A heteropoly acid-porous MOFs composite material, a preparation method thereof and an oil product treatment method

The solvothermal synthesis of heteropolyacid-hierarchical porous MOFs composites solved the problem of low denitrification and desulfurization efficiency in diesel fuel, achieving high-efficiency denitrification and desulfurization under mild conditions. Furthermore, the materials are easy to regenerate and are suitable for oil processing.

CN117942945BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211339207.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2026-11-20
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve efficient denitrification and desulfurization of diesel fuel under mild conditions. Furthermore, deep hydrodenitrification technology consumes a large amount of hydrogen and requires significant equipment investment, while oxidative desulfurization has a substantial impact on the octane number of oil products.

Method used

A heteropolyacid-hierarchical porous MOFs composite material is used. The heteropolyacid is combined with the hierarchical porous MOFs by a solvothermal synthesis method to form a composite with microporous and mesoporous structures. The heteropolyacid is distributed in the pores, and the electron confinement effect is used to achieve synergistic denitrification and desulfurization.

Benefits of technology

It achieves efficient denitrification and desulfurization of fuel under mild conditions. The composite material is easy to recycle and maintains good adsorption denitrification and oxidative desulfurization effects, significantly improving the efficiency of removing aromatic sulfur-containing compounds and nitrogen-containing compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117942945B_ABST
    Figure CN117942945B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of heteropoly acid-multistage hole MOFs composite material and preparation method, oil processing method, heteropoly acid-multistage hole MOFs composite material includes multistage hole MOFs base material and the heteropoly acid and / or heteropoly acid salt that is combined in multistage hole MOFs base material, at least part of the heteropoly acid and / or heteropoly acid salt is distributed in the channel of multistage hole MOFs base material;Heteropoly acid-multistage hole MOFs composite material has the multistage hole structure of micropore and mesopore;The total mass ratio of polyatomic in heteropoly acid and / or heteropoly acid salt in heteropoly acid-multistage hole MOFs composite material is 2-10%.Preparation method includes: make heteropoly acid and multistage hole MOFs or make heteropoly acid salt and multistage hole MOFs dispersed in the mixed solvent of alcohol and water, then solvent hot synthesis is carried out and solid product is separated.The composite material in the present application, heteropoly acid is limited in the channel of multistage hole MOFs by electronic confinement effect, and heteropoly acid and multistage hole MOFs in composite material synergistic effect while having high efficient denitrification and desulfurization efficacy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of MOFs material technology, specifically to a heteropolyacid-hierarchical porous MOFs composite material and its preparation method, as well as an oil treatment method. Background Technology

[0002] The nitrogen-containing and sulfur-containing compounds in gasoline and diesel fuel produce NO upon combustion. x and SO x This leads to acid rain. With increasingly stringent environmental protection requirements, people have higher and higher demands for the cleanliness of oil products. Oil denitrification and desulfurization have received attention from various countries, and the search for desulfurization and denitrification technologies under mild conditions has become a key research direction.

[0003] Currently, diesel denitrification mainly involves hydrodenitrification and non-hydrodenitrification processes. Deep hydrodenitrification technology consumes a large amount of hydrogen, requires significant equipment investment, and is costly. Compared to industrial-scale hydrodenitrification, adsorption denitrification technology overcomes the drawback of octane number reduction and also solves the problems of high equipment investment and operating costs, making it one of the key technologies developed by domestic and international oil companies in recent years. Similarly, compared to hydrodesulfurization, oxidative desulfurization has been proven to efficiently remove thiophene compounds from fuel oil under normal temperature and pressure conditions, especially aromatic sulfur-containing compounds with high electron density of sulfur atoms. Its reaction is mild, its production cost is low, and it does not damage the octane number of the fuel, making it a clean fuel desulfurization method worthy of promotion.

[0004] How to develop a material that simultaneously possesses efficient desulfurization and denitrification capabilities is a pressing technical problem that needs to be solved. Summary of the Invention

[0005] The purpose of this invention is to provide a heteropolyacid-hierarchical porous MOFs composite material and its preparation method, as well as an oil treatment method, so that heteropolyacids and hierarchical porous MOFs can form a composite material with efficient denitrification and desulfurization functions through the electron confinement effect.

[0006] In a first aspect, the present invention relates to a heteropolyacid-hierarchical porous MOFs composite material, the heteropolyacid-hierarchical porous MOFs composite material comprising a hierarchical porous MOFs substrate and a heteropolyacid and / or heteropolyacid salt composited in the hierarchical porous MOFs substrate, wherein at least a portion of the heteropolyacid and / or heteropolyacid salt is distributed in the channels of the hierarchical porous MOFs substrate; the heteropolyacid-hierarchical porous MOFs composite material has a hierarchical porous structure of micropores and mesopores; and the total mass percentage of the polyatoms in the heteropolyacid and / or heteropolyacid salt in the heteropolyacid-hierarchical porous MOFs composite material is 2-10%.

[0007] In a second aspect, the present invention relates to a method for preparing the heteropolyacid-hierarchical porous MOFs composite material, the method comprising: dispersing the heteropolyacid and hierarchical porous MOFs or dispersing the heteropolyacid salt and hierarchical porous MOFs in a mixed solvent composed of alcohol and water, and then performing solvothermal synthesis and separating the solid phase product.

[0008] Optionally, the heteropolyacid is selected from phosphomolybdic acid, phosphotungstic acid, or vanadium oxyphosphomolybdic acid; the heteropolyacid salt is 1-butyl-3-methylimidazolium phosphomolybdate.

[0009] Optionally, the multi-level porous MOFs are selected from multi-level porous MOF-808 or multi-level porous MOF-66.

[0010] Optionally, the mass ratio of the heteropolyacid to the hierarchical porous MOFs and the heteropolyacid salt to the hierarchical porous MOFs are each independently 1:(5-20).

[0011] Optionally, the alcohol is selected from one or more combinations of methanol, ethanol, propanol and ethylene glycol; the volume ratio of the alcohol to water in the mixed solvent is 1:(0.1-10).

[0012] Optionally, when dispersed in the mixed solvent, the mass ratio of the total mass of the heteropolyacid and the hierarchical porous MOFs to the mixed solvent, or the mass ratio of the total mass of the heteropolyacid salt and the hierarchical porous MOFs to the mixed solvent, is independently 1:(100-300).

[0013] Optionally, the temperature of the solvothermal synthesis is 80-200℃, and the time of the solvothermal synthesis is 2-12 hours.

[0014] Thirdly, the present invention relates to an oil processing method, the oil processing method comprising: dispersing a heteropolyacid-hierarchical porous MOFs composite material in the oil, wherein the heteropolyacid-hierarchical porous MOFs composite material is the heteropolyacid-hierarchical porous MOFs composite material or is prepared by the preparation method.

[0015] Optionally, the mass ratio of the heteropolyacid-hierarchical porous MOFs composite material to the oil is 1:(100-1000); preferably, the oil contains one or more combinations of indole, quinoline, dibenzothiophene, and 4,6-dimethyldibenzothiophene; more preferably, when the oil contains dibenzothiophene and / or 4,6-dimethyldibenzothiophene, the oil treatment method further includes: dispersing an oxidant into the oil, wherein the oxidant is selected from at least one of H2O2, O2, and tert-butyl hydroperoxide; even more preferably, the oil contains 200-500 ppm indole and 200-500 ppm quinoline, or the oil contains 500-1000 ppm dibenzothiophene and 500-1000 ppm 4,6-dimethyldibenzothiophene.

[0016] Beneficial effects:

[0017] In the heteropoly acid-hierarchical porous MOFs composite material of the present invention, the heteropoly acid is confined in the channels of the hierarchical porous MOFs through electronic confinement. The heteropoly acid and the hierarchical porous MOFs in the composite material have synergistic effects and simultaneously have efficient denitrification and desulfurization functions. Attached Figure Description

[0018] Figure 1 This is a graph showing the change in DBT removal conversion rate over time for PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, HP-UiO-66-1~3, PMA@UiO-66, and PMA / UiO-66.

[0019] Figure 2 This is a graph showing the change in the conversion rate of 4,6-DMDBT removal from PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, HP-UiO-66-1~3, and PMA@UiO-66 over time.

[0020] Figure 3 The N2 adsorption-desorption curves are for PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, HP-UiO-66-1~3 and PMA / UiO-66.

[0021] Figure 4 These are pore size distribution diagrams for PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, HP-UiO-66-1~3, and PMA / UiO-66.

[0022] Figure 5These are the X-ray photoelectron spectroscopy (XPS) spectra of PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, as well as PMA and VO-PMA.

[0023] Figure 6 These are the X-ray photoelectron spectroscopy (XPS) spectra of PMA@HP-UiO-66-1~66-2, VO-PMA@HP-UiO-66-1~66-2, as well as PMA and VO-PMA.

[0024] Figure 7 These are the XRD spectra of PMA@HP-UiO-66-1~66-3, VO-PMA@HP-UiO-66-1~66-3, and HP-UiO-66-1~3;

[0025] Figures 8-1 to 8-4 This is a transmission electron microscope (TEM) image and elemental distribution map of PMA@HP-UiO-66-1;

[0026] Figures 9-1 to 9-4 This is a transmission electron microscope (TEM) image and elemental distribution map of the PMA@HP-UiO-66-2.

[0027] Figures 10-1 to 10-4 This is a transmission electron microscope (TEM) image and elemental distribution map of PMA@HP-UiO-66-3;

[0028] Figures 11-1 to 11-5 This is a VO-PMA@HP-UiO-66-1 transmission electron microscope (TEM) and elemental distribution map;

[0029] Figures 12-1 to 12-5 This is a VO-PMA@HP-UiO-66-2 transmission electron microscope (TEM) and its elemental distribution map;

[0030] Figures 13-1 to 13-5 This is a VO-PMA@HP-UiO-66-3 transmission electron microscope (TEM) and elemental distribution map;

[0031] Figure 14 This is a graph showing the relationship between the kinetic rate constant k and temperature for PMA@HP-UiO-66-1~66-3 and VO-PMA@HP-UiO-66-1~66-3 in the oxidative desulfurization reaction. Detailed Implementation

[0032] The present application will now be described in further detail with reference to the accompanying drawings and embodiments. Through these descriptions, the features and advantages of the present application will become clearer and more apparent.

[0033] The term “exemplary” as used herein means “serving as an example, embodiment, or illustration.” Any embodiment illustrated herein as “exemplary” is not necessarily to be construed as superior to or better than other embodiments. Although various aspects of embodiments are shown in the accompanying drawings, the drawings are not necessarily drawn to scale unless specifically indicated otherwise.

[0034] Furthermore, the technical features involved in the different embodiments of this application described below can be combined with each other as long as they do not conflict with each other.

[0035] In a first aspect, the present invention relates to a heteropolyacid-hierarchical porous MOFs composite material, the heteropolyacid-hierarchical porous MOFs composite material comprising a hierarchical porous MOFs substrate and a heteropolyacid and / or heteropolyacid salt composited in the hierarchical porous MOFs substrate, wherein at least a portion of the heteropolyacid and / or heteropolyacid salt is distributed in the channels of the hierarchical porous MOFs substrate; the heteropolyacid-hierarchical porous MOFs composite material has a hierarchical porous structure of micropores and mesopores; and the total mass percentage of the polyatoms in the heteropolyacid and / or heteropolyacid salt in the heteropolyacid-hierarchical porous MOFs composite material is 2-10%.

[0036] It should be noted that the heteropolyacid-hierarchical porous MOFs composite material of the present invention can also be represented as HPAs@HP-MOFs composite material, wherein HPAs represents heteropolyacid, MOFs represents metal-organic framework compounds or metal framework materials, and HP-MOFs represents hierarchical porous metal framework materials. The HPAs@HP-MOFs composite material of the present invention combines the advantages of both materials. It possesses the hierarchical porous defect structure of HP-MOFs, providing open adsorption, reaction sites, and Lewis acid active centers for reactants. Furthermore, through the confinement effect, it anchors the catalytic active centers of HPAs within the channels of HP-MOFs, generating electronic confinement, spatial confinement, and kinetic confinement effects. HPAs provide... The synergistic effect of the acid sites and metal active centers of HPAs and HP-MOFs enables the dual functions of oil denitrification and desulfurization, effectively oxidizing and removing aromatic sulfur compounds from fuel oil while also effectively removing nitrogen compounds. Therefore, the heteropolyacid-hierarchical porous MOFs composite material of the present invention is a composite material with dual functions of oil denitrification and desulfurization.

[0037] It should be noted that the heteropolyacid contains one or more polyatomic atoms. If the heteropolyacid is phosphomolybdic acid (PMA), then the total mass percentage of polyatomic atoms in the heteropolyacid-hierarchical porous MOFs composite material of 2-10% means that the mass percentage of Mo in the heteropolyacid-hierarchical porous MOFs composite material of 2-10%. If the heteropolyacid is vanadium oxyphosphomolybdic acid (VO-PMA), then it means that the total mass percentage of the two polyatomic atoms, Mo and V, is 2-10%.

[0038] Secondly, the present invention relates to a method for preparing the heteropolyacid-hierarchical porous MOFs composite material, the method comprising:

[0039] Heteropolyacids are dispersed with hierarchical porous MOFs or heteropolyacid salts are dispersed with hierarchical porous MOFs in a mixed solvent of alcohol and water, and then solvothermal synthesis is carried out and the solid products are separated.

[0040] It should be noted that in the preparation method of this invention, a stepwise synthesis method based on hierarchical porous MOFs and heteropolyacids is adopted, and the heteropolyacid-hierarchical porous MOFs composite material can be obtained by solvothermal synthesis. The heteropolyacid-hierarchical porous MOFs composite material obtained by the above preparation method contains both hierarchical porous MOFs and heteropolyacids. The heteropolyacids can be distributed in the channels of the hierarchical porous MOFs. HPAs and HP-MOFs exert a synergistic effect, and the heteropolyacids HPAs in the composite material provide... Acid sites and metal active centers: The hierarchical porous MOFs in the composite material provide open adsorption and reaction sites and Lewis acid active centers for reactants. The synergistic effect of Brønsted acid and Lewis acid significantly improves the efficiency of denitrification and desulfurization of oil products.

[0041] It should be noted that, as a preferred embodiment, the preparation method of the present invention further includes a washing step. After separating the solid product, the generated solid powder can be washed with water and ethanol, and may also include a drying step after washing.

[0042] According to one embodiment of the second aspect of the present invention, the heteropoly acid is selected from phosphomolybdic acid, phosphotungstic acid or vanadium oxyphosphomolybdic acid; the heteropoly acid salt is 1-butyl-3-methylimidazolium phosphomolybdate.

[0043] It should be noted that heteropolyacids (HPAs) are oxypolyacids composed of heteroatoms and polyatoms linked by oxygen atom coordination in a specific structure. They are bifunctional green catalysts exhibiting both acid-base and redox properties. Solid heteropolyacid compounds consist of heteropoly anions, cations (protons, metal cations, organic cations), and water or organic molecules. Heteroatoms in heteropolyacids generally refer to P, Si, Fe, Co, etc., while polyatoms generally refer to Mo, W, V, Nb, Ta, etc. For example, in phosphomolybdic acid (PMA), Mo is a polyatomic element, and in vanadium oxyphosphomolybdic acid (VO-PMA), both Mo and V are polyatomic elements. The molecular formula of vanadium oxyphosphomolybdic acid can be represented as [VO(H₂O)₅]H[PMo 12 O 40 ]·23H2O.

[0044] The composite material of the present invention is not limited to the heteropolyacids or heteropolyacid salts that can synergistically combine with the hierarchical porous MOFs, but may also be other heteropolyacids or heteropolyacid salts.

[0045] According to one embodiment of the second aspect of the present invention, the multi-level porous MOFs are selected from multi-level porous MOF-808 or multi-level porous MOF-66.

[0046] It should be noted that the hierarchical porous UiO-66 can be selected from those with different pore sizes. The hierarchical porous MOFs that can synergistically combine with the heteropolyacid to form the composite material are not limited to hierarchical porous MOF-808 or hierarchical porous UiO-66, and the hierarchical porous MOF-808 or hierarchical porous UiO-66 can be commercially available or self-made products. High-performance heteropolyacid-hierarchical porous MOF composite materials can be prepared according to the described preparation method.

[0047] According to one embodiment of the second aspect of the present invention, the mass ratio of the heteropolyacid to the hierarchical porous MOFs and the heteropolyacid salt to the hierarchical porous MOFs are each independently 1:(5-20).

[0048] It should be noted that the preparation is carried out at the stated mass ratio to ensure that the heteropolyacid maintains a suitable mass proportion in the hierarchical porous MOFs in the resulting composite material, thereby obtaining excellent performance. As a preferred embodiment, the mass ratio of the heteropolyacid to the hierarchical porous MOFs and the heteropolyacid salt to the hierarchical porous MOFs is 1:10, which can further significantly improve the performance of the prepared composite material.

[0049] According to one embodiment of the second aspect of the present invention, the alcohol is selected from one or more combinations of methanol, ethanol, propanol and ethylene glycol;

[0050] The volume ratio of alcohol to water in the mixed solvent is 1:(0.1-10).

[0051] It should be noted that when the mixed solvent contains two or more alcohols, the volume ratio of 1:(0.1-10) means that the total volume of the alcohols and the volume ratio of water are 1:(0.1-10), and the volume ratio between the alcohols is not limited.

[0052] It should be noted that in the preparation method of the present invention, a mixed solvent of alcohol and water is cleverly used as the reaction solvent, allowing the heteropolyacid and hierarchical porous MOFs to undergo a solvothermal reaction at a certain mass ratio, thus effectively obtaining a composite with excellent performance. In a preferred embodiment, the volume ratio of alcohol to water in the mixed solvent is 1:1, and the alcohol is ethanol. This allows for better dispersion and composite formation of the heteropolyacid and hierarchical porous MOFs, resulting in electron transfer due to an electron confinement effect between the heteropolyacid and the hierarchical porous MOFs, thereby forming a composite.

[0053] According to one embodiment of the second aspect of the present invention, when dispersed in the mixed solvent, the mass ratio of the total mass of the heteropolyacid and the hierarchical porous MOFs to the mixed solvent, or the mass ratio of the total mass of the heteropolyacid salt and the hierarchical porous MOFs to the mixed solvent, is independently 1:(100-300).

[0054] According to one embodiment of the second aspect of the present invention, the temperature of the solvothermal synthesis is 80-200°C, and the time of the solvothermal synthesis is 2-12 hours.

[0055] In summary, the preparation method of the present invention has easily controllable conditions, simple equipment requirements, and the potential for large-scale production.

[0056] Thirdly, the present invention relates to an oil processing method, the oil processing method comprising: dispersing a heteropolyacid-hierarchical porous MOFs composite material in the oil, wherein the heteropolyacid-hierarchical porous MOFs composite material is the heteropolyacid-hierarchical porous MOFs composite material described in the first aspect of the present invention or is prepared by the preparation method described in the second aspect of the present invention.

[0057] It should be noted that the heteropolyacid-hierarchical porous MOFs composite material can be directly used for fuel adsorption denitrification and oxidative desulfurization reactions, achieving efficient denitrification and desulfurization under mild conditions. Furthermore, the heteropolyacid-hierarchical porous MOFs composite material is easily regenerated, and after regeneration, it can restore its excellent dual-function adsorption denitrification and oxidative desulfurization capabilities.

[0058] According to one embodiment of the third aspect of the present invention, the mass ratio of the heteropolyacid-hierarchical porous MOFs composite material to the oil is 1:(100-1000); preferably, the oil contains one or more combinations of indole, quinoline, dibenzothiophene, and 4,6-dimethyldibenzothiophene; more preferably, when the oil contains dibenzothiophene and / or 4,6-dimethyldibenzothiophene, the oil treatment method further includes: dispersing an oxidant into the oil, wherein the oxidant is selected from at least one of H2O2, O2, and tert-butyl hydroperoxide; even more preferably, the oil contains 200-500 ppm indole and 200-500 ppm quinoline, or the oil contains 500-1000 ppm dibenzothiophene and 500-1000 ppm 4,6-dimethyldibenzothiophene.

[0059] It should be noted that, according to experimental testing, using an octane solution containing 200 ppm indole and / or 200 ppm quinoline as a nitrogen-containing simulated oil, the composite of the present invention exhibits highly efficient denitrification efficiency at room temperature. Using an octane solution containing 500 ppm dibenzothiophene (DBT) and / or 500 ppm 4,6-dimethyldibenzothiophene (4,6-DMDBT) as a sulfur-containing simulated oil, the composite of the present invention exhibits highly efficient catalytic desulfurization efficiency at a mild reaction temperature of 20-80°C.

[0060] It should be noted that the compound of the present invention not only has excellent denitrification and catalytic desulfurization effects on oils containing the above-mentioned nitrogen and sulfur substances, but also has excellent denitrification and catalytic desulfurization effects on various types of oils.

[0061] In summary, the composites of this invention contain hierarchical porous metal-organic frameworks (HP-MOFs) with microporous and mesoporous structures, as well as numerous defects and unsaturated coordination metal sites. The heteropoly acids (HPAs) possess… The acid sites and metal active centers work together to achieve a synergistic effect, enabling oil to undergo both adsorption denitrification and oxidative desulfurization.

[0062] The present invention will be further described in detail below through examples, but these examples are not intended to limit the invention.

[0063] Except for the self-made reagents used in the preparation examples below, all other reagents used in the following examples are commercially available reagents.

[0064] In the following examples, PMA represents phosphomolybdic acid, HPW represents phosphotungstic acid, VO-PMA represents vanadium oxyphosphomolybdic acid, and [Bmim]3PMo 12 O 40 This refers to 1-butyl-3-methylimidazolium phosphomolybdate. HP-UiO-66-1, HP-UiO-66-2, and HP-UiO-66-3 refer to hierarchical porous UiO-66-1, hierarchical porous UiO-66-2, and hierarchical porous UiO-66-3, respectively. A certain heteropolyacid@a certain HP-UiO-66, such as PMA@HP-UiO-66-1, represents a composite material of PMA and HP-UiO-66-1. Among these, HP-UiO-66-1, HP-UiO-66-2, HP-UiO-66-3, HP-MOF-808, vanadium oxyphosphomolybdate VO-PMA, and 1-butyl-3-methylimidazolium phosphomolybdate [Bmim]3PMo 12 O 40 It is prepared as follows.

[0065] Example of HP-UiO-66-1 preparation:

[0066] Terephthalic acid (BDC, 0.066 g, 0.4 mmol) and zinc acetate dihydrate (Zn(CH3COO)2·2H2O, 0.220 g, 1.0 mmol) were dissolved separately in 7.5 mL of N,N-dimethylformamide (DMF). After stirring each solution for 10 minutes, the two solutions were mixed and stirred at room temperature for 24 hours. The resulting white suspension was centrifuged and washed with DMF at least three times to obtain a white MOF-5 product. The nano-MOF-5 particles were dispersed in 4 mL of DMF for later use. Zirconium tetrachloride (ZrCl4, 0.106 g, 0.45 mmol) and BDC (0.075 g, 0.45 mmol) were dissolved in a mixed solvent of 20 mL of DMF and 5.6 mL of glacial acetic acid (HAc) and sonicated for 10 minutes. 2 mL of the prepared DMF nano-MOF-5 particles (MOF-5 DMF dispersion) was added to the solution, and the suspension was sonicated for another 10 minutes. The mixture was then transferred to a hydrothermal reactor and placed in an oven at 120°C for 24 hours. After cooling to room temperature, the solid was collected by centrifugation and washed three times with DMF. The obtained solid product was dispersed in a hydrochloric acid solution at pH 1.0 and stirred for about 10 minutes. The final product was then centrifuged, washed three times with DMF and acetone, and dried overnight in an oven at 60°C. The final white powder product was named HP-UiO-66-1.

[0067] Example of HP-UiO-66-2 preparation:

[0068] Zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 0.148 g, 0.5 mmol) and benzoic acid (HBC, 1.830 g, 15 mmol) were dissolved in 20 mL of DMF. The mixture was sonicated and then placed in an oven at 120 °C for 12 hours. After cooling to room temperature, ZrCl4 (0.120 g, 0.5 mmol) and BDC (0.166 g, 1.0 mmol) were added. After sonication for another 10 minutes, the mixture was placed in a preheated oven at 120 °C for another 24 hours. After cooling to room temperature, the solid was collected by centrifugation and washed using the same method as HP-UiO-66-1. The final white powder product was named HP-UiO-66-2.

[0069] Example of HP-UiO-66-3 preparation:

[0070] Zn(NO3)2·6H2O (0.400 g, 1.347 mmol), 2-methylimidazole (0.2 g, 2.436 mmol), ZrCl4 (0.233 g, 1 mmol), and BDC (0.166 g, 1 mmol) were dispersed in DMF (44 mL) and HAc (12 mL). The mixture was sonicated for 30 minutes and then transferred to a hydrothermal reactor, where it was stored in an oven at 120 °C for 24 hours. After cooling to room temperature, the white solid was collected by centrifugation and processed using the same method as HP-UiO-66-1. The final white powder product was named HP-UiO-66-3.

[0071] Example of HP-MOF-808 preparation:

[0072] 0.89 g Zn(NO3)2·6H2O, 0.44 g 2-methylimidazole, 0.52 g ZrCl4, and 0.16 g trimellitic acid were dispersed in a mixed solution of 80 mL LDM and 80 mL HAc. The mixture was sonicated for 30 minutes and then transferred to a hydrothermal reactor, where it was stored in an oven at 120 °C for 36 hours. After cooling to room temperature, the white solid was collected by centrifugation and processed using the same method as HP-UiO-66-1. The final white solid product was HP-MOF-808.

[0073] Example of UiO-66 preparation:

[0074] ZrCl4 (0.233 g, 1 mmol) and BDC (0.166 g, 1 mmol) were dispersed in a mixture of DMF (44 mL) and HAc (12 mL). The mixture was sonicated for 30 minutes and then transferred to a hydrothermal reactor, where it was stored in an oven at 120 °C for 24 hours. After cooling to room temperature, the white solid was collected by centrifugation, washed with DMF, and the resulting white powder was named UiO-66.

[0075] Example of preparation of vanadium oxyphosphomolybdic acid (VO-PMA):

[0076] Dissolve 4.43g PMA in 10mL of water, stir slowly and add 0.78g of barium hydroxide octahydrate (Ba(OH)2·8H2O), then quickly add 0.395g of vanadium oxysulfate. After stirring for 30 minutes, filter off the precipitate and evaporate the solution to dryness to obtain a green solid, which is VO-PMA.

[0077] 1-Butyl-3-methylimidazolium phosphomolybdate [Bmim]3PMo 12 O 40 Preparation example:

[0078] 1-Butyl-3-methylimidazolium chloride ([Bmim]Cl, 1.27 g) and PMA (4.43 g) were dissolved in 10 mL of water respectively. The [Bmim]Cl solution was added dropwise to a phosphomolybdic acid solution with constant stirring to form a yellow precipitate. The solid was collected by centrifugation and washed with deionized water, then dried at 60 °C overnight to obtain the yellow solid, which is [Bmim]3PMo. 12 O 40 .

[0079] Example 1: Preparation of PMA@HP-UiO-66-1 composite material

[0080] Weigh 30 mg PMA and 300 mg HP-UiO-66-1 prepared in the above preparation example, disperse them in a 60 mL mixture of ethanol and water (volume ratio 1:1), transfer the mixture to a hydrothermal reactor, heat it in a constant temperature oven at 100 °C for 12 hours, wash it with water and ethanol, collect the resulting solid powder, and record it as material PMA@HP-UiO-66-1.

[0081] Example 2: Preparation of VO-PMA@HP-UiO-66-1 composite material

[0082] The preparation method of material PMA@HP-UiO-66-1 in Example 1 is similar, except that 30mg PMA is replaced with an equal amount of VO-PMA, and the resulting solid powder is denoted as material VO-PMA@HP-UiO-66-1.

[0083] Example 3: Preparation of [Bmim]3PMo 12 O 40 @HP-UiO-66-1 composite material

[0084] The preparation method of material PMA@HP-UiO-66-1 in Example 1 is similar, except that 30 mg of PMA is replaced with an equal amount of [Bmim]3PMo. 12 O 40 The resulting solid powder is denoted as material [Bmim]3PMo. 12 O 40 @HP-UiO-66-1.

[0085] Example 4: Preparation of HPW@HP-UiO-66-1 composite material

[0086] The preparation method of material PMA@HP-UiO-66-1 in Example 1 is similar, except that 30mg PMA is replaced with an equal amount of HPW, and the resulting solid powder is denoted as material HPW@HP-UiO-66-1.

[0087] Example 5: Preparation of PMA@HP-UiO-66-2 and PMA@HP-UiO-66-3 composite materials

[0088] The preparation method of material PMA@HP-UiO-66-1 in Example 1 is similar, except that 300mg of HP-UiO-66-1 is replaced with equal amounts of HP-UiO-66-2 and HP-UiO-66-3 prepared in the above preparation examples, respectively. The resulting solid powders are denoted as materials PMA@HP-UiO-66-2 and PMA@HP-UiO-66-3, respectively.

[0089] Example 6: Preparation of VO-PMA@HP-UiO-66-2 and VO-PMA@HP-UiO-66-3 composite materials

[0090] The preparation method of material VO-PMA@HP-UiO-66-1 in Example 2 is similar, except that 300mg of HP-UiO-66-1 is replaced with equal amounts of HP-UiO-66-2 and HP-UiO-66-3 prepared in the above preparation examples, respectively. The resulting solid powders are denoted as materials VO-PMA@HP-UiO-66-2 and VO-PMA@HP-UiO-66-3, respectively.

[0091] Example 7

[0092] Similar to the preparation method in Example 1, except that 300 mg of HP-UiO-66-1 was replaced with an equal amount of HP-MOF-808 prepared in the above preparation example, and PMA@HP-MOF-808 composite material was obtained.

[0093] Example 8

[0094] The preparation method is similar to that in Example 1, except that 30 mg PMA was replaced with 15 mg PMA and 60 mg PMA, respectively, to obtain 5% PMA@HP-UiO-66-1 and 20% PMA@HP-UiO-66-1.

[0095] Comparative Example 1

[0096] Similar to the preparation method in Example 1, except that 300 mg HP-UiO-66-1 was replaced with an equal amount of UiO-66 prepared in the above preparation example to obtain PMA@UiO-66 composite material.

[0097] Comparative Example 2

[0098] 23.6 mg PMA, 83.5 mg BDC, and 116.5 mg ZrCl4 were dispersed in a mixed solution of 3.6 mL HAc and 30 mL DMF. After sonication for 30 minutes, the mixture was transferred to a hydrothermal reactor and stored in an oven at 120 °C for 24 h. After cooling to room temperature, the solid was collected by centrifugation, washed with DMF, and dried overnight at 60 °C. The resulting solid powder was designated as material PMA / UiO-66.

[0099] Test Example 1

[0100] The composite materials prepared by the above examples, HP-UiO-66-1 to HP-UiO-66-3 prepared by the above preparation examples, and PMA@UiO-66 prepared by Comparative Example 1 were used as denitrification reagents to perform adsorption denitrification tests to calculate the denitrification rate.

[0101] The reaction conditions were as follows: 30 mg of denitrification reagent was added to 10 g of nitrogen-containing simulated oil, and the mixture was stirred at 500 rpm at room temperature for one hour. After centrifugation, the supernatant was collected, and the concentrations of indole and quinoline before and after adsorption were analyzed by liquid chromatography. The nitrogen-containing simulated oil was an octane solution containing 200 ppm quinoline and 200 ppm indole. The PMA@HP-UiO-66-1 composite material (prepared in Example 1) after the adsorption reaction was collected, soaked in anhydrous ethanol for 2.5 hours, centrifuged, and the resulting solid powder was dried at 60 °C for 12 hours, and denoted as material PMA@HP-UiO-66-1-regenerated.

[0102] Table 1 below shows the denitrification rate of indole and quinoline in nitrogen-containing simulated oil after stirring at room temperature for 1 hour.

[0103] Denitrification rate (%) = (Concentration of nitrogen compounds in nitrogen-containing simulated oil before adsorption - Concentration of nitrogen compounds in nitrogen-containing simulated oil after adsorption) ÷ Concentration of nitrogen compounds in nitrogen-containing simulated oil before adsorption × 100%.

[0104] Table 1

[0105]

[0106] As shown in Table 1, compared to HP-UiO-66-1 to 3, the heteropolyacid@HP-UiO-66 composite material significantly improves the removal efficiency of both basic nitrogen compounds (quinoline) and non-basic nitrogen compounds (indole). This is because heteropolyacids can provide Brønsted acid (B) sites, and the hierarchical porous defects in the framework material can provide Lewis acid (L) sites. The synergistic effect of B and L acids enables the composite material to effectively remove nitrogen-containing compounds from fuel oil, resulting in a significant denitrification effect on simulated oil within 1 hour. The composite material prepared in this embodiment of the invention exhibits good stability and is easy to recycle; efficient denitrification function can be restored through regeneration.

[0107] Test Example 2

[0108] The composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2 and VO-PMA@HP-UiO-66-3 prepared in the above examples, HP-UiO-66-1 to 3 prepared in the three preparation examples, PMA@UiO-66 prepared in Comparative Example 1, and PMA / UiO-66 prepared in Comparative Example 2 were subjected to oxidation desulfurization reaction detection.

[0109] The reaction conditions were as follows: 50 mg of the composite material was added to 10 g of sulfur-containing simulated oil, and hydrogen peroxide tert-butyl oxidant was added at an O / S ratio of 3. The mixture was stirred at 500 rpm and 80 °C. The changes in the concentrations of DBT (dibenzothiophene) and 4,6-DMDBT (4,6-dimethyldibenzothiophene) were analyzed by gas chromatography. The sulfur-containing simulated oil was an octane solution containing 500 ppm DBT and 500 ppm 4,6-DMDBT.

[0110] Conversion rate (%) = (Concentration of aromatic sulfur compounds in the sulfur-containing simulated oil before reaction - Concentration of aromatic sulfur compounds in the sulfur-containing simulated oil at a certain time) ÷ Concentration of aromatic sulfur compounds in the sulfur-containing simulated oil before reaction * 100%.

[0111] Figure 1 and Figure 2 The conversion rates of DBT and 4,6-DMDBT in sulfur-containing simulated oil over time are shown respectively.

[0112] Figure 1 and Figure 2 It is evident that, compared to HP-UiO-66-1~3, both PMA@HP-UiO-66-1~3 and VO-PMA@HP-UiO-66-1~3 significantly improve the conversion rate of sulfur-containing compounds, indicating that the prepared composite materials exhibit excellent catalytic activity in the oxidative desulfurization reaction. Under the selected reaction conditions, several HPAs@HP-UiO-66 composite materials can achieve deep desulfurization in a short time. The hierarchical porous defect structure in the composite material can provide open adsorption / reaction sites for reactants, anchoring HPAs in the composite material through the confinement effect. This integrates the advantages of hierarchical porous defect MOFs and HPAs, and the two exert a synergistic effect, significantly improving the removal of aromatic sulfur-containing compounds. Regarding the other composite materials prepared in the above examples: [Bmim]3PMo... 12 O 40Under the same conditions, @HP-UiO-66-1 and HPW@HP-UiO-66-1 showed significantly higher desulfurization effects than HP-UiO-66-1 to 3. Other composite materials prepared in the above examples, such as 5% PMA@HP-UiO-66-1 and 20% PMA@HP-UiO-66-1, were also tested under the same conditions, showing significantly higher desulfurization effects than HP-UiO-66-1. The PMA@UiO-66 and PMA / UiO-66 prepared in Comparative Examples 1 and 2 contained only microporous structures. Under the same conditions, their desulfurization effects were tested, and the results showed that their desulfurization effects were significantly worse than those of the several HPAs@HP-UiO-66 composite materials, demonstrating the importance of hierarchical porous materials in the substrate.

[0113] Test Example 3

[0114] The composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above examples, HP-UiO-66-1 to 3 prepared in the three preparation examples, and PMA / UiO-66 prepared in Comparative Example 2 were subjected to N2 adsorption-desorption detection. The obtained N2 adsorption-desorption curves are shown below. Figure 3 As shown, the pore size distribution diagrams obtained from pore size detection are as follows: Figure 4 As shown. The specific surface area of ​​the composite materials prepared in the above embodiments is 500-1200 m². 2 / g, combined Figure 4 The presence of micropores and mesopores in the composite material is evident, indicating that the composite material prepared in the above embodiments possesses a hierarchical porous structure of micropores and mesopores. Other composite materials prepared in the above embodiments include: [Bmim]3PMo. 12 O 40 @HP-UiO-66-1 and HPW@HP-UiO-66-1 were tested under the same conditions, and the results showed that they also possessed a hierarchical porous structure of micropores and mesopores. The pore volume of the composite materials prepared in the above examples was smaller than that of HP-UiO-66-1 to 3, indicating that the heteropolyacids were distributed within the channels of the hierarchical porous MOFs in the prepared composite materials. The N2 adsorption-desorption curve and pore size distribution diagram of the PMA / UiO-66 composite material prepared in Comparative Example 2 showed that only a microporous structure existed. The PMA@UiO-66 composite material prepared in Comparative Example 1 was subjected to N2 adsorption-desorption detection and pore size detection under the same conditions, and the results showed that this composite material was similar to the composite material prepared in Comparative Example 2, possessing only a microporous structure.

[0115] Test Example 4

[0116] XPS (Mo) analysis was performed on the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above examples, as well as PMA and VO-PMA. The obtained XPS (Mo) spectra are shown below. Figure 5 As shown. XPS(P) analysis was performed on the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, as well as PMA and VO-PMA prepared in the above examples. The obtained X-ray photoelectron spectroscopy (XPS(P) spectra) are shown below. Figure 6 As shown.

[0117] It can be seen that compared to PMA and VO-PMA, the binding energies of Mo and P elements in the composite material are shifted towards lower binding energies. This indicates that HP-UiO-66 has an electron confinement effect on HPAs, with some electrons transferring from HP-UiO-66 to HPAs, increasing the electron density around P and Mo elements in HPAs and decreasing the binding energy. XPS (Mo) and XPS (P) analyses were performed on the other composite materials prepared in the above examples, and the results show that the metal skeleton material in the composite materials prepared in the other examples all exhibit the aforementioned electron confinement effect on the heteropolyacids.

[0118] Test Example 5

[0119] The XRD patterns of the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above examples, as well as HP-UiO-66-1 to 3 prepared in the three preparation examples, were obtained by XRD analysis. Figure 7 As shown.

[0120] pass Figure 7It can be seen that the XRD patterns of the composite materials prepared in the above embodiments show characteristic diffraction peaks of hierarchical porous MOFs, indicating that the hierarchical porous MOFs can still maintain good crystallinity and morphology after the composite process with heteropolyacids. The heteropolyacids introduced into the composite materials do not show obvious diffraction peaks in the XRD, indicating that the heteropolyacids are mainly located inside the pores of the hierarchical porous MOFs. XRD analysis of other composite materials prepared in the above embodiments also showed that the hierarchical porous MOFs in the composite materials can still maintain good crystallinity and morphology.

[0121] Test Example 6

[0122] Transmission electron microscopy (TEM) analysis was performed on the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above examples. The obtained TEM images and elemental distribution maps are shown in the figures below. Figures 8-1 to 8-4 9-1~9-4, 10-1~10-4, 11-1~11-5, 12-1~12-5 and 13-1~13-5.

[0123] The TEM and elemental distribution maps of the above composite materials show that the elements are uniformly distributed within the material and do not aggregate on the surface. This indicates that HPAs are well confined within HP-UiO-66, and that HP-UiO-66 exhibits a spatial confinement effect on HPAs. Transmission electron microscopy analysis of other composites prepared in the above examples under the same conditions also showed that the elements in the composite materials were uniformly distributed within the material and did not aggregate on the surface.

[0124] Test Example 7

[0125] Figure 14 The diagram illustrates the relationship between the kinetic rate constant k and temperature in the oxidative desulfurization reaction of the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above embodiments. Since the oxidation process of 4,6-DMDBT is a pseudo-first-order reaction, the relationship between ln(CO / C) and time t varies for different catalysts. The linear relationship is given by C0 / C, defined as the initial sulfur concentration of 4,6-DMDBT divided by the unreacted sulfur concentration of 4,6-DMDBT, and k represents the rate constant of the reaction at the current temperature. This is based on the Arrhenius equation. (A and R are constants). The apparent activation energy (Ea) of the reaction can be calculated using the rate constant k at different temperatures (T). Based on the slope of the straight line in the figure, the activation energy of the composite material is calculated to be 50-60 kJ / mol. The activation energy of VO-PMA confined by HP-UiO-66 is lower than that of PMA, indicating a kinetic confinement effect.

[0126] Test Example 8

[0127] The contents of Mo and V in the composite materials PMA@HP-UiO-66-1, PMA@HP-UiO-66-2, PMA@HP-UiO-66-3, VO-PMA@HP-UiO-66-1, VO-PMA@HP-UiO-66-2, and VO-PMA@HP-UiO-66-3 prepared in the above embodiments were quantitatively analyzed by inductively coupled plasma optical emission spectrometry (ICP-OES) to demonstrate the content of supported heteropolyacids. The measured data are detailed in Table 2 below.

[0128] Table 2

[0129]

[0130] The ICP detection data in Table 2 further corroborates that the composite material prepared in the embodiments of the present invention successfully introduced heteropolyacids into hierarchical porous MOFs. Quantitative analysis of other composite materials prepared in the above embodiments using inductively coupled plasma optical emission spectrometry (ICP-OES) also detected the content of elements in the heteropolyacids, and the total mass percentage of polyatoms in the heteropolyacids or heteropolyacid salts in the heteropolyacid-hierarchical porous MOFs composite material was 2-10%. Combined with the characterization results from ICP and XRD, it can be seen that the composite material of the present invention is a composite material containing both heteropolyacids and hierarchical porous MOFs.

[0131] In the description of this application, it should be noted that the terms "upper", "lower", "inner", "outer", "front", "rear", "left", "right", etc., indicate the orientation or positional relationship based on the orientation or positional relationship in the working state of this application. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0132] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0133] The present application has been described above with reference to preferred embodiments; however, these embodiments are merely exemplary and illustrative. Various substitutions and modifications can be made to the present application based on these embodiments, all of which fall within the protection scope of the present application.

Claims

1. A method for preparing a heteropolyacid-hierarchical porous MOF composite material, characterized in that, The preparation method includes: Heteropolyacids are dispersed in a mixed solvent of alcohol and water, or heteropolyacid salts are dispersed in a mixed solvent of alcohol and water, and then solvothermal synthesis is performed and the solid product is separated. The volume ratio of alcohol to water in the mixed solvent is 1:(0.1-10). The heteropolyacid-hierarchical porous MOFs composite material comprises a hierarchical porous MOFs substrate and a heteropolyacid and / or heteropolyacid salt composited in the hierarchical porous MOFs substrate, wherein at least a portion of the heteropolyacid and / or heteropolyacid salt is distributed in the channels of the hierarchical porous MOFs substrate; the heteropolyacid-hierarchical porous MOFs composite material has a hierarchical porous structure of micropores and mesopores; the total mass percentage of the polyatoms in the heteropolyacid and / or heteropolyacid salt in the heteropolyacid-hierarchical porous MOFs composite material is 2-10%; the hierarchical porous MOFs are selected from hierarchical porous MOF-808 or hierarchical porous MOF-66.

2. The preparation method according to claim 1, characterized in that, The heteropoly acid is selected from phosphomolybdic acid, phosphotungstic acid, or vanadium oxyphosphomolybdic acid; the heteropoly acid salt is 1-butyl-3-methylimidazolium phosphomolybdate.

3. The preparation method according to claim 1, characterized in that, The mass ratio of the heteropolyacid to the hierarchical porous MOFs and the heteropolyacid salt to the hierarchical porous MOFs are each independently 1:(5-20).

4. The preparation method according to claim 1, characterized in that, The alcohol is selected from one or more combinations of methanol, ethanol, propanol, and ethylene glycol.

5. The preparation method according to claim 1, characterized in that, When dispersed in the mixed solvent, the mass ratio of the total mass of the heteropolyacid and the hierarchical porous MOFs to the mixed solvent, or the mass ratio of the total mass of the heteropolyacid salt and the hierarchical porous MOFs to the mixed solvent, is independently 1:(100-300).

6. The preparation method according to claim 1, characterized in that, The temperature of the solvothermal synthesis is 80-200℃, and the time of the solvothermal synthesis is 2-12 hours.

7. A heteropolyacid-hierarchical porous MOF composite material prepared by the preparation method according to any one of claims 1 to 6, characterized in that, The heteropolyacid-hierarchical porous MOFs composite material comprises a hierarchical porous MOFs substrate and a heteropolyacid and / or heteropolyacid salt composited in the hierarchical porous MOFs substrate, wherein at least a portion of the heteropolyacid and / or heteropolyacid salt is distributed in the channels of the hierarchical porous MOFs substrate; the heteropolyacid-hierarchical porous MOFs composite material has a hierarchical porous structure of micropores and mesopores; the total mass percentage of the polyatoms in the heteropolyacid and / or heteropolyacid salt in the heteropolyacid-hierarchical porous MOFs composite material is 2-10%; the hierarchical porous MOFs are selected from hierarchical porous MOF-808 or hierarchical porous MOF-66.

8. A method for desulfurizing and denitrogenating oil products, characterized in that, The oil desulfurization and denitrification treatment method includes: The heteropolyacid-hierarchical porous MOFs composite material is dispersed in the oil, wherein the heteropolyacid-hierarchical porous MOFs composite material is the heteropolyacid-hierarchical porous MOFs composite material of claim 7.

9. The method for desulfurizing and denitrogenating oil products according to claim 8, characterized in that, The mass ratio of the heteropolyacid-hierarchical porous MOFs composite material to the oil is 1:(100-1000).

10. The method for desulfurizing and denitrogenating oil products according to claim 9, characterized in that, The oil contains one or more of the following: indole, quinoline, dibenzothiophene, and 4,6-dimethyldibenzothiophene.

11. The method for desulfurizing and denitrogenating oil products according to claim 10, characterized in that, When the oil contains dibenzothiophene and / or 4,6-dimethyldibenzothiophene, the oil desulfurization and denitrification treatment method further includes: An oxidant is dispersed into the oil, wherein the oxidant is selected from at least one of H2O2, O2 and tert-butyl hydroperoxide.

12. The method for desulfurizing and denitrogenating oil products according to claim 11, characterized in that, The oil contains 200-500 ppm indole and 200-500 ppm quinoline, or the oil contains 500-1000 ppm dibenzothiophene and 500-1000 ppm 4,6-dimethyldibenzothiophene.

Citation Information

Patent Citations

  • Preparation and application of hierarchical pore metal-organic framework loaded heteropolyacid catalyst

    CN107694611A