Negative electrode sheet, its manufacturing method, secondary battery, battery module, battery pack and electrical device.
By setting an ion transport layer on the surface of the negative electrode active material layer, the problem of expansion of the negative electrode sheet in lithium-ion batteries is solved, the cycle life and safety performance of the battery are improved, and the continuous replenishment of lithium ions inside the negative electrode active layer is realized.
Patent Information
- Application Number
- CN202280060213.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-07
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-07-07
AI Technical Summary
During the cycle of lithium-ion batteries, the negative electrode sheet is prone to expansion, which can lead to a decline in battery performance or even failure. Existing technologies are unable to effectively solve this problem.
An ion transport layer is set on the surface of the negative electrode active material layer. The electronic conductivity of the ion transport layer is not higher than 1×10-7S/cm, and the lithium ion conductivity is not lower than 1×10-4S/cm. It is formed by ion-conducting polymer, electrolyte salt, inorganic fast ion conductor and inorganic ceramic to reduce the expansion rate of the negative electrode sheet.
It significantly improves the cycle life and safety performance of the battery, reduces the expansion rate of the electrode, ensures that lithium ions are continuously replenished inside the negative electrode active layer, and avoids lithium metal deposition on the surface.
Smart Images

Figure CN117941090B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of secondary battery technology, and in particular to a negative electrode sheet, a manufacturing method, a secondary battery, a battery module, a battery pack, and an electrical device. Background Technology
[0002] In recent years, the application scope of rechargeable batteries has become increasingly wide, and they have been deeply applied to energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace and other fields.
[0003] During the cycle of use, the negative electrode of a lithium-ion battery is prone to expansion, which can reduce the performance of the lithium-ion battery and even cause battery failure or safety accidents. Summary of the Invention
[0004] This application was made in view of the above-mentioned problems, and its purpose is to provide a negative electrode sheet with a low expansion rate after repeated use, thereby improving the cycle performance of the battery.
[0005] A first aspect of this application provides a negative electrode sheet, comprising: a negative electrode active material layer, and an ion transport layer located on at least one surface of the negative electrode active material layer, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and ionic conductivity not less than 1×10 -4 S / cm.
[0006] Therefore, this application solves the problem of lithium metal preferentially depositing on the negative electrode surface, leading to severe cell volume expansion, by setting an ion transport layer on the surface of the negative electrode active material layer. The ion transport layer makes it difficult for lithium ions to be deposited as lithium metal on the surface of the negative electrode active layer. Lithium ions diffuse, allowing for a continuous replenishment of lithium ions inside the negative electrode active layer, thereby achieving lithium metal deposition in the pores inside the electrode. The negative electrode of this application reduces the electrode expansion rate and significantly improves the cycle life of the battery.
[0007] In any embodiment, the ion transport layer comprises an ion-conducting polymer and an electrolyte salt. Forming the ion transport layer with an ion-conducting polymer and an electrolyte salt can reduce the negative electrode plate's...
[0008] Increased expansion rate improves battery cycle life.
[0009] In any embodiment, the ion transport layer further comprises at least one of an inorganic fast ion conductor and an inorganic ceramic. The addition of an inorganic fast ion conductor can further improve the ionic conductivity of the ion transport layer. The addition of inorganic ceramic can improve the strength of the ion transport layer, thereby further reducing the expansion rate of the negative electrode and improving the cycle performance of the battery cell.
[0010] In any embodiment, the ion-conducting polymer is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinyl alcohol, and polymethacrylate.
[0011] In any embodiment, the inorganic fast ion conductor is selected from one or more of garnet-type lithium lanthanum zirconium oxide (LLZO), perovskite-structured lithium lanthanum titanium oxide (LLTO), lithium aluminum titanium phosphate (LATP), and sulfide solid electrolytes or their doped and modified materials.
[0012] In any embodiment, based on the total mass of the ion transport layer, the mass content of the ion-conducting polymer is 20% to 90%, optionally 50% to 80%; or the mass content of the electrolyte salt is 10% to 50%, optionally 10% to 30%; or the mass content of the inorganic fast ion conductor is 0% to 20%, optionally 5% to 10%; or the mass content of the inorganic ceramic is 0% to 10%, optionally 5% to 10%.
[0013] In any embodiment, the ion transport layer is a composite material formed by crosslinking components comprising a first polymeric monomer, a plasticizer, and an electrolyte salt.
[0014] The cross-linking of the first polymer monomer forms a continuous phase in the composite material, providing a substrate framework with sufficient mechanical strength for the ion transport layer. The plasticizer and electrolyte salt in the composite material enhance its ionic conductivity. This composite material exhibits high ionic conductivity and low electronic conductivity, reducing the expansion rate of the negative electrode and improving the battery's cycle performance.
[0015] In any embodiment, the first polymerizing monomer is selected from one or more of ester monomers, sulfone monomers, amide monomers, nitrile monomers or ether monomers; or the plasticizer is selected from one or more of ester or sulfone monomers.
[0016] In any embodiment, the plasticizer is selected from at least one of methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0017] In any embodiment, the component further comprises one or more of a second polymerizing monomer, a thickener, and an inorganic ceramic.
[0018] In composite materials, adding a second polymerizing monomer can improve the polymerization efficiency and degree of polymerization of the first polymerizing monomer; adding a thickener can adjust the viscosity of the components and prevent the ion transport layer from penetrating into the pores inside the negative electrode active material layer, thereby reducing the performance of the negative electrode sheet; adding inorganic ceramics can further improve the strength of the ion transport layer and improve the safety and cycle performance of the battery.
[0019] In any embodiment, based on the total mass of the ion transport layer, the mass content of the first polymeric monomer is 0% to 30%, optionally 5% to 30%, or the mass content of the second polymeric monomer is 0% to 30%, optionally 5% to 20%, or the mass content of the plasticizer is 30% to 80%, optionally 40% to 70%, or the mass content of the electrolyte salt is 10% to 20%, or the mass content of the thickener is 0% to 10%, optionally 3% to 10%, or the mass content of the inorganic ceramic is 0% to 50%, optionally 0% to 20%.
[0020] In any embodiment, the component further comprises an active site initiator selected from one or more peroxide compounds or azo compounds.
[0021] In any embodiment, the inorganic ceramic is selected from one or more of alumina, boehmite, zirconium oxide, aluminum nitride, titanium dioxide, magnesium oxide, silicon carbide, calcium carbonate, and diatomaceous earth.
[0022] In any embodiment, the electrolyte salt is selected from one or more lithium salts and sodium salts.
[0023] In any embodiment, the thickener and the plasticizer are miscible, and the thickener is selected from one or more of polyvinyl alcohol formaldehyde, polyvinylidene fluoride and its copolymers, polydifluoroethylene, polyvinylidene fluoride, trichloroethylene, polytetrafluoroethylene, acrylic acid adhesive, epoxy resin, polyethylene oxide, polyacrylonitrile, sodium carboxymethyl cellulose, styrene-butadiene rubber, polymethyl methacrylate, polymethyl methacrylate, polyacrylamide, and polyvinylpyrrolidone.
[0024] A third aspect of this application provides a method for manufacturing a negative electrode sheet, the method comprising the following steps: coating an ion transport layer onto the surface of a negative electrode active material layer to obtain a negative electrode sheet, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 S / cm. The method is simple, low-cost, and easy to promote and apply.
[0025] In any embodiment, the ion transport layer comprises an ion-conducting polymer, an electrolyte salt, an inorganic fast ion conductor, and an inorganic ceramic.
[0026] The fourth aspect of this application provides a method for manufacturing a negative electrode sheet, the method comprising the following steps: in-situ synthesis of an ion transport layer on the surface of a negative electrode active material layer to obtain a negative electrode sheet, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 S / cm.
[0027] In any embodiment, the ion transport layer is a composite material formed by cross-linking the components of a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, a thickener, an inorganic ceramic, and an initiator.
[0028] This method, through in-situ synthesis, can further improve the tightness of the connection between the ion transport layer and the negative electrode active material layer, and reduce the deposition of negative electrode metal on the surface of the negative electrode active material layer.
[0029] This application provides a fifth aspect of a secondary battery, comprising a positive electrode, an electrolyte, and a negative electrode manufactured by the method of the first or second aspect of this application, or a negative electrode manufactured by the method of the third or fourth aspect of this application. This battery exhibits excellent cycle performance.
[0030] In any embodiment, the ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte is less than 1, and can be selected as 0.3 to 0.7.
[0031] A sixth aspect of this application provides a battery module, including the secondary battery of the fifth aspect of this application.
[0032] A seventh aspect of this application provides a battery pack that includes the battery module of the sixth aspect of this application.
[0033] The eighth aspect of this application provides an electrical device including at least one selected from the fifth aspect of this application, the sixth aspect of this application, or the seventh aspect of this application. Attached Figure Description
[0034] Figure 1 This is a schematic diagram of lithium ion deposition on the surface of a traditional negative electrode after cycling.
[0035] Figure 2 This is a scanning electron microscope image of lithium ions deposited on the surface of the negative electrode after cycling of a traditional negative electrode sheet.
[0036] Figure 3 This is a schematic diagram of lithium ions deposited in the negative electrode active material layer after cycling of the negative electrode sheet in this application.
[0037] Figure 4 This is a schematic diagram of a secondary battery according to one embodiment of this application.
[0038] Figure 5 yes Figure 4 An exploded view of a secondary battery according to an embodiment of this application is shown.
[0039] Figure 6 This is a schematic diagram of a battery module according to one embodiment of this application.
[0040] Figure 7 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0041] Figure 8 yes Figure 7 An exploded view of a battery pack according to one embodiment of this application is shown.
[0042] Figure 9 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0043] Explanation of reference numerals in the attached figures:
[0044] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Top cover assembly; 6 Negative electrode sheet; 61 Current collector; 62 Negative electrode active material layer; 63 Lithium metal; 64 Ion transport layer. Detailed Implementation
[0045] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the positive electrode active material, its manufacturing method, positive electrode sheet, secondary battery, battery module, battery pack, and electrical device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0046] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0048] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0049] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0050] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0051] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0052] Traditional lithium-ion batteries often employ a high CB (capacity-to-weight ratio) design, meaning the negative electrode capacity is slightly higher than the positive electrode capacity. During our research, we unexpectedly discovered that using a low CB design, where the negative electrode capacity is slightly lower than the positive electrode capacity, can improve the battery's energy density. However, when low CB electrodes are applied to battery systems containing liquid electrolytes, the expansion on the negative electrode side is significant, posing certain obstacles to the cell's structural design and application. Figure 1 As shown, the conventional negative electrode 6 includes a current collector 61 and a negative electrode active material layer 62 located on at least one surface of the current collector. A low-CB design causes excess lithium source from the positive electrode to deposit on the surface of the negative electrode active material layer 62, forming a lithium metal layer 63 and causing negative electrode expansion, as shown in the scanning electron microscope image. Figure 2 As shown. Based on the above-mentioned technical problems, this application develops a negative electrode sheet with a low expansion rate, which can significantly improve the cycle performance of the battery.
[0053] [Negative electrode plate]
[0054] Based on this, this application proposes a negative electrode sheet, comprising: a negative electrode active material layer, and an ion transport layer located on at least one surface of the negative electrode active material layer, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and ionic conductivity not less than 1×10 -4 S / cm.
[0055] In this paper, the term "electronic conductivity" is a parameter used to describe the ease with which electric charge flows in a material, and it is the inverse of resistivity.
[0056] In this document, the term "ionic conductivity" is a measure used to describe the tendency for ionic conduction to occur in a substance. In some embodiments, the ionic conductivity is the lithium-ion conductivity. In some embodiments, the ionic conductivity is the sodium-ion conductivity.
[0057] In some embodiments, the ionic conductivity of the ion transport layer is not less than 1×10⁻⁶. -3 S / cm.
[0058] In some embodiments, the ion transport layer is located on the surface of the negative electrode active material layer that is in contact with the electrolyte.
[0059] like Figure 3As shown, the negative electrode of this application solves the problem of severe cell volume expansion caused by the preferential deposition of lithium metal 63 on the negative electrode surface by setting an ion transport layer 64 on the surface of the negative electrode active material layer 62. The ion transport layer 64 makes it difficult for lithium ions to be deposited as lithium metal 63 on the surface of the negative electrode active layer 62. Lithium ions diffuse, allowing for a continuous replenishment of lithium ions inside the negative electrode active layer 62, thereby achieving the deposition of lithium metal 63 in the pores inside the electrode. The negative electrode of this application reduces the expansion rate of the electrode and improves the cycle life of the battery.
[0060] In some embodiments, the ion transport layer comprises an ion-conducting polymer and an electrolyte salt.
[0061] In this paper, the term "ionically conductive polymer" refers to conductive polymer materials in which the charge carriers are mainly positive and negative ions.
[0062] In some embodiments, the ion-conducting polymer itself does not possess ions, but can complex ionic compounds and allow dissociated ions to move directionally within them under the influence of an electric field. In some embodiments, the ion-conducting polymer refers to a polymer in which the dissociated ions diffuse through chain segment movement. Such ion-conducting polymers often require use under swelling conditions to better conduct dissociated ions.
[0063] In this article, the term "electrolyte salt" refers to a salt that can be used as a liquid electrolyte in a battery.
[0064] In some embodiments, the electrolyte salt may be one or more of lithium salts and sodium salts, and may be selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorophosphate, lithium difluorodioxalate phosphate, lithium tetrafluorooxalate phosphate, NaPF6, NaClO4, NaBCl4, NaSO3CF3, and Na(CH3)C6H4SO3.
[0065] Using ion-conducting polymers and electrolyte salts to form an ion transport layer can reduce the expansion rate of the negative electrode and improve the cycle life of the battery.
[0066] In some embodiments, the ion transport layer further comprises at least one of an inorganic fast ion conductor and an inorganic ceramic.
[0067] In this paper, the term "inorganic fast ion conductor" refers to inorganic compounds that act as fast ion conductors, also known as solid electrolytes. It possesses ionic conductivity (1 × 10⁻⁶) comparable to that of liquid electrolytes within a certain temperature range. -6 S·cm -1 It has low ionic conductivity activation energy (≤0.40eV).
[0068] In this article, the term "inorganic ceramics" refers to a class of inorganic non-metallic materials made from natural or synthetic compounds through shaping and high-temperature sintering. It possesses advantages such as high melting point, high hardness, high wear resistance, and oxidation resistance.
[0069] The addition of inorganic fast ion conductors can further improve the ionic conductivity of the ion transport layer. The addition of inorganic ceramics can improve the strength of the ion transport layer, thereby further reducing the expansion rate of the negative electrode and improving the cycle performance of the battery cell.
[0070] In some embodiments, the ion-conducting polymer is selected from one or more of polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinyl alcohol (PVA), and polymethacrylate (PMA).
[0071] In some embodiments, the inorganic fast ion conductor is selected from one or more of garnet-type lithium lanthanum zirconium oxide (LLZO), perovskite-structured lithium lanthanum titanium oxide (LLTO), lithium aluminum titanium phosphate (LATP), and sulfide solid electrolytes or their doped and modified materials.
[0072] In this paper, the term "garnet-type lithium lanthanum zirconium oxide" refers to the general formula Li7La3Zr2O. 12 Compounds.
[0073] In this paper, the term "perovskite-structured lithium lanthanum titanium oxide" refers to lithium lanthanum titanium oxide with the general formula Li 3x La 0.67-x Compounds of TiO3.
[0074] In some embodiments, the mass content of the ion-conducting polymer is 20% to 90%, optionally 50% to 80%, based on the total mass of the ion transport layer. In some embodiments, the upper or lower limit of the mass content of the ion-conducting polymer can be selected from any one of 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, and 75%.
[0075] In some embodiments, the mass content of the electrolyte salt is 10% to 50%, optionally 10% to 30%, based on the total mass of the ion transport layer. In some embodiments, the upper or lower limit of the mass content of the electrolyte salt can be selected from 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, and 50%.
[0076] In some embodiments, based on the total mass of the ion transport layer, the mass content of the inorganic fast ion conductor is 0% to 20%, optionally 5% to 10%.
[0077] In some embodiments, the mass content of inorganic ceramics is 0% to 10% based on the total mass of the ion transport layer, and can be optionally 5% to 10%.
[0078] In some embodiments, the composite material is formed by crosslinking components comprising a first polymeric monomer, a plasticizer, and an electrolyte salt. In some embodiments, the first polymeric monomer refers to a monomer that constitutes a structural unit of the continuous phase of the composite material. The first polymeric monomer crosslinks to form the skeleton of the composite material, and the plasticizer and electrolyte salt are present in the crosslinked network for ion transport.
[0079] In this article, the term "plasticizer" refers to a substance added to a polymer material that increases the plasticity of the polymer.
[0080] The composite material forms a continuous phase through cross-linking of monomers, providing a robust framework with sufficient mechanical strength for the ion transport layer. Plasticizers and electrolyte salts in the composite material enhance its ionic conductivity. This composite material exhibits high ionic conductivity and low electronic conductivity, reducing the expansion rate of the negative electrode and improving the battery's cycle performance.
[0081] In some embodiments, the polymerization monomer is selected from one or more of ester monomers, sulfone monomers, amide monomers, nitrile monomers or ether monomers.
[0082] In this article, the term "ester monomer" refers to a monomer containing an ester group.
[0083] In this article, the term "sulfone monomer" refers to monomers containing a sulfone group.
[0084] In this article, the term "amide monomer" refers to a monomer containing an amide group.
[0085] In this article, the term "nitrile monomer" refers to monomers containing a cyano group.
[0086] In this article, the term "ether monomer" refers to a monomer containing an ether group.
[0087] In some embodiments, the ester monomers include carbonate monomers, sulfate monomers, sulfonate monomers, phosphate monomers, and carboxylic acid ester monomers. In some embodiments, the carbonate monomers are selected from one or more of vinylene carbonate, ethylene carbonate, ethylene carbonate, propylene carbonate, butene carbonate, fluoroethylene carbonate, and chloroethylene carbonate. In some embodiments, the sulfate monomers are selected from one or more of vinyl vinyl sulfite, vinyl sulfite, 4-methylvinyl sulfate, and 4-ethylvinyl sulfate. In some embodiments, the sulfonate monomers are selected from one or more of 1,3-propenesulfonate lactone, 1,3-propanesulfonate lactone, 1,4-butanesulfonate lactone, and methanedisulfonate methylenecyclohexylene. In some embodiments, the phosphate ester monomers are selected from one or more of dimethyl vinyl phosphate, diethyl vinyl phosphate, diethylpropenyl phosphate, diethylbutenyl phosphate, diethyl-1-buten-2-ylphosphonate, diethylethynyl phosphate, vinyltrifluoromethyl phosphate, vinyl-1-trifluoroethyl phosphate, diethylfluorovinyl phosphate, and 1-trifluoropropenylethyl phosphate. In some embodiments, the carboxylic acid ester monomers are selected from vinyl acetate.
[0088] In some embodiments, the sulfone monomer is selected from one or more of methyl vinyl sulfone, ethyl vinyl sulfone, cyclobutene sulfone, cyclobutene sulfone, and cycloethylene sulfoxide.
[0089] In some embodiments, the amide monomer is selected from acrylamide.
[0090] In some embodiments, the nitrile monomer is selected from one or more of acrylonitrile, succinic anhydride, glutaronitrile, and adiponitrile.
[0091] In some embodiments, the ether monomer includes one or more selected from 1,3-dioxopentane, ethylene oxide, 1,2-epoxypropane, 4-methyl-1,3-dioxopentane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, ethylene glycol diglycidyl ether, and triethylene glycol divinyl ether.
[0092] In some embodiments, the polymerizing monomer is selected from one or more of vinylene carbonate, vinyl sulfite, ethylene carbonate, 1,3-propenyl sulfonate lactone, methyl vinyl sulfone, ethyl vinyl sulfone, methyl methacrylate, vinyl acetate, and acrylamide.
[0093] In some embodiments, the plasticizer is selected from one or more ester or sulfone monomers.
[0094] In some embodiments, the plasticizer is selected from one or more of methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0095] In some embodiments, the crosslinking polymerization is initiated by electron beam initiation, ultraviolet light initiation, or initiator initiation.
[0096] In some embodiments, the components also include one or more of a second polymeric monomer thickener and inorganic ceramics.
[0097] In some embodiments, the composite material is formed by crosslinking of components including a first polymeric monomer, a plasticizer, an electrolyte salt, and a thickener.
[0098] In some embodiments, the composite material is formed by crosslinking components comprising a first polymeric monomer, a plasticizer, an electrolyte salt, and an inorganic ceramic.
[0099] In some embodiments, the composite material is formed by crosslinking components comprising a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, and a thickener.
[0100] In some embodiments, the composite material is formed by crosslinking components comprising a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, and an inorganic ceramic.
[0101] In some embodiments, the composite material is formed by crosslinking components comprising a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, a thickener, and an inorganic ceramic.
[0102] In this article, the term "thickener" refers to a substance that increases the viscosity of a system, keeps the system in a uniform and stable suspended or emulsified state, or forms a gel.
[0103] In some embodiments, the components forming the composite material also include a second polymeric monomer, which can improve the crosslinking efficiency, crosslinking degree and strength of the composite material, thereby optimizing the path of plasticizer and electrolyte salt diffusion and transport of ions in the crosslinked network, and further improving the ionic conductivity of the ion transport layer.
[0104] In some embodiments, the second polymerizing monomer is selected from one or more acrylic or acrylate monomers.
[0105] In some embodiments, the second polymerizing monomer is selected from acrylic acid, methacrylic acid, methyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, isodecanyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, isobornyl methacrylate, ethoxyethoxyethyl acrylate, cyanoacrylate, caprolactone acrylate, 2-phenoxyethyl acrylate, tetrahydrofuran acrylate, ethoxytetrahydrofuran acrylate, cyclotrimethylolpropane acrylate, 2-carboxyethyl acrylate, cyclohexyl acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,3- Butylene glycol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 2-(propylene oxide) neopentyl glycol diacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate One or more of the following: acrylate, polycyclohexyl acrylate, methoxy polyethylene glycol acrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, methoxy polyethylene glycol methacrylate, pentaerythritol triacrylate, propoxylated glycerol triacrylate, tri(2-hydroxyethyl)isocyanurate triacrylate, di(trimethylolpropane)tetraacrylate, pentaerythritol tetraacrylate, 4(ethoxy)pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.
[0106] In composite materials, adding a second monomer can improve the polymerization efficiency and degree of polymerization of the first monomer. Adding a thickener can adjust the viscosity of the components, preventing the ion transport layer from penetrating into the pores inside the negative electrode active material layer, thus reducing the performance of the negative electrode and contributing to further improvement in battery cycle performance. Adding inorganic ceramics to composite materials can further enhance the strength of the ion transport layer, contributing to further improvement in battery safety and cycle performance.
[0107] In some embodiments, based on the total mass of the ion transport layer, the mass content of the first polymeric monomer is 0%–30%, optionally 5%–30%; the mass content of the second polymeric monomer is 0%–30%, optionally 5%–20%; the mass content of the plasticizer is 30%–80%, optionally 40%–70%; the mass content of the electrolyte salt is 10%–20%; the mass content of the thickener is 0%–10%, optionally 3%–10%; or the mass content of the inorganic ceramic is 0%–50%, optionally 0%–20%. In some embodiments, the upper or lower limit of the mass content of the polymeric monomer can be selected as 5%, 10%, 15%, 20%, 25%, and 30%, based on the total mass of the ion transport layer. In some embodiments, the lower or upper limit of the mass content of the second polymeric monomer can be selected as 5%, 10%, 15%, 20%, 25%, or 30%, based on the total mass of the ion transport layer. In some embodiments, the upper or lower limit of the mass content of the plasticizer can be selected as 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%, based on the total mass of the ion transport layer. In some embodiments, the lower or upper limit of the mass content of the electrolyte salt can be selected as 10%, 15%, or 20%, based on the total mass of the ion transport layer. In some embodiments, the lower or upper limit of the mass content of the thickener can be selected as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, based on the total mass of the ion transport layer. In some embodiments, the lower or upper limit of the mass content of the inorganic ceramic can be selected as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50%, based on the total mass of the ion transport layer.
[0108] In some embodiments, the component further comprises an active site initiator selected from one or more peroxide compounds or azo compounds. In some embodiments, the peroxide compounds include, but are not limited to, acyl peroxides such as benzoyl peroxide and lauroyl peroxide, and persulfates such as ammonium persulfate; the azo initiators include, but are not limited to, azobisisobutyronitrile and azobisisoheptanenitrile. In some embodiments, the active site initiator is thermally initiated, with the thermal initiation temperature selected from 50°C to 85°C.
[0109] In some embodiments, the inorganic ceramic is selected from one or more of alumina, boehmite, zirconium oxide, aluminum nitride, titanium dioxide, magnesium oxide, silicon carbide, calcium carbonate, and diatomaceous earth.
[0110] In some embodiments, the electrolyte salt is selected from one or more lithium salts and sodium salts.
[0111] In some embodiments, the thickener and plasticizer are miscible. The thickener is selected from one or more of polyvinyl alcohol formaldehyde, polyvinylidene fluoride and its copolymers, polyvinyl difluoride, polyvinylidene fluoride, trichloroethylene, polytetrafluoroethylene, acrylic acid adhesive, epoxy resin, polyethylene oxide, polyacrylonitrile, sodium carboxymethyl cellulose, styrene-butadiene rubber, polymethyl methacrylate, polymethyl methacrylate, polyacrylamide, and polyvinylpyrrolidone. By selecting a thickener miscible with the plasticizer, the thickening effect of the thickener can be further enhanced.
[0112] This application provides a method for manufacturing a negative electrode sheet, the method comprising the following steps: coating an ion transport layer onto the surface of a negative electrode active material layer to obtain a negative electrode sheet, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. - 7 S / cm, and lithium-ion conductivity not less than 1×10 -4 S / cm.
[0113] It is understandable that coating can be performed in any way, such as spraying, adhesive coating, gravure coating, etc. This method is simple, low-cost, and easy to promote and apply.
[0114] In some embodiments, the ion transport layer comprises an ion-conducting polymer, an electrolyte salt, an inorganic fast ion conductor, and an inorganic ceramic.
[0115] This application provides a method for manufacturing a negative electrode sheet, the method comprising the following steps: in-situ synthesis of an ion transport layer on the surface of a negative electrode active material layer to obtain a negative electrode sheet, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 S / cm.
[0116] It can be understood that in-situ synthesis refers to the process of setting the material on the surface of the negative electrode active material layer and then in-situ initiating polymerization to synthesize the ion transport layer on the surface of the negative electrode active material layer.
[0117] In some embodiments, the ion transport layer is a composite material formed by cross-linking the components of a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, a thickener, an inorganic ceramic, and an initiator.
[0118] This method, through in-situ synthesis, can further improve the tightness of the connection between the ion transport layer and the negative electrode active material layer, and reduce the deposition of negative electrode metal on the surface of the negative electrode active material layer.
[0119] In some embodiments, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0120] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0121] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0122] In some embodiments, the negative electrode active material layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0123] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0124] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0125] [Positive electrode plate]
[0126] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, the positive electrode film layer including the positive electrode active material of the first aspect of this application.
[0127] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0128] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0129] In some embodiments, the positive electrode active material may be a known battery positive electrode active material. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.15 Al0.05 At least one of O2 and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0130] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0131] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0132] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0133] [Electrolytes]
[0134] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0135] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0136] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0137] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0138] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0139] [Isolation membrane]
[0140] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0141] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0142] [Rechargeable Battery]
[0143] This application provides a secondary battery, including a positive electrode, an electrolyte, and a negative electrode manufactured by a method for manufacturing a negative electrode as described in any embodiment.
[0144] In some embodiments, the ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte is less than 1, and can be selected as 0.3 to 0.7. In some embodiments, the upper or lower limit of the ratio of the lithium-ion conductivity of the ion transport layer to the lithium-ion conductivity of the electrolyte can be selected from 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9.
[0145] During charging, lithium ions are extracted from the positive electrode active material and embedded in the negative electrode active material. Once the negative electrode is fully embedded, the lithium ions gain electrons and are deposited as lithium metal. Due to the high specific surface area inside the negative electrode active material layer, the lithium ions inside the negative electrode are rapidly consumed, resulting in a temporary lithium ion shortage. When more lithium ions diffuse from the positive electrode to the negative electrode, they directly gain electrons on the negative electrode surface and are converted into a metallic state, causing almost all the lithium metal to be deposited on the negative electrode surface.
[0146] When an ion transport layer covers the surface of the negative electrode, and the ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte is less than 1 (i.e., the lithium-ion conductivity of the ion transport layer is lower than that of the electrolyte), this difference in conductivity reduces the lithium-ion conduction speed on the electrode surface. This provides a time difference for lithium-ion diffusion within the active material layer of the electrolyte, making it easier for lithium ions to deposit inside the negative electrode and less likely to deposit as lithium metal on the surface of the active layer. This reduces the battery's expansion rate and improves its cycle performance.
[0147] The ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte can be selected as 0.3 to 0.7, which can ensure a suitable time difference for lithium-ion diffusion inside the electrode, further reduce the battery expansion rate, and improve the battery cycle performance.
[0148] In some implementations, the CB value of the battery is less than 1.
[0149] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0150] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 4 This is an example of a square-structured secondary battery 5.
[0151] In some implementations, refer to Figure 5The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 using a winding or stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0152] [Battery Module]
[0153] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0154] Figure 6 This is battery module 4, used as an example. (See reference...) Figure 6 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0155] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0156] [Battery Pack]
[0157] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0158] Figure 7 and Figure 8 This is battery pack 1 as an example. (See reference...) Figure 7 and Figure 8 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0159] [Electrical appliances]
[0160] In one embodiment of this application, an electrical device is provided, including the battery in any of the embodiments.
[0161] The electrical device includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0162] As the electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.
[0163] Figure 9 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0164] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.
[0165] Example
[0166] Example 1
[0167] 1) Preparation of negative electrode sheet
[0168] Preparation of the negative electrode active material layer: Graphite, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 94:3:3. The mixture was then coated onto the surface of copper foil with a coating amount of 1.40 mA·h / cm². 2 This makes CB = 0.4, and after drying and cold pressing, the negative electrode active material layer is obtained.
[0169] Preparation of the ion transport layer: Polymethyl methacrylate (PMMA), LiFSI, LLZO, and alumina were thoroughly mixed in an NMP solvent system at a weight ratio of 6:2:1:1 to prepare a slurry. The slurry was then coated onto the surface of the prepared negative electrode active material layer to a thickness of 10 μm. After coating, the material was dried in a vacuum oven at 80 °C for 12 h to obtain the negative electrode sheet. The electrode sheet was then cut to the appropriate size for later use.
[0170] 2) Preparation of positive electrode sheet
[0171] NCM811 was thoroughly mixed with conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) in an N-methylpyrrolidone solvent system at a weight ratio of 94:3:3. The mixture was then coated onto aluminum foil, dried, and cold-pressed to obtain the positive electrode sheet with a coating weight of 3.5 mAh / cm². 2 Cut them to the appropriate size for later use.
[0172] 3) Separating membrane
[0173] Polyethylene film (PE diaphragm) is used as the separation membrane.
[0174] 4) Preparation of electrolyte
[0175] The electrolyte solvent is EC∶EMC∶DMC=1∶1∶1, and the lithium salt is LiFSI with a concentration of 1M / L.
[0176] 5) Battery manufacturing
[0177] Assemble laminated cells using double-sided positive electrodes, separators, and single-sided negative electrodes. Assemble bare cells in the order of negative electrode, separator, positive electrode, separator, negative electrode, ensuring the separator acts as an isolation layer between the positive and negative electrodes. Place the bare cells in outer packaging to obtain dry cells. Inject 0.3g of electrolyte into each cell, vacuum seal after injection, and allow to stand and soak.
[0178] In Comparative Examples 1-3, no ion transport layer was coated on the negative electrode sheet; other preparation methods were the same.
[0179] Example 1: Adjust the coating amount of the negative electrode active material layer according to the designed CB value.
[0180] In Comparative Example 1, when the CB value is 0.7, the coating amount of the negative electrode active material layer is 2.45 mA·h / cm. 2 In Comparative Example 2, when the CB value is 0.4, the coating amount of the negative electrode active material layer is 1.40 mA·h / cm. 2 In Comparative Example 3, when the CB value is 1, the coating amount of the negative electrode active material layer is 3.5 mAh / cm². 2 .
[0181] The negative electrode sheet of Comparative Example 4 was formed in the same way as in Example 1, except that the ion transport layer contained only PMMA polymer.
[0182] The secondary batteries of Examples 2-14 and Comparative Examples 1-4 are prepared in a similar manner to the secondary battery of Example 1, but the composition of the negative electrode and the product parameters are adjusted. The different product parameters are detailed in Table 1.
[0183] The relevant parameters of the cathode materials of Examples 1 to 14 and Comparative Examples 1 to 4 are shown in Table 1 below.
[0184] The secondary batteries in Examples 15-28 are prepared using methods similar to those in Example 1, but the composition and preparation method of the negative electrode sheet are adjusted. Taking Example 15 as an example, the preparation method of its negative electrode sheet is as follows:
[0185] Example 15
[0186] Preparation of negative electrode sheet:
[0187] Preparation of the negative electrode active material layer: Graphite, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 94:3:3. The mixture was then coated onto the surface of copper foil with a coating amount of 2.45 mAh / cm². 2 This results in CB=0.7. After drying and cold pressing, the negative electrode active material layer is obtained.
[0188] Preparation of the ion transport layer: A slurry was prepared by thoroughly mixing the first monomer vinylene carbonate (VC), the second monomer polyethylene glycol diacrylate (PEGDA), a mixture of plasticizers ethyl methyl carbonate and ethylene carbonate (EMC+EC), a thickener PVDF, an electrolyte salt LiFSI, and inorganic ceramic alumina in a weight ratio of 20:5:40:5:20:10. The slurry was then coated onto the surface of the prepared negative electrode active material layer to a thickness of 5 μm. The thickener PVDF is soluble in the plasticizer to provide thickening. Before coating, a UV initiator, diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide (TPO), was added to the slurry. After coating, the ion transport layer was exposed to a 365 nm UV light source at a power of 2 W / cm². 2 Irradiation under certain conditions for 1 minute causes the slurry to solidify and form a composite material, resulting in a negative electrode sheet. The electrode sheet is then cut to the appropriate size for later use.
[0189] The secondary batteries in Examples 15-28 are prepared in a similar manner to the secondary battery in Example 15, but the composition of the negative electrode and the product parameters are adjusted. The different product parameters are detailed in Table 2.
[0190] In Comparative Example 5, the steps for preparing the ion transport layer involved thoroughly mixing the polymeric monomer vinylene carbonate (VC), the second polymeric monomer polyethylene glycol diacrylate (PEGDA), and a mixture of plasticizers ethyl methyl carbonate and ethylene carbonate (EMC+EC) at a weight ratio of 20:5:75 to prepare a slurry, thus preparing the ion transport layer. Other steps were the same as in Example 15.
[0191]
[0192]
[0193] II. Performance Testing
[0194] The performance test data for Examples 1-14 and Comparative Examples 1, 2, and 4 are shown in Table 3. The performance test data for Examples 15-28 and Comparative Examples 1, 2, and 5 are shown in Table 4. The performance test methods are as follows:
[0195] 1. Calculation of CB value
[0196] A battery is assembled using coated positive and negative electrode sheets. The CB value of the battery is obtained by dividing the areal capacity of the negative electrode sheet by the areal capacity of the positive electrode sheet, i.e., CB = negative electrode areal capacity / positive electrode areal capacity.
[0197] 2. Lithium-ion conductivity test
[0198] The coating is applied to the surface of a blank aluminum foil and cut into small circular pieces with a diameter of 20 mm. A coin cell is assembled in the following order: positive electrode shell, small circular piece (coated side up), gasket, spring contact, and negative electrode shell. Electrochemical impedance spectroscopy (EIS) is used on a Solartron 1470E CellTest multichannel electrochemical workstation to test the Nyquist plot. The Nyquist plot is then analyzed using the equivalent circuit curve fitting method. The x-coordinate of the intersection of the semicircle and the oblique line in the Nyquist plot is taken as the resistance R. The test voltage can be 10 mV, and the test frequency can be 0.1 Hz to 100 kHz.
[0199] The ionic conductivity λ1 of the coating is calculated using the formula λ=d / RS, where λ represents ionic conductivity, d represents coating thickness, R represents resistance, and S represents coating area.
[0200] The ionic conductivity of the electrolyte was directly measured using a conductivity meter to obtain λ2.
[0201] 3. Electronic conductivity test
[0202] The coating was applied to the surface of a blank aluminum foil and cut into small circular pieces with a diameter of 20 mm. The coin cell was assembled in the following order: positive electrode shell, small circular piece (coated side up), gasket, spring, and negative electrode shell. The test was conducted using the constant potential mode of the Solartron 1470E CellTest multichannel electrochemical workstation. The voltage U was set to 1 V and the time was set to 2 h. The stable current in the final stage was recorded as I. The formula λe = dI / SU was used, where d represents the thickness of the coating, S represents the area of the coating, and I and U are the program settings.
[0203] 4. Expansion Rate Test
[0204] Before cell assembly, the thickness L0 of the negative electrode sheet was measured. At an ambient temperature of 25°C, the battery was allowed to stand for 5 minutes, then charged at 1 / 3C to 4.25V. It was then charged at 4.25V under constant voltage until the current ≤0.05mA. After standing for 5 minutes, it was discharged at 1 / 3C to 2.8V. After standing for 5 minutes, it was charged at 1 / 3C to 4.25V. It was then charged at 4.25V under constant voltage until the current ≤0.05mA. The battery was then disassembled, and the thickness L1 of the negative electrode sheet was recorded. The expansion rate α = (L1 - L0) / L1 was calculated.
[0205] 5. Measurement of cell polarization voltage
[0206] At an ambient temperature of 25°C, the battery was left to stand for 5 minutes, then charged at 1 / 3C (46mA) to 4.25V. It was then charged at a constant voltage of 4.25V until the current ≤0.05mA. The average charging voltage was calculated by dividing the charging energy by the charging capacity. After leaving the battery to stand for 5 minutes, it was discharged at 1 / 3C to 2.8V. The average discharging voltage was calculated by dividing the discharging energy by the discharging capacity. The polarization voltage of the battery was obtained by subtracting the discharging voltage from the average charging voltage. This embodiment uses data from the second cycle to calculate the polarization voltage.
[0207] 6. Energy density test
[0208] The processed negative electrode sheet, positive electrode sheet, and separator are assembled into a large soft-pack battery by winding. The electrolyte is injected according to the electrolyte injection coefficient of 2g / Ah, and charged to 4.25V at a constant current of 0.33C. After standing for 5 minutes, it is discharged to 2.8V at a constant current of 0.33C. The discharge energy Q during the discharge stage is read, and the cell mass m is weighed using a balance. The energy density is Q / m.
[0209] 7. Cycle life
[0210] After letting the pouch battery rest for 5 minutes, charge it to 4.25V at a constant current of 0.33C (46mA), then charge it to 4.25V at a constant voltage of 4.25V until the current is less than 0.05C (7mA). After letting it rest for 5 minutes, discharge it to 2.8V at a constant current of 0.33C to obtain the first cycle discharge capacity C0 of the battery. Repeat the above cycle until Cn is less than or equal to C0. The number of cycles is recorded as the cycle life.
[0211] 8. First week discharge capacity test
[0212] After the soft-pack battery is left to stand for 5 minutes, it is charged at a constant current of 0.33C (46mA) to 4.25V, and then charged at a constant voltage of 4.25V until the current is less than 0.05C to obtain the first week's charging capacity of the battery; after being left to stand for 5 minutes, it is discharged at a constant current of 0.33C to 2.8V to obtain the first week's discharging capacity of the battery.
[0213]
[0214]
[0215] Batteries for each embodiment and comparative example were prepared according to the above method, and various performance parameters were measured. The results are shown in Tables 3 and 4.
[0216] In Comparative Example 3, when the CB value of the battery is 1, the energy density of the battery is 302 Wh / kg. For the comparative examples and embodiments with a CB value of 0.7, the energy density of the battery is 333 Wh / kg. For the comparative examples and embodiments with a CB value of 0.4, the energy density of the battery is further increased to 369 Wh / kg. It can be seen that the design of a low CB value is beneficial to improving the energy density of the battery.
[0217] The negative electrode sheet in Examples 1-28 includes a negative electrode active material layer and an ion transport layer located on the surface of the negative electrode active material layer in contact with the electrolyte. The electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and ionic conductivity not less than 1×10 -4 S / cm. From the comparison of Examples 1-14 with Comparative Examples 1, 2, and 4, and the comparison of Examples 15-28 with Comparative Examples 1, 2, and 5, it can be seen that this negative electrode sheet, by setting an ion transport layer on the surface where the negative electrode active material layer contacts the electrolyte, reduces the expansion rate of the negative electrode sheet and improves the cycle life of the battery. When the ionic conductivity is not less than 1×10⁻⁶... - 3 At a value of S / cm, the expansion rate of the negative electrode sheet decreases more significantly, and the cycle life of the battery improves more dramatically. In Examples 1-14, compared to Comparative Example 4, the ionic conductivity of the ion transport layer is not less than 1×10⁻⁶. -4 S / cm enables the battery to maintain a high first-cycle discharge capacity while improving cycle life.
[0218] In Examples 9 and 10, the ion transport layer contains only ion-conducting polymer and electrolyte salt. Compared with Comparative Example 1, this negative electrode sheet reduces the expansion rate of the negative electrode sheet and improves the cycle life of the battery.
[0219] In Examples 1-8 and 11-13, the ion transport layer, in addition to the ion-conducting polymer and electrolyte salt, also contains at least one of an inorganic fast ion conductor and an inorganic ceramic. Compared with Comparative Examples 1, 2, and 4, this negative electrode sheet reduces the expansion rate of the negative electrode sheet and improves the cycle life of the battery. Compared with Example 10, Examples 11 and 12 further improve the cycle life of the battery by adding an inorganic fast ion conductor or an inorganic ceramic.
[0220] The negative electrode sheet in Examples 15-28 includes a negative electrode active material layer and an ion transport layer located on at least one surface of the negative electrode active material layer, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 The ion transport layer has a conductivity of S / cm and is a composite material formed by cross-linking components including a first polymeric monomer, a second polymeric monomer, a plasticizer, and an electrolyte salt. Compared to Comparative Examples 1, 2, and 5, this negative electrode sheet reduces the expansion rate of the negative electrode sheet and improves the cycle life of the battery. In Examples 15-28, compared to Comparative Example 5, the ionic conductivity of the ion transport layer is higher than 1×10⁻⁶. -3 S / cm enables the battery to maintain a high first-cycle discharge capacity while improving cycle life.
[0221] The negative electrode sheets in Examples 18-22 and 26-28 include a negative electrode active material layer and an ion transport layer located on at least one surface of the negative electrode active material layer, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 The ion transport layer, with a density of S / cm, is a composite material formed by cross-linking components including a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, and a thickener. Compared to Comparative Examples 1, 2, and 5, this negative electrode sheet exhibits reduced expansion rate and improved battery cycle life. Compared to Example 24, the addition of the thickener prevents the negative electrode active material layer from seeping down during coating, further enhancing battery cycle performance.
[0222] The negative electrode sheets in Examples 15-17, 23, and 25 include a negative electrode active material layer and an ion transport layer located on at least one surface of the negative electrode active material layer, wherein the electronic conductivity of the ion transport layer is not higher than 1×10⁻⁶. -7 S / cm, and lithium-ion conductivity not less than 1×10 -4 S / cm, the ion transport layer is a composite material, which is formed by cross-linking of components including a first polymeric monomer, a second polymeric monomer, a plasticizer, an electrolyte salt, a thickener, and inorganic ceramics. Compared with Comparative Examples 1, 2, and 5, this negative electrode sheet reduces the expansion rate of the negative electrode sheet and improves the cycle life of the battery. Compared with Example 20, the addition of inorganic ceramics in Example 25 further improves the cycle life of the battery.
[0223] In the negative electrode sheets of Examples 1-28, the ratio of lithium-ion conductivity of the ion transport layer to lithium-ion conductivity of the electrolyte is less than 1. This negative electrode sheet reduces the expansion rate and improves the cycle life of the battery. When the ratio of lithium-ion conductivity of the ion transport layer to lithium-ion conductivity of the electrolyte is 0.3-0.7, the expansion rate of the negative electrode sheet decreases further, and the cycle life is further improved.
[0224] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A secondary battery, characterized in that, It includes a positive electrode, an electrolyte, and a negative electrode; wherein, the negative electrode includes: current collector, A layer of negative electrode active material located on at least one surface of the current collector, and An ion transport layer located on the surface of the negative electrode active material layer away from the current collector. The electronic conductivity of the ion transport layer is no higher than 1×10⁻⁶. -7 S / cm, and ionic conductivity not less than 1×10 -4 S / cm; The ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte is less than 1. The ion transport layer enables lithium ions to extend into the interior of the negative electrode active material layer, thereby achieving the deposition of lithium metal in the pores inside the negative electrode active material layer. The CB value of the secondary battery is less than 1.
2. The secondary battery according to claim 1, characterized in that, The ion transport layer comprises an ion-conducting polymer and an electrolyte salt.
3. The secondary battery according to claim 2, characterized in that, The ion transport layer also includes at least one of inorganic fast ion conductors and inorganic ceramics.
4. The secondary battery according to claim 2 or 3, characterized in that, The ion-conducting polymer is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinyl alcohol, and polymethacrylate.
5. The secondary battery according to claim 3, characterized in that, The inorganic fast ion conductor is selected from one or more of the following: garnet-type lithium lanthanum zirconium oxide (LLZO), perovskite-structured lithium lanthanum titanium oxide (LLTO), lithium aluminum titanium phosphate (LATP), and sulfide solid electrolytes or their doped and modified materials.
6. The secondary battery according to claim 3, characterized in that, Based on the total mass of the ion transport layer, the mass content of the ion-conducting polymer is 20%~90%; or The electrolyte salt has a mass content of 10% to 50%; or The inorganic fast ion conductor has a mass content of 0%~20%; or The inorganic ceramic has a mass content of 0% to 10%.
7. The secondary battery according to claim 6, characterized in that, Based on the total mass of the ion transport layer, the mass content of the ion-conducting polymer is 50%~80%; or The electrolyte salt has a mass content of 10% to 30%; or The inorganic fast ion conductor has a mass content of 5% to 10%; or The inorganic ceramic content is 5% to 10% by mass.
8. The secondary battery according to claim 1, characterized in that, The ion transport layer is a composite material formed by cross-linking components including a first polymer monomer, a plasticizer, and an electrolyte salt.
9. The secondary battery according to claim 8, characterized in that, The first polymerization monomer is selected from one or more of ester monomers, sulfone monomers, amide monomers, nitrile monomers or ether monomers.
10. The secondary battery according to claim 9, characterized in that, The plasticizer is selected from at least one of methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
11. The secondary battery according to claim 8, characterized in that, The components also include one or more of a second polymerizing monomer, a thickener, and an inorganic ceramic.
12. The secondary battery according to claim 11, characterized in that, Based on the total mass of the ion transport layer, the mass content of the first polymeric monomer is 0%~30%, or The mass content of the second polymerizable monomer is 0%~30%, or The plasticizer has a mass content of 30% to 80%, or The electrolyte salt has a mass content of 10% to 20%, or The thickener has a mass content of 0% to 10%, or The inorganic ceramic has a mass content of 0% to 50%.
13. The secondary battery according to claim 12, characterized in that, Based on the total mass of the ion transport layer, the mass content of the first polymeric monomer is 5%~30%, or The mass content of the second polymerizing monomer is 5%~20%, or The plasticizer has a mass content of 40% to 70%, or The thickener has a mass content of 3% to 10%, or The inorganic ceramic has a mass content of 0% to 20%.
14. The secondary battery according to claim 8, characterized in that, The component also includes an active site initiator, which is selected from one or more peroxide compounds or azo compounds.
15. The secondary battery according to claim 3, characterized in that, The inorganic ceramic is selected from one or more of alumina, boehmite, zirconium oxide, aluminum nitride, titanium dioxide, magnesium oxide, and silicon carbide.
16. The secondary battery according to claim 2, characterized in that, The electrolyte salt is selected from one or more lithium salts and sodium salts.
17. The secondary battery according to claim 11, characterized in that, The thickener and the plasticizer are miscible, and the thickener is selected from one or more of polyvinyl alcohol formaldehyde, polyvinylidene fluoride and its copolymers, polytetrafluoroethylene, acrylic acid glue, epoxy resin, polyethylene oxide, polyacrylonitrile, sodium carboxymethyl cellulose, styrene-butadiene rubber, polymethyl acrylate, polymethyl methacrylate, polyacrylamide, and polyvinylpyrrolidone.
18. The secondary battery according to claim 1, characterized in that, The method for manufacturing the negative electrode sheet includes the following steps: The slurry of the ion transport layer is coated onto the surface of the negative electrode active material layer to obtain the negative electrode sheet.
19. The secondary battery according to claim 1, characterized in that, The method for manufacturing the negative electrode sheet includes the following steps: The negative electrode sheet is obtained by in-situ polymerization to synthesize the ion transport layer on the surface of the negative electrode active material layer.
20. The secondary battery according to claim 1, characterized in that, The ratio of the lithium-ion conductivity λ1 of the ion transport layer to the lithium-ion conductivity λ2 of the electrolyte is 0.3 to 0.
7.
21. A battery module, characterized in that, The secondary battery includes any one of claims 1-20.
22. A battery pack, characterized in that, Includes the battery module as described in claim 21.
23. An electrical appliance, characterized in that, It includes at least one selected from the secondary battery of any one of claims 1-20, the battery module of claim 21, or the battery pack of claim 22.
Citation Information
Patent Citations
Positive electrode plate, negative electrode plate and high-rate rapid-charge lithium ion battery
CN110061188A
Functional coating, electrode plate and electrochemical device
CN112038644A
Electrode and electrochemical element
CN113380981A