 2+ The molar ratio to Cr(III) is 1:2.5.
[0074] According to calculation, the hexavalent chromium removal rate is 100% and the total chromium removal rate is 99.4%.
[0075] Example 5
[0076] The PW with a phosphotungstic acid loading of 6.7% in Preparation Example 1 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 6. The initial concentration of hexavalent chromium ions in the chromium-containing water was 40 ppm, the catalyst dosage was 1 mg / mL, the illumination wavelength was full-band, and the reaction was carried out at room temperature for 12 hours. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, where Zn 2+ The molar ratio to Cr(III) is 1:1.8.
[0077] According to calculation, the hexavalent chromium removal rate is 99.9% and the total chromium removal rate is 99.4%.
[0078] Example 6
[0079] The PW with a phosphotungstic acid loading of 6.7% in Preparation Example 1 12 @ZIF-8 was used as a catalyst to perform photoreduction treatment on chromium-containing water with a pH of 6. The initial concentration of hexavalent chromium ions in the chromium-containing water was 60 ppm, the catalyst dosage was 3 mg / mL, the illumination wavelength was full-band, and the reaction was carried out at room temperature for 24 hours. After the reaction, chromium-containing hydrotalcite PW was obtained. 12 @ZnCr-LDH, where Zn 2+ The molar ratio to Cr(III) is 1:1.1.
[0080] After calculation, the hexavalent chromium removal rate is 100% and the total chromium removal rate is 100%.
[0081] Comparative Example 1
[0082] The chromium-containing water body is treated according to the method of Example 1, except that the pH value of the chromium-containing water body is 3.
[0083] According to calculation, the removal rate of hexavalent chromium is 76.8% and the removal rate of total chromium is 53.2%.
[0084] Comparative Example 2
[0085] The chromium-containing water body was treated according to the method of Example 1, except that the catalyst was ZIF-8 obtained in Comparative Preparation Example 1.
[0086] According to calculation, the removal rate of hexavalent chromium is 49.8% and the removal rate of total chromium is 37.3%.
[0087] Comparative Example 3
[0088] The chromium-containing water body is treated according to the method of Example 1, except that the catalyst is pure phosphotungstic acid.
[0089] After calculation, the hexavalent chromium removal rate is 25.0% and the total chromium removal rate is 0%.
[0090] From the above results, it can be seen that the removal efficiency of hexavalent chromium and the removal rate of total chromium can be improved by combining polyacid with zeolite imidazolate framework; with the increase of reaction time, the removal rate of hexavalent chromium and total chromium in water by the catalyst increases; the higher the initial concentration, the longer the time required to completely remove the hexavalent chromium and total chromium in the water; in the pH range of 6-8, the reaction rate decreases slightly with the increase of pH value, and at the same time, increasing the loading amount of polyacid within a certain range helps to improve the removal performance of hexavalent chromium under the same conditions.
[0091] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for photocatalytic treatment of hexavalent chromium in water, characterized in that: The method comprises: using a supported polyacid@zeolite imidazolate framework material as a catalyst, performing light reduction treatment on a chromium-containing water body with a pH of 5-9; The method obtains chromium-containing hydrotalcite loaded with polyacid and having a hollow shell structure; The polyacid in the supported polyacid@zeolite imidazolate framework material is selected from at least one of phosphotungstic acid, phosphomolybdic acid and phosphomolybdicvanadic polyacid.
2. The method according to claim 1, wherein: The initial concentration of hexavalent chromium ions in the chromium-containing water is 1-300 ppm; And / or, the pH is 6-9.
3. The method according to claim 2, wherein: The initial concentration of hexavalent chromium ions in the chromium-containing water is 1-100 ppm.
4. The method according to claim 1 or 2, wherein: The wavelength of the light is the full wavelength or ultraviolet wavelength; And / or, the light reduction treatment time is 30 min-24 h; And / or, the temperature of the light reduction treatment is 20-60°C.
5. The method according to claim 4, wherein: The light reduction treatment lasts for 12-24 hours.
6. The method according to claim 4, wherein: The temperature of the light reduction treatment is 25°C.
7. The method according to any one of claims 1 to 3, wherein: Calculated by the volume of the chromium-containing water body, the dosage of the supported polyacid@zeolite imidazole ester framework material is 0.1-5 mg / mL.
8. The method according to claim 7, wherein: Based on the volume of the chromium-containing water body, the dosage of the supported polyacid@zeolite imidazole ester framework material is 0.5-3 mg / mL.
9. The method according to any one of claims 1 to 3, wherein: The supported polyacid@zeolite imidazolate framework material is prepared by encapsulating the polyacid in the zeolite imidazolate framework material through an in-situ encapsulation method.
10. The method according to any one of claims 1 to 3, wherein: The zeolite imidazolate framework material in the supported polyacid@zeolite imidazolate framework material is selected from at least one of ZIF-8, ZIF-65, ZIF-67, ZIF-71 and ZIF-90; And / or, in the supported polyacid@zeolite imidazolate framework material, the loading amount of the polyacid is 4.8-15%.
11. The method according to claim 10, wherein: The polyacid in the supported polyacid@zeolite imidazolate framework material is phosphotungstic acid or phosphomolybdic acid.
12. The method according to claim 10, wherein: The zeolite imidazolate framework material in the supported polyacid@zeolite imidazolate framework material is ZIF-8.
13. The method according to claim 10, wherein: In the supported polyacid@zeolite imidazole ester framework material, the loading amount of the polyacid is 6.7%.
14. The method according to any one of claims 1 to 3, wherein: The product obtained by the method is separated into solid and liquid and then dried to obtain chromium-containing hydrotalcite.
15. A chromium-containing hydrotalcite obtained by the method according to any one of claims 1 to 14, wherein: The chromium-containing hydrotalcite is loaded with polyacid and has a hollow shell structure.
16. The chromium-containing hydrotalcite according to claim 15, wherein: The molar ratio of the divalent metal ion to Cr(III) in the chromium-containing hydrotalcite is 1:4-4:1; And / or, the polyacid is phosphotungstic acid or phosphomolybdic acid.
17. The chromium-containing hydrotalcite according to claim 16, wherein: The molar ratio of the divalent metal ions to Cr(III) in the chromium-containing hydrotalcite is 1:1-3.
18. The chromium-containing hydrotalcite according to claim 16, wherein: The divalent metal ion is Zn 2+ and / or Co 2+ .
19. Use of the chromium-containing hydrotalcite according to any one of claims 15 to 18 as a catalyst in photocatalytic water decomposition to produce hydrogen, photocatalytic organic matter degradation and electrochemical sensors.
Citation Information
Patent Citations
ZnTi hydrotalcite nanosheet catalyst and application of catalyst in hydrogen preparation by photoactivating and decomposing water
CN102872918A
Solid heteropoly acid composite catalyst with surface modified with variable valency metal ions, and preparation method and application thereof